Diversion device and method suitable for high MgO nickel slag
By designing a horizontal furnace body and dual spray gun system in the nickel smelting process, combining electrode heating and vulcanizing agent spraying, the problem of high tailslag nickel content in the depletion of high MgO nickel slag electric furnace is solved, and more efficient nickel recycling and Energy utilization.
Patent Information
- Application Number
- CN202411153986.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing nickel smelting process, the high content of tailslag nickel slag electric furnaces is high, the reduction agent utilization effect is poor, and the slag sulfonium separation is insufficient, resulting in the imperfect depletion effect, affecting economic benefits and environmental evaluation.
A horizontal furnace body leaning device suitable for high MgO nickel slag is designed, combining side blowing spray gun, electrode heating and vulcanizing agent spraying to form reduction + vulcanization + settlement separation in the form of dual heating to improve power Learn conditions and heat utilization.
It effectively reduces the nickel content in the depleted slag to less than 0.35%, improves the recovery rate of valuable metals such as nickel, and is suitable for the treatment of high MgO nickel slag, improving the depletion effect and energy efficiency.
Smart Images

Figure CN119020600A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metallurgy, and in particular to a device and method suitable for depleting high-MgO nickel slag. Background Art
[0002] Nickel (Ni) is a metal that has the characteristics of anti-oxidation, anti-corrosion, high temperature resistance, high strength, good ductility, etc. It is widely used and is indispensable in various industries such as aerospace, aviation, navigation, national defense, scientific research, industry, agriculture, medical care, automobiles, steel and civil use. In particular, it has the largest consumption proportion in the steel and non-ferrous metal smelting industry. The demand for nickel in the fields of high-tech and new energy technology is also very strong, especially for ternary power battery materials. The more advanced nickel smelting processes currently used at home and abroad are: flash smelting, top blowing smelting, and side blowing smelting.
[0003] Flash smelting belongs to the suspension smelting process, and its process flow includes: nickel concentrate, flux batching - drying - concentrate burner spraying into the reaction tower - flash smelting - production of nickel matte and smelting slag. This process has strict requirements on the particle size, moisture, composition and stability of the materials entering the furnace. If quartz stone is used as flux, the quartz stone needs to be finely ground and mixed with dry concentrate. Flash smelting requires that the materials entering the furnace must be dry powder, and has high requirements on material composition and stability. It has poor adaptability to raw materials, especially strict requirements on the MgO content in the material. The process flow is long and the operation is complicated.
[0004] Top-blowing smelting (including Ausmelt and ISA two kinds of submerged spray gun top-blowing processes) belongs to the molten pool smelting process, and its process flow includes: nickel concentrate, flux and other ingredients - granulation - furnace top mobile feeder added into the furnace - top-blowing smelting - electric furnace sedimentation separation - production of low nickel matte and waste slag. The raw materials of this process need to be granulated before entering the furnace, and the particle size of the materials entering the furnace is required to be 5-25mm. The requirements for material composition and stability are broader than flash smelting, but an electric furnace is required to clarify nickel matte and smelting slag outside the furnace, and the electric furnace also has the effect of nickel slag depletion. The top-blowing smelting process is long and energy consumption is high; at the same time, top-blowing smelting is a single-gun operation, and the wind needs to be stopped for insulation when the spray gun is replaced, so the smelting operation rate is low, and the smelting spray gun is inserted into the slag layer with a single gun, and the service life is short. In addition, the single-gun operation has a large blast volume, strong stirring of the molten pool, and large splashing, so the required furnace height is high, the spray gun is long, the plant height increases accordingly, and the investment is high.
[0005] Side-blowing smelting is also a molten pool smelting process, and its process flow includes: nickel concentrate, flux and other ingredients - adding them into the furnace by a mobile feeder on the top of the furnace - side-blowing smelting - producing nickel matte and smelting slag. This process requires the material particle size to be ≤25mm, and the requirements for material composition and stability are more extensive than those for flash smelting. The spray guns on both sides are buried in the slag layer, and the spray guns on both sides need to be quickly blocked when the air is stopped due to an accident, which is labor-intensive for workers.
[0006] At present, flash smelting, top-blown smelting and side-blown smelting require an electric furnace outside the furnace to deplete the smelting slag. However, the effect of electric furnace depletion or sedimentation is not ideal. The main problems are: first, the power consumption is large and the energy utilization efficiency is low; second, most of the reducing agent put into the electric furnace floats to the surface of the melt, and the reducing agent utilization effect is poor; third, the kinetic conditions cannot promote the separation of slag and matte; fourth, the furnace wall is prone to slagging due to insufficient heat transfer, which affects the efficiency of the electric furnace. In particular, when processing nickel slag containing high-melting-point substances such as MgO (MgO content of 6-20wt%), the MgO content of the settled electric furnace slag will be high, and the nickel content of the slag will be further affected. Usually, the nickel content of the slag after electric furnace depletion is greater than 0.5%. The high nickel content of the tailings has become the crux of the economic operation of the nickel smelting system, seriously affecting the economic benefits and environmental evaluation indicators of the nickel smelting system. Summary of the invention
[0007] The main purpose of the present invention is to provide a depletion device and method suitable for high-MgO nickel slag, so as to solve the problems of poor depletion effect caused by high nickel content in tailings, poor reducing agent utilization, insufficient slag-matte separation, etc. in the high-MgO nickel slag electric furnace depletion process in the prior art.
