Preparation method and use method of ultra-high-purity cadmium

By employing a two-stage vacuum volatilization melting method, the preparation process of high-purity cadmium was simplified, effectively removing both low-boiling-point and high-boiling-point impurities, improving purification efficiency, and obtaining high-purity 6N cadmium. This solved the problems of complex processes and high material waste rates in existing technologies.

CN119020606APending Publication Date: 2024-11-26YINTAI SCI & TECH HIGH TECH ZONE LIUZHOU CITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049650.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing technologies for preparing high-purity cadmium involve complex processes, low processing efficiency, and high material waste, making it difficult to effectively remove impurities, especially low-boiling-point and high-boiling-point impurities.

Method used

A two-stage vacuum volatilization melting method is adopted. First, low-boiling-point impurities are removed at 500-700℃, then the main cadmium metal is removed and condensed and collected at 800-900℃, and finally high-boiling-point impurities are left, which simplifies the process and improves the purification efficiency.

Benefits of technology

The preparation process was simplified, the purification efficiency was improved, and the production cost was reduced, resulting in high-purity 6N cadmium that meets the purity requirements of high-tech fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974549510000051
    Figure BDA0004974549510000051
  • Figure BDA0004974549510000061
    Figure BDA0004974549510000061
Patent Text Reader

Abstract

The invention relates to a preparation method and a use method of ultra-high-purity cadmium, and belongs to the field of high-purity metal preparation. The invention provides a preparation method of ultra-high-purity cadmium. The preparation method mainly comprises the following steps: S1) carrying out first-time vacuum volatilization smelting on raw material cadmium at 500-700 DEG C to remove low-boiling-point volatile impurities in the raw material cadmium in a metal vapor manner; s2) performing secondary vacuum volatilization smelting on the raw material cadmium in the step S1) at 800-900 DEG C, so that the metal main body cadmium in the raw material cadmium is volatilized; and (S3) condensing and collecting the cadmium metal steam in the step (S2) to obtain ultra-high-purity cadmium, wherein high-boiling-point and non-volatile impurities in the ultra-high-purity cadmium are left in residual materials. According to the method, two types of impurities in metal cadmium can be effectively removed by adopting a two-time vacuum high-temperature smelting volatilization process to extract high-purity cadmium, namely, low-boiling-point volatile impurities are removed in the step S1, then non-volatile impurities in the metal cadmium are removed in the step S2, and finally 6N high-purity cadmium is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-purity metal preparation, and relates to a preparation method and a use method of ultra-high purity cadmium, and specifically, to a preparation method of 6N high-purity cadmium. Background Art

[0002] High-purity cadmium is widely used in high-tech fields such as semiconductors, optoelectronic materials and electronic devices, and energy materials for energy storage and nuclear energy. With the continuous development of high-tech fields, these fields have higher and higher requirements for material purity, and the technology for preparing high-purity cadmium has gradually attracted widespread attention. At present, the commonly used methods for preparing high-purity cadmium mainly include electrolytic refining, chemical precipitation, vacuum volatilization smelting, etc. Among them, the electrolytic refining method usually uses crude cadmium as a raw material to cast an anode in the preparation of high-purity cadmium. During the electrolysis process, impurities such as Pb, Zn, and TI are close to cadmium in potential and easily enter the electrolyte, thereby affecting the progress of the electrolysis process. Taking Pb as an example, Pb entering the electrolyte will change the pH value of the electrolyte, affect the stability and efficiency of the electrolysis process, and form a precipitation layer on the surface of the anode, thereby shortening the electrode life and affecting the progress of the electrolysis process. The process with patent number CN201110448870.1 adopts the method of placing the raw material cadmium in a zone melting tube and passing a reducing gas to melt it, repeating the above operation to finally obtain high-purity cadmium. The process technology for preparing high-purity cadmium by heating and smelting is complex, with low processing efficiency and high material waste rate.

[0003] In view of this, a method of using two vacuum volatilization smeltings to prepare 6N high-purity cadmium is proposed, and the advantages of vacuum volatilization smelting are used to solve the problems of the traditional process for preparing 6N high-purity cadmium: complex process, low processing efficiency and high material waste rate. Summary of the invention

[0004] Technical issues to be solved

[0005] In order to avoid the shortcomings of the prior art, the present invention proposes a preparation method and a use method of ultra-high purity cadmium, and provides a preparation method for 6N high-purity cadmium based on two vacuum volatilization smelting processes, thereby overcoming the defects of the above-mentioned prior art.