[0008] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a depletion device suitable for high-MgO nickel slag, which comprises: a horizontal furnace body, the horizontal furnace body having a first end and a second end opposite to the first end, and along the direction from the first end to the second end, the inner cavity of the horizontal furnace body comprises a feeding zone, a blowing zone, an electrode zone, a settling zone and a discharge zone which are connected in sequence; the feeding zone is provided with a high-MgO nickel slag inlet; the blowing zone is provided with at least two blowing ports, wherein a part of the blowing ports are arranged at the top of the blowing zone, and another part of the blowing ports are arranged at the side of the blowing zone; the settling zone is provided with a smoke outlet; the discharge zone is provided with a nickel matte discharge port and a slag discharge port; at least two spray guns, which are connected to each of the spray ports one by one; the spray guns are used to spray a reducing agent, a fuel, an oxygen-containing gas and a sulfiding agent into the interior of the blowing zone; an electrode is provided in the electrode zone, and the electrode passes through the top wall of the electrode zone and extends to the interior of the electrode zone for electrode heating.
[0009] Furthermore, the total length of the horizontal furnace body along the direction from the first end to the second end is recorded as L, the length of the feed zone is recorded as L1, the length of the blowing zone is recorded as L2, the length of the electrode zone is recorded as L3, the length of the sedimentation zone is recorded as L4, and the length of the discharge zone is recorded as L5, then L1 / L=1 / 15~1 / 8, L2 / L=1 / 8~1 / 5, L3 / L=1 / 2~3 / 5, L4 / L=1 / 8~1 / 5, L5 / L=1 / 15~1 / 8.
[0010] Furthermore, the injection zone is provided with 2 to 12 injection ports, the depletion device comprises 2 to 12 spray guns, and the spray guns are connected to each injection port one by one; the electrodes are 1 to 4 groups of three-phase electrodes, and the power of the electrodes is 5 to 15 MVA.
[0011] Furthermore, the reducing agent is selected from one or more of pulverized coal, natural gas, and hydrogen; the fuel is selected from one or more of natural gas, pulverized coal, carbon powder, heavy oil, liquefied petroleum gas, shale gas, and coalbed methane; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 21 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
[0012] Furthermore, the horizontal furnace body is a rectangular furnace body or a quasi-rectangular furnace body, and the direction from the first end to the second end is the length direction. The furnace body is 20 to 40 meters long, 5 to 10 meters wide, and 5 to 10 meters high.
[0013] Furthermore, the lance includes a side-blowing lance and a top-blowing lance. The side-blowing lance is inserted horizontally or obliquely downward into the slag melt layer through the blowing port on the side of the blowing zone, and the top-blowing lance is inserted vertically into the slag melt layer through the blowing port at the top of the blowing zone.
[0014] Furthermore, the distance between the nozzle of the side-blowing lance and the bottom wall of the blowing zone is 0.8 to 2 meters, and the distance between the nozzle of the top-blowing lance and the bottom wall of the blowing zone is 0.5 to 2 meters.
[0015] Furthermore, the side-blowing lance is used for spraying the solids among the reducing agent, the fuel, the oxygen-containing gas and the sulfiding agent, and the top-blowing lance is used for spraying the gas and liquid among the reducing agent, the fuel, the oxygen-containing gas and the sulfiding agent.
[0016] Furthermore, there is one high-MgO nickel slag inlet, which is arranged at the top of the feeding area; there are 2 to 4 nickel matte discharge ports, which are arranged at the bottom of the discharge area; and there are 2 to 5 slag discharge ports, which are arranged at the side of the discharge area.
[0017] Furthermore, the depletion device also includes: a chimney, which is arranged at the smoke outlet, and a secondary combustion device is arranged in the chimney, which is used to perform secondary combustion on the depleted flue gas discharged from the smoke outlet to obtain secondary combustion flue gas; a dust collection and purification unit, which is connected to the chimney and is used to perform dust collection and purification on the secondary combustion flue gas.
[0018] According to another aspect of the present invention, there is also provided a method for impoverishing high-MgO nickel slag, wherein the MgO content in the high-MgO nickel slag is 6 to 20 wt %. The high-MgO nickel slag is impoverished by using the above-mentioned impoverishment device, and the impoverishment process comprises the following steps: introducing high-MgO nickel slag into a horizontal furnace body through a high-MgO nickel slag inlet; spraying a reducing agent, a fuel, an oxygen-containing gas and a sulfiding agent into a spraying zone through a spray gun, and simultaneously turning on the electrode to heat the electrode zone, so that the high-MgO nickel slag undergoes an impoverishment reaction inside the horizontal furnace body; sedimenting and separating the melt after the impoverishment reaction in a sedimentation zone to form nickel matte and impoverished slag; discharging the nickel matte from a nickel matte discharge port in a discharge zone, and discharging the impoverished slag from a slag discharge port in the discharge zone.
[0019] Furthermore, during the depletion reaction, the temperature inside the horizontal furnace is controlled to be 1000-1600°C, preferably 1300-1400°C.
[0020] Furthermore, the reducing agent is selected from one or more of pulverized coal, natural gas, and hydrogen; the fuel is selected from one or more of natural gas, pulverized coal, carbon powder, and heavy oil; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 22 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
[0021] Furthermore, the injection flow rate of the reducing agent is 200-1000 Nm 3 / h; when the fuel is gas, the injection flow rate is 20~400Nm 3 / h, the injection flow rate for solid is 20~400kg / h; the injection flow rate for oxygen-containing gas is 1000~3000Nm 3 / h, the injection flow rate of the sulfiding agent is 50-300kg / h; preferably, when the reducing agent, fuel, oxygen-containing gas and solid in the sulfiding agent are injected, one or more of nitrogen, air and oxygen-enriched air are used as carrier gas for injection; preferably, when the reducing agent, fuel, oxygen-containing gas and gas in the sulfiding agent are injected, the injection pressure is 0.1-0.8MPa.
[0022] Furthermore, during the depletion reaction, the slag type is controlled to be FeO 30-40%, MgO 8-15%, SiO2 30-40%, and CaO 10-15%.
[0023] Furthermore, the nickel content in the high-MgO nickel slag is 0.8-3wt%, and the nickel content in the depleted slag is less than 0.2%.
[0024] The depletion device provided by the present invention is used to carry out depletion treatment on high-MgO nickel slag, which has a better depletion effect. The nickel content in the obtained depleted slag can reach below 0.35%, and the recovery rate of valuable metals such as nickel is improved. It is very suitable for the treatment of high-MgO nickel slag. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0026] Figure 1 A schematic structural diagram of a depletion device suitable for high-MgO nickel slag according to an embodiment of the present invention is shown; and
[0027] Figure 2 Shows Figure 1 Top view of the depletion device suitable for high-MgO nickel slag.
[0028] The above drawings include the following reference numerals:
[0029] 10. Horizontal furnace body; 11. Feeding area; 12. Spraying area; 13. Electrode area; 14. Sedimentation area; 15. Discharging area; 111. High MgO nickel slag inlet; 141. Smoke outlet; 151. Nickel matte discharge port; 152. Slag discharge port; 20. Spray gun; 21. Side-blowing spray gun; 22. Top-blowing spray gun; 30. Electrode; 40. Chimney. DETAILED DESCRIPTION
[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0031] Terminology explanation:
[0032] Smelting: It is an important step in the pyrometallurgical process of nickel-containing materials, preparing a eutectic of main metal sulfide and iron sulfide called matte.
[0033] Nickel slag: a by-product produced during the pyrometallurgical smelting process of nickel-containing ores, including but not limited to nickel smelting slag, blowing slag, electric furnace slag, etc.
[0034] Side blowing: a smelting method in which reactants are blown into the furnace from the side.
[0035] As described in the background technology of the present invention, in the prior art, the high-MgO nickel slag electric furnace depletion process has the problems of high nickel content in the tailings, poor utilization of reducing agents, insufficient slag-matte separation, etc., which lead to poor depletion effect. In order to solve the above problems, the present invention provides a depletion device suitable for high-MgO nickel slag, such as Figure 1 and2 As shown, the depletion device comprises a horizontal furnace body 10, at least two spray guns 20, and an electrode 30; the horizontal furnace body 10 has a first end and a second end opposite to the first end, and along the direction from the first end to the second end, the inner cavity of the horizontal furnace body 10 comprises a feeding area 11, a spraying area 12, an electrode area 13, a settling area 14, and a discharge area 15 which are connected in sequence; the feeding area 11 is provided with a high MgO nickel slag inlet 111; the spraying area 12 is provided with at least two spray ports, and a part of the spray ports is provided with At the top of the injection zone 12, another part of the injection ports are arranged on the side of the injection zone 12; the sedimentation zone 14 is provided with a smoke outlet 141; the discharge zone 15 is provided with a nickel matte discharge port 151 and a slag discharge port 152; the spray gun 20 is connected to each injection port one by one; the spray gun 20 is used to spray the reducing agent, fuel, oxygen-containing gas and sulfiding agent into the injection zone 12; the electrode 30 is arranged in the electrode zone 13, and the electrode 30 extends through the top wall of the electrode zone 13 to the inside of the electrode zone 13 and performs electrode heating.
[0036] The depletion device provided by the present invention integrates the functions of side-blowing and top-blowing reduction, sulfurization, heating and sedimentation separation on the basis of the depletion electric furnace, realizes the reduction + sulfurization + depletion + sedimentation separation in the dual heating form of electrode heating and fuel heating, and effectively improves the depletion effect. Specifically, in the depletion device of the present invention, the inner cavity of the horizontal furnace body 10 includes a feeding area 11, a blowing area 12, an electrode area 13, a sedimentation area 14 and a discharge area 15 connected in sequence. In the actual process of treating high-MgO nickel slag, after feeding it from the high-MgO nickel slag inlet 111, a reducing agent, a fuel, an oxygen-containing gas and a sulfurizing agent are sprayed into the inside of the blowing area 12 through a spray gun 20, and supplementary heat is performed inside the electrode area 13 through an electrode 30. The material sprayed by the spray gun 20 can increase the reducing atmosphere of the molten pool, accelerate the chemical reaction from the perspective of reaction kinetics, improve the slag-matte separation conditions, and reduce the adhesion of the furnace wall. The fuel sprayed in and the oxygen-containing gas combustion provide heat combined with electrode heating to maintain or increase the melt temperature, reduce the slag viscosity, and promote chemical reactions and slag-matte separation. Spraying a sulfiding agent can also further improve the depletion effect. After the depletion reaction in the spraying zone 12 and the electrode zone 13, the material enters the sedimentation zone and can be fully settled to form slag-matte separation, and is discharged from the nickel matte discharge port 151 and the slag discharge port 152 of the discharge zone 15. In addition, when the above-mentioned depletion device is used to treat high-MgO nickel slag, the reducing agent is more fully utilized, and the form of spraying + electric heating is more energy-saving and has a higher heat utilization rate.
[0037] Therefore, the use of the depletion device provided by the present invention to carry out depletion treatment on high-MgO nickel slag has a better depletion effect, and the nickel content in the obtained depleted slag can reach below 0.35%. At the same time, the recovery rate of valuable metals such as nickel is improved, which is very suitable for the treatment of high-MgO nickel slag.