[0006] Technical Solution

[0007] A method for preparing ultra-high purity cadmium, characterized in that the steps are as follows:

[0008] Step 1: subjecting the raw material cadmium to a first vacuum volatilization smelting at 500 to 700°C to remove low-boiling-point volatile impurities in the raw material cadmium in the form of metal vapor;

[0009] Step 2: subjecting the raw material cadmium treated in step 1 to a second vacuum volatilization smelting at 800-900° C., so that the main metal cadmium in the raw material cadmium is volatilized to obtain metal cadmium vapor;

[0010] Step 3: Condensing and collecting the metallic cadmium vapor obtained in step 2 to obtain 6N ultra-high purity cadmium.

[0011] The vacuum degree of the vacuum volatilization in step 1 and step 2 is 1.0-9.0×10 -3 -10 -5 Pa.

[0012] The vacuum volatilization time in step 1 is 2.00-6.00 hours.

[0013] The vacuum volatilization time of step 1 is 6.00-12.00 hours.

[0014] The raw material cadmium includes one or more of crude cadmium and refined cadmium.

[0015] The heating process of step 1 uses induction heating to gradually increase the temperature: the raw cadmium is placed in a mold and preheated at 200° C.-400° C. for 0.50-1.00 h, and then heated at 500° C.-700° C. for 2.00-6.00 h to perform the first vacuum volatilization melting.

[0016] The heating process in step 2 uses induction heating to gradually increase the temperature: the raw cadmium obtained in step 1 is heated at 800° C.-900° C. for 6.00-12.00 hours, and a second vacuum volatilization smelting is performed to obtain metallic cadmium vapor.

[0017] The low-boiling-point volatile impurities in step 1 include one or more of zinc, aluminum, magnesium, lead, and thallium.

[0018] The high boiling point and non-volatile impurities in step 2 include one or more of copper, iron, tin, silicon and sulfur.

[0019] A method for using the ultra-high purity cadmium prepared by the method, characterized in that the ultra-high purity cadmium is used in semiconductors, optoelectronic materials and electronic devices, and energy materials are used in energy storage and nuclear energy high-tech fields.

[0020] Beneficial Effects

[0021] The present invention proposes a method for preparing ultra-high purity cadmium and a method for using the same, which belong to the field of high-purity metal preparation. The method for preparing ultra-high purity cadmium provided by the present invention mainly comprises: S1) subjecting the raw material cadmium to a first vacuum volatilization smelting at 500 to 700°C to remove low-boiling volatile impurities in the raw material cadmium in the form of metal vapor; S2) subjecting the raw material cadmium in S1) to a second vacuum volatilization smelting at 800-900°C to volatilize the metal main body cadmium in the raw material cadmium; S3) condensing and collecting the metal cadmium vapor in S2) to obtain ultra-high purity cadmium, while the high-boiling non-volatile impurities therein remain in the residue. The present invention can effectively remove two types of impurities in metal cadmium by using two vacuum high-temperature smelting and volatilization processes to refine high-purity cadmium: first, low-boiling volatile impurities are removed in S1), and secondly, non-volatile impurities in metal cadmium are removed in S2), and finally 6N high-purity cadmium is obtained. DETAILED DESCRIPTION

[0022] The present invention will be further described with reference to the embodiments:

[0023] The object of the present invention is to provide a method for preparing 6N high-purity cadmium based on double vacuum volatilization smelting, thereby overcoming the defects of the above-mentioned prior art. In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below.

[0024] The method for preparing ultra-high purity cadmium of the present invention comprises: firstly, heating the raw material cadmium at 1.0-9.0×10 -3 -10 -5 Pa, the low-boiling-point volatile impurities in the raw cadmium are removed by volatilization in the form of steam by gradually increasing the temperature in the temperature range of 500-700°C by induction heating. Then, the raw cadmium that has undergone the first vacuum volatilization smelting is subjected to the second vacuum volatilization smelting to reduce the raw cadmium to 1.0-9.0×10 -3 -10 -6 Under the vacuum condition of 1.5 Pa, the metal main body cadmium is volatilized by induction heating in the temperature range of 800-900°C, and then the volatilized metal cadmium vapor is condensed and collected in a condensation collection device to obtain 6N high-purity cadmium, and high-boiling point difficult-to-volatilize impurities remain in the residue.