[0038] In order to give full play to the role of each zone, while using the injection material to improve the kinetic conditions and thus cooperate with the electrode heating to better achieve the depletion effect, the comprehensive purpose of further reducing the nickel content in the slag, improving the nickel recovery rate, and improving the sedimentation separation effect is achieved. In a preferred embodiment, the total length of the horizontal furnace body 10 from the first end to the second end is recorded as L, the length of the feeding zone 11 is recorded as L1, the length of the injection zone 12 is recorded as L2, the length of the electrode zone 13 is recorded as L3, the length of the sedimentation zone 14 is recorded as L4, and the length of the discharge zone 15 is recorded as L5, then L1 / L=1 / 15~1 / 8, L2 / L=1 / 8~1 / 5, L3 / L=1 / 2~3 / 5, L4 / L=1 / 8~1 / 5, L5 / L=1 / 15~1 / 8. In this way, material blowing is performed in the front section of the horizontal furnace body 10 to increase the dynamic conditions and stir the molten pool; electrode heating is performed in the middle section to promote a more complete depletion reaction; sedimentation separation is performed in the rear section to further improve the recovery rate of valuable metals and reduce the content of valuable metals such as Ni, Co, Cu, and precious metals in the tailings. The combination of each section has a more comprehensive excellent effect. More preferably, L1 / L=1 / 15~1 / 3, L2 / L=1 / 8~1 / 6, L3 / L=1 / 2~3 / 5, L4 / L=1 / 6~1 / 5, and L5 / L=1 / 15~1 / 13.
[0039] In a preferred embodiment, the horizontal furnace body 10 is a rectangular furnace body (such as Figure 1 and 2 The furnace body is a rectangular furnace body (as shown in the figure) or a rectangular furnace body, and the length direction from the first end to the second end is the length direction, and the furnace body is 20 to 40 meters long, 5 to 10 meters wide, and 5 to 10 meters high. Setting the overall size to the above range is more suitable for the actual nickel slag production and can give full play to the advantages of each functional area. More preferably, the furnace body is 20 to 30 meters long, 6 to 8 meters wide, and 7 to 8 meters high.
[0040] According to the size of the furnace body, those skilled in the art can select the specific number of spray guns. In a preferred embodiment, the spraying zone 12 is provided with 2 to 12 spray ports, and the depletion device includes 2 to 12 spray guns 20, and the spray guns 20 are connected to each spray port one by one. Setting such a number of spray guns makes the spraying of each material more uniform and more suitable for the processing amount of nickel slag. More preferably, the electrode 30 is 1 to 4 groups of three-phase electrodes, and the power of the electrode 30 is 5 to 15 MVA. With such a setting, combined with the spraying of materials by the spray gun, the temperature of the molten pool is more uniform and appropriate, and the depletion effect and sedimentation separation effect are better.
[0041] Exemplarily, the reducing agent includes but is not limited to one or more of pulverized coal, natural gas, and hydrogen; the fuel includes but is not limited to one or more of natural gas, pulverized coal, carbon powder, heavy oil, liquefied petroleum gas, shale gas, and coalbed methane; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 21 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
[0042] In order to further enhance the reaction efficiency and improve the depletion effect, in a preferred embodiment, the lance 20 includes a side-blowing lance 21 and a top-blowing lance 22. The side-blowing lance 21 is inserted horizontally or obliquely downward into the slag melt layer through the blowing port on the side of the blowing zone 12, and the top-blowing lance 22 is inserted vertically into the slag melt layer through the blowing port at the top of the blowing zone 12. More preferably, the distance between the nozzle of the side-blowing lance 21 and the bottom wall of the blowing zone 12 is 0.8 to 2 meters, and the distance between the nozzle of the top-blowing lance 22 and the bottom wall of the blowing zone 12 is 0.5 to 2 meters.
[0043] In a preferred embodiment, the side-blowing lance 21 is used to spray the solids among the reducing agent, fuel, oxygen-containing gas and sulfiding agent, and the top-blowing lance 22 is used to spray the gas and liquid among the reducing agent, fuel, oxygen-containing gas and sulfiding agent. This spraying method is more conducive to improving the kinetic conditions of the depletion reaction, improving the reaction depth, and maintaining the molten pool temperature to further improve the sedimentation separation effect, promote slag-matte separation, and reduce furnace wall adhesion.
[0044] Preferably, there is one high-MgO nickel slag inlet 111 , which is arranged at the top of the feeding area 11 ; there are 2 to 4 nickel matte discharge ports 151 , which are arranged at the bottom of the discharge area 15 ; there are 2 to 5 slag discharge ports 152 , which are arranged at the side of the discharge area 15 .
[0045] A large amount of flue gas will also be generated during the above depletion reaction. In a preferred embodiment, Figure 1As shown, the depletion device also includes: a chimney 40, which is arranged at the smoke outlet 141, and a secondary combustion device is arranged in the chimney 40, which is used to perform secondary combustion on the depleted flue gas discharged from the smoke outlet 141 to obtain secondary combustion flue gas (mainly composed of SO2 and CO2); a dust collection and purification unit, which is connected to the chimney 40 and is used to perform dust collection and purification on the secondary combustion flue gas. CO, S, etc. in the depleted flue gas can be further burned by the secondary combustion device, and then the dust is removed by the dust collection and purification unit. More preferably, a waste heat boiler is also arranged between the chimney 40 and the dust collection and purification unit, which is used to recover the waste heat of the secondary combustion flue gas before dust collection and purification. In the actual processing process, the temperature of the depleted flue gas discharged from the smoke outlet 141 can often reach about 1350°C, and the secondary combustion flue gas can be initially cooled to about 350°C by the waste heat boiler. Further preferably, a surface cooler is also arranged between the waste heat boiler and the dust collection and purification unit, so that the secondary combustion flue gas can be further cooled. The specific dust collection and purification unit is preferably a bag dust collector or an electric dust collector. After dust collection and purification, the purified flue gas can be sent to the tail gas desulfurization system for treatment, and the flue dust is transported back to the smelting batching and granulation process of the nickel-containing material to participate in the preparation of the nickel-containing material.
[0046] According to another aspect of the present invention, there is also provided a method for impoverishing high-MgO nickel slag, wherein the MgO content in the high-MgO nickel slag is 6 to 20 wt%. The present invention adopts the above-mentioned impoverishment device to carry out impoverishment treatment on the high-MgO nickel slag, and the impoverishment treatment process comprises the following steps: introducing high-MgO nickel slag into the horizontal furnace body 10 through the high-MgO nickel slag inlet 111; spraying reducing agent, fuel, oxygen-containing gas and sulfiding agent into the spraying zone 12 through the spray gun 20, and at the same time opening the electrode 30 to perform electrode heating on the electrode zone 13, so that the high-MgO nickel slag undergoes an impoverishment reaction inside the horizontal furnace body 10; sedimenting and separating the melt after the impoverishment reaction through the sedimentation zone 14 to form nickel matte and impoverished slag; discharging the nickel matte from the nickel matte discharge port 151 of the discharge zone 15, and discharging the impoverished slag from the slag discharge port 152 of the discharge zone 15.
[0047] The depletion device provided by the present invention integrates the functions of side-blowing and top-blowing reduction, sulfurization, heating and sedimentation separation on the basis of the depletion electric furnace, realizes the reduction + sulfurization + depletion + sedimentation separation in the dual heating form of electrode heating and fuel heating, and effectively improves the depletion effect. Specifically, in the depletion device of the present invention, the inner cavity of the horizontal furnace body 10 includes a feeding area 11, a blowing area 12, an electrode area 13, a sedimentation area 14 and a discharge area 15 connected in sequence. In the actual process of treating high-MgO nickel slag, after feeding it from the high-MgO nickel slag inlet 111, a reducing agent, a fuel, an oxygen-containing gas and a sulfurizing agent are sprayed into the inside of the blowing area 12 through a spray gun 20, and supplementary heat is performed inside the electrode area 13 through an electrode 30. The material sprayed by the spray gun 20 can increase the reducing atmosphere of the molten pool, accelerate the chemical reaction from the perspective of reaction kinetics, improve the slag-matte separation conditions, and reduce the adhesion of the furnace wall. The fuel sprayed in and the oxygen-containing gas combustion provide heat combined with electrode heating to maintain or increase the melt temperature, reduce the slag viscosity, and promote chemical reactions and slag-matte separation. Spraying a sulfiding agent can also further improve the depletion effect. After the depletion reaction in the spraying zone 12 and the electrode zone 13, the material enters the sedimentation zone and can be fully settled to form slag-matte separation, and is discharged from the nickel matte discharge port 151 and the slag discharge port 152 of the discharge zone 15. In addition, when the above-mentioned depletion device is used to treat high-MgO nickel slag, the reducing agent is more fully utilized, and the form of spraying + electric heating is more energy-saving and has a higher heat utilization rate.
[0048] Therefore, the use of the depletion device provided by the present invention to carry out depletion treatment on high-MgO nickel slag has a better depletion effect, and the nickel content in the obtained depleted slag can reach below 0.35%. At the same time, the recovery rate of valuable metals such as nickel is improved, which is very suitable for the treatment of high-MgO nickel slag.
[0049] In order to further improve the depletion effect, reduce the nickel content in the depleted slag, and increase the nickel recovery rate in the nickel slag, in a preferred embodiment, during the depletion reaction, the temperature inside the horizontal furnace body 10 is controlled to be 1000-1600°C. More preferably, the temperature inside the horizontal furnace body 10 is controlled to be 1300-1400°C. At such a depletion reaction temperature, valuable metals such as nickel can more fully enter the nickel matte and be fully separated from the depleted slag. At this time, the slag discharge temperature is about 1280-1350°C, and the furnace wall bonding is further improved.
[0050] In a preferred embodiment, the reducing agent is selected from one or more of pulverized coal, natural gas, and hydrogen; the fuel is selected from one or more of natural gas, pulverized coal, carbon powder, and heavy oil; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 22 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
[0051] In order to give full play to the reducing effect, heating effect, sulfurization effect, and improvement of kinetic conditions of the injected materials and achieve better depletion effect, in a preferred embodiment, the injection flow rate of the reducing agent is 200-1000 Nm 3 / h; the fuel injection flow rate is 20~400Nm 3 / h, the injection flow rate for solid is 20~400kg / h; the injection flow rate for oxygen-containing gas is 1000~3000Nm 3 / h; the injection flow rate of the sulfiding agent is 50-300kg / h; preferably, when injecting the reducing agent, fuel, oxygen-containing gas and solid in the sulfiding agent, one or more of nitrogen, air and oxygen-enriched air are used as carrier gas for injection; preferably, when injecting the reducing agent, fuel, oxygen-containing gas and gas in the sulfiding agent, the injection pressure is 0.1-0.8MPa. Under the above-mentioned injection process, the functions of stirring the molten pool, heating the body temperature and providing a reducing atmosphere can be more fully exerted, and it is also beneficial to further reduce the Fe3O4 content in the slag (can be reduced to less than 5%), reduce the viscosity of the slag, and create favorable conditions for the second half of the sedimentation.
[0052] In order to make slag formation more complete and make the temperature of the depletion reaction process more suitable, in a preferred embodiment, during the depletion reaction process, the slag type is controlled to be 30-40% FeO, 8-15% MgO, 30-40% SiO2, and 10-15% CaO. Specifically, it is preferred to add flux such as lime to control the slag type when feeding nickel slag.
[0053] The present invention is more suitable for treating high-MgO nickel slag, and its depletion effect is more significant. In a more preferred embodiment, the nickel content in the high-MgO nickel slag is 0.8-3wt%, and the nickel content in the depleted slag is less than 0.2%.
[0054] In the actual processing process, after the nickel slag is treated by the above-mentioned depletion device, the obtained nickel matte can be recycled to the previous smelting process and the generated depleted slag can be dumped or used for other purposes.
[0055] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0056] Example 1
[0057] use Figure 1 and 2 The depletion unit shown treats high-MgO nickel slag, the main components of which are as follows:
[0058]
[0059] The depletion device includes a horizontal furnace body, 6 side-blowing lances, 3 top-blowing lances, and 2 sets of three-phase electrodes; the horizontal furnace body is a rectangular furnace body with a length of 30 meters, a width of 8 meters, and a height of 7 meters. The inner cavity of the horizontal furnace body includes a feeding area, a blowing area, an electrode area, a settling area, and a discharge area that are connected in sequence, wherein L1 / L=1 / 15, L2 / L=1 / 6, L3 / L=1 / 2, L4 / L=1 / 5, and L5 / L=1 / 15; a high-MgO nickel slag inlet is provided in the feeding area; 9 blowing ports are provided in the blowing area, wherein 3 blowing ports are provided at the top, and 6 blowing ports are evenly provided at the front and rear sides of the blowing area; a smoke outlet is provided at the top of the settling area, which is connected to the chimney, and the chimney A secondary combustion burner is arranged in the middle; two nickel matte discharge ports, one in front and one in the back, are arranged in the discharge area, and three slag discharge ports are arranged on the end side wall; the spray guns are connected to each injection port one by one; the spray guns are used to spray reducing agent (natural gas), fuel (pulverized coal), oxygen-containing gas (oxygen-enriched air with an oxygen volume content of 60-80%) and sulfiding agent (nickel concentrate) into the injection area; the electrode is arranged in the electrode area, and the electrode passes through the top wall of the electrode area to extend to the inside of the electrode area and performs electrode heating, and its power is 10MVA.
[0060] The specific operation process is as follows:
[0061] High MgO nickel smelting slag is added into the furnace chamber of a horizontal furnace body; while adding the nickel slag, flux lime and the like are added to adjust the slag type and melting point of the molten pool in the furnace, the smelting temperature is controlled at 1300-1400°C, and the slag type is controlled to be: FeO 40%, MgO 8%, SiO2 40%, CaO 15%.
[0062] Six side-blowing spray guns are used to spray oxygen-enriched air and natural gas into the furnace from the side of the spray zone. The distance between the nozzle and the bottom wall of the spray zone is 0.8 to 2 meters. The oxygen-enriched concentration is 60%. The oxygen-enriched air volume of each side-blowing spray gun is 500Nm 3 / h, natural gas volume 100Nm 3 / h; using 3 top-blowing spray guns with air as carrier gas to add reducing agent pulverized coal and sulfiding agent nickel concentrate from the top of the spraying zone, the distance between the nozzle and the bottom wall of the spraying zone is 0.5 to 2 meters, and each top-blowing spray gun sprays 50kg / h of pulverized coal and 30kg / h of nickel concentrate to reduce and deplete the nickel slag;
[0063] After depletion, the melt is heated by electrodes in the electrode zone and separated by sedimentation in the sedimentation zone to generate nickel matte and depleted slag. When the slag layer in the furnace reaches a certain thickness, it is semi-continuously discharged from the slag discharge port at one end of the depletion furnace. The slag discharge temperature is about 1280-1350℃.
[0064] The temperature of the smelting flue gas produced by the depletion reaction is about 1350℃. The CO in the flue gas is secondary burned after air leakage in the upper part of the furnace body and the ascending flue. After the waste heat boiler initially cools the gas to 350℃ to recover the waste heat, it is cooled by the surface cooler and dusted by the bag filter before being sent to the tail gas desulfurization treatment. The smoke dust is transported back to the batching and granulation process to participate in the preparation of nickel-containing materials.
[0065] The products after depletion are nickel matte (low nickel matte) and depleted slag. In terms of mass percentage, the content of Ni in nickel matte is 6-25%, the content of Fe is 45-65%, and the content of S is 10-25%. The discharge temperature of nickel matte is about 1340℃. The nickel content in depleted slag is less than 0.2%, which is stored or sold as general solid waste after water crushing.
[0066] Example 2
[0067] use Figure 1 and 2 The depletion unit shown treats high-MgO nickel slag, the main components of which are as follows:
[0068]
[0069] The depletion device includes a horizontal furnace body, 4 side-blowing lances, 2 top-blowing lances, and 2 sets of three-phase electrodes; the horizontal furnace body is a rectangular furnace body with a length of 20 meters, a width of 6 meters, and a height of 7 meters. The inner cavity of the horizontal furnace body includes a feeding area, a blowing area, an electrode area, a settling area, and a discharge area that are connected in sequence, wherein L1 / L=1 / 13, L2 / L=1 / 8, L3 / L=3 / 5, L4 / L=1 / 8, and L5 / L=1 / 13; a high-MgO nickel slag inlet is provided in the feeding area; 6 blowing ports are provided in the blowing area, wherein 2 blowing ports are provided at the top, and 4 blowing ports are provided at the front and rear sides of the blowing area in a front-to-back manner; a smoke outlet is provided at the top of the settling area, which is connected to the chimney, and the chimney A secondary combustion burner is arranged in the middle; two nickel matte discharge ports, one in front and one in the back, are arranged in the discharge area, and three slag discharge ports are arranged on the end side wall; the spray guns are connected to each injection port one by one; the spray guns are used to spray reducing agent (natural gas), fuel (pulverized coal), oxygen-containing gas (oxygen-enriched air with an oxygen volume content of 70%) and sulfiding agent (nickel concentrate) into the injection area; the electrode is arranged in the electrode area, and the electrode passes through the top wall of the electrode area to extend to the inside of the electrode area and performs electrode heating, and its power is 15MVA.
[0070] The specific operation process is as follows:
[0071] High MgO nickel smelting slag is added into the furnace chamber of a horizontal furnace body; while adding the nickel slag, flux lime and the like are added to adjust the slag type and melting point of the molten pool in the furnace, the smelting temperature is controlled at 1300-1400°C, and the slag type is controlled to be: FeO 30%, MgO 8%, SiO2 40%, CaO 15%.
[0072] Six side-blowing spray guns are used to spray oxygen-enriched air and natural gas into the furnace from the side of the spray zone. The distance between the nozzle and the bottom wall of the spray zone is 0.8 to 2 meters. The oxygen-enriched concentration is 80%. The oxygen-enriched air volume of each side-blowing spray gun is 500Nm 3 / h, natural gas volume 100Nm 3 / h; using 3 top-blowing spray guns with air as carrier gas to add reducing agent pulverized coal and sulfiding agent nickel concentrate from the top of the spraying zone, the distance between the nozzle and the bottom wall of the spraying zone is 0.5 to 2 meters, and each top-blowing spray gun sprays 50kg / h of pulverized coal and 30kg / h of nickel concentrate to reduce and deplete the nickel slag;
[0073] After depletion, the melt is heated by electrodes in the electrode zone and separated by sedimentation in the sedimentation zone to generate nickel matte and depleted slag. When the slag layer in the furnace reaches a certain thickness, it is semi-continuously discharged from the slag discharge port at one end of the depletion furnace. The slag discharge temperature is about 1280-1350℃.
[0074] The temperature of the smelting flue gas produced by the depletion reaction is about 1350℃. The CO in the flue gas is secondary burned after air leakage in the upper part of the furnace body and the ascending flue. After the waste heat boiler initially cools the gas to 350℃ to recover the waste heat, it is cooled by the surface cooler and dusted by the bag filter before being sent to the tail gas desulfurization treatment. The smoke dust is transported back to the batching and granulation process to participate in the preparation of nickel-containing materials.
[0075] The products after depletion are nickel matte (low nickel matte) and depleted slag. In terms of mass percentage, the content of Ni in nickel matte is 20-25%, the content of Fe is 40-50%, and the content of S is 20-25%. The discharge temperature of nickel matte is about 1380℃. The nickel content in depleted slag is less than 0.2%, which is stored or sold as general solid waste after water crushing.
[0076] In conclusion, the present invention effectively improves the depletion efficiency and effect, increases the nickel recovery rate, and reduces the nickel content in the depleted slag.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A depletion device suitable for high-MgO nickel slag, characterized in that: include: A horizontal furnace body (10), the horizontal furnace body (10) having a first end and a second end opposite to the first end, and along the direction from the first end to the second end, the inner cavity of the horizontal furnace body (10) comprises a feeding zone (11), a blowing zone (12), an electrode zone (13), a settling zone (14) and a discharge zone (15) which are connected in sequence; the feeding zone (11) is provided with a high-MgO nickel slag inlet (111); the blowing zone (12) is provided with at least two blowing ports, wherein a part of the blowing ports is provided at the top of the blowing zone (12), and another part of the blowing ports is provided at the side of the blowing zone (12); the settling zone (14) is provided with a smoke outlet (141); the discharge zone (15) is provided with a nickel matte discharge port (151) and a slag discharge port (152); at least two spray guns (20), the spray guns (20) being connected to the respective spray ports one by one; the spray guns (20) being used to spray the reducing agent, the fuel, the oxygen-containing gas and the sulfiding agent into the spraying zone (12); An electrode (30) is arranged in the electrode area (13), and the electrode (30) passes through the top wall of the electrode area (13) and extends to the interior of the electrode area (13) to perform electrode heating.
2. The depletion device according to claim 1, characterized in that: The total length of the horizontal furnace body (10) along the direction from the first end to the second end is recorded as L, the length of the feeding zone (11) is recorded as L1, the length of the blowing zone (12) is recorded as L2, the length of the electrode zone (13) is recorded as L3, the length of the settling zone (14) is recorded as L4, and the length of the discharge zone (15) is recorded as L5, then L1 / L=1 / 15-1 / 8, L2 / L=1 / 8-1 / 5, L3 / L=1 / 2-3 / 5, L4 / L=1 / 8~1 / 5, L5 / L=1 / 15~1 / 8.
3. The depletion device according to claim 1, characterized in that: The blowing zone (12) is provided with 2 to 12 blowing ports, the depletion device comprises 2 to 12 spray guns (20), and the spray guns (20) are connected to each of the blowing ports in a one-to-one correspondence; the electrode (30) is 1 to 4 groups of three-phase electrodes, and the power of the electrode (30) is 5 to 15 MVA.
4. The depletion device according to claim 1, characterized in that: The reducing agent is selected from one or more of pulverized coal, natural gas, and hydrogen; the fuel is selected from one or more of natural gas, pulverized coal, carbon powder, heavy oil, liquefied petroleum gas, shale gas, and coalbed methane; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 21 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
5. The depletion device according to any one of claims 1 to 4, characterized in that: The horizontal furnace body (10) is a rectangular furnace body or a quasi-rectangular furnace body, and the direction from the first end to the second end is the length direction. The furnace body is 20 to 40 meters long, 5 to 10 meters wide, and 5 to 10 meters high.
6. The depletion device according to claim 5, characterized in that The spray gun (20) includes a side-blowing spray gun (21) and a top-blowing spray gun (22). The side-blowing spray gun (21) is inserted horizontally or obliquely downward into the slag melt layer through the spray port at the side of the spray zone (12), and the top-blowing spray gun (22) is inserted vertically into the slag melt layer through the spray port at the top of the spray zone (12).
7. The depletion device according to claim 6, characterized in that The distance between the nozzle of the side-blowing lance (21) and the bottom wall of the blowing zone (12) is 0.8 to 2 meters, and the distance between the nozzle of the top-blowing lance (22) and the bottom wall of the blowing zone (12) is 0.5 to 2 meters.
8. The depletion device according to claim 6, characterized in that The side-blowing lance (21) is used for spraying the reducing agent, the fuel, the oxygen-containing gas and the solids in the sulfiding agent, and the top-blowing lance (22) is used for spraying the reducing agent, the fuel, the oxygen-containing gas and the gas and liquid in the sulfiding agent.
9. The depletion device according to any one of claims 1 to 8, characterized in that The number of the high-MgO nickel slag inlet (111) is one and is arranged at the top of the feeding area (11); the number of the nickel matte discharge ports (151) is 2 to 4 and is arranged at the bottom of the discharge area (15); the number of the slag discharge ports (152) is 2 to 5 and is arranged at the side of the discharge area (15).
10. The depletion device according to any one of claims 1 to 8, characterized in that The depletion device also includes: A chimney (40) is arranged at the smoke outlet (141), and a secondary combustion device is arranged in the chimney (40) for performing secondary combustion on the depleted smoke discharged from the smoke outlet (141) to obtain secondary combustion smoke; A dust collection and purification unit is connected to the chimney (40) and is used for collecting and purifying the secondary combustion flue gas.
11. A method for depleting high-MgO nickel slag, wherein the MgO content in the high-MgO nickel slag is 6-20wt%, characterized in that: The high-MgO nickel slag is subjected to a depletion treatment using a depletion device according to any one of claims 1 to 10, wherein the depletion treatment process comprises the following steps: introducing the high-MgO nickel slag into the horizontal furnace body (10) through a high-MgO nickel slag inlet (111); A reducing agent, a fuel, an oxygen-containing gas and a sulfiding agent are sprayed into the spraying zone (12) through a spray gun (20), and at the same time, the electrode (30) is turned on to perform electrode heating on the inside of the electrode zone (13), so that the high-MgO nickel slag undergoes a depletion reaction inside the horizontal furnace body (10); The melt after the depletion reaction is subjected to sedimentation and separation in a sedimentation zone (14) to form nickel matte and depleted slag; the nickel matte is discharged from a nickel matte discharge port (151) of a discharge zone (15), and the depleted slag is discharged from a slag discharge port (152) of the discharge zone (15).
12. The depletion method according to claim 11, characterized in that: During the depletion reaction, the temperature inside the horizontal furnace body (10) is controlled to be 1000-1600° C., preferably 1300-1400° C.
13. The depletion method according to claim 12, characterized in that: The reducing agent is selected from one or more of pulverized coal, natural gas, and hydrogen; the fuel is selected from one or more of natural gas, pulverized coal, carbon powder, and heavy oil; the oxygen-containing gas is air or oxygen-enriched air, and the oxygen volume content in the oxygen-enriched air is preferably 22 to 90%, more preferably 60 to 80%; the sulfiding agent is selected from one or more of nickel sulfide ore, pyrite, sulfur powder, and gypsum powder.
14. The depletion method according to any one of claims 11 to 13, characterized in that: The injection flow rate of the reducing agent is 200-1000 Nm 3 / h; when the fuel is gas, the injection flow rate is 20 to 400 Nm 3 / h, the injection flow rate of solid is 20~400kg / h; the injection flow rate of the oxygen-containing gas is 1000~3000Nm 3 / h, the injection flow rate of the sulfiding agent is 50-300kg / h; preferably, when the reducing agent, the fuel, the oxygen-containing gas and the solid in the sulfiding agent are injected, one or more of nitrogen, air and oxygen-enriched air are used as carrier gases for injection; preferably, when the reducing agent, the fuel, the oxygen-containing gas and the gas in the sulfiding agent are injected, the injection pressure is 0.1-0.8MPa.
15. The depletion method according to claim 14, characterized in that: During the depletion reaction, the slag type is controlled to be FeO 30-40%, MgO 8-15%, SiO2 30-40%, and CaO 10-15%.
16. The depletion method according to any one of claims 11 to 15, characterized in that The nickel content in the high-MgO nickel slag is 0.8-3wt%, and the nickel content in the depleted slag is less than 0.2%.