[0025] The raw material cadmium used includes one or more of crude cadmium and refined cadmium.

[0026] The first vacuum volatilization smelting mainly includes gradually heating the raw material cadmium within the temperature range of 500-700°C by induction heating, and removing the low-boiling-point volatile impurities in the raw material cadmium by volatilization through metal vapor. The removed low-boiling-point volatile impurities include at least one of water zinc, aluminum, magnesium, lead, and thallium.

[0027] The second vacuum volatilization smelting mainly includes: subjecting the raw material cadmium that has undergone the first vacuum volatilization smelting to the second vacuum volatilization smelting, using the induction heating method in the temperature range of 800-900°C to volatilize the metal main body cadmium in the raw material cadmium, and then condensing and collecting the volatilized metal cadmium in a condensation collection device to obtain 6N high-purity cadmium, wherein high-boiling-point difficult-to-volatilize impurities are all left in the residue. The removed high-boiling-point difficult-to-volatilize impurities include at least one of copper, iron, tin, silicon and sulfur.

[0028] The first vacuum volatilization smelting and the second vacuum volatilization smelting are respectively carried out in different smelting equipment, and low-boiling-point volatile impurities and metal cadmium vapor are collected by different smelting condensation collection devices.

[0029] The preparation method of 6N high-purity cadmium provided in an embodiment of the present invention uses crude cadmium or refined cadmium as a raw material, and adopts two vacuum volatilization and smelting steps to remove impurities in the raw cadmium: first, low-boiling point volatile impurities, and secondly, high-boiling point difficult-to-volatilize impurities. The present invention proposes a targeted solution for the impurities in the raw cadmium, preferentially removing low-boiling point volatile impurities in the raw cadmium, and adopts a method of preferentially volatilizing metallic cadmium for difficult-to-volatilize impurities. The two steps are combined to effectively remove impurities in the raw cadmium to obtain 6N high-purity cadmium. The above preparation method preferentially volatilizes and removes low-boiling point impurities under relatively low temperature and vacuum conditions, and then volatilizes, condenses and collects the metal main body cadmium under relatively high temperature range and vacuum conditions, leaving high-boiling point difficult-to-volatilize impurities in the residue to obtain 6N high-purity cadmium.

[0030] The present invention adopts a new idea, using a two-step vacuum volatilization smelting method to remove impurities in the raw material cadmium, and finally obtains 6N high-purity cadmium. The above preparation method simplifies the process of preparing high-purity cadmium by the traditional method, and the two-step refining improves the purification efficiency. The new process is simple, the technical conditions are stable, the product quality is reliable, and the production cost is reduced to obtain high-purity cadmium.

[0031] The features and properties of the present invention are further described in detail below with reference to examples.

[0032] Example 1

[0033] A method for preparing 6N high-purity cadmium comprises the following steps:

[0034] The raw material crude cadmium is placed in the crucible of the vacuum distillation equipment, and the vacuum degree is 2.0-9.0×10 -2 Pa, the temperature range is 500-700℃, and the volatile smelting is carried out for 6.00h. The low-boiling point volatile impurities in the raw cadmium are volatilized and removed in the form of steam. Then, the raw cadmium removed by the first vacuum volatilization is subjected to the second vacuum volatilization smelting, and the vacuum degree is 1.0-9.0×10 -4Pa, the temperature range is 800-900℃, the metal main body cadmium is volatilized, the volatilization time is 6h, the high boiling point difficult to volatilize impurities remain in the crucible, the metal cadmium vapor is condensed and collected to obtain 6N high-purity cadmium.

[0035] Example 2

[0036] A method for preparing 6N high-purity cadmium comprises the following steps:

[0037] The raw material refined cadmium is placed in the crucible of the vacuum distillation equipment at a vacuum degree of 2.0-9.0×10 -3 Pa, the temperature range is 500-700℃, and the volatile smelting is carried out for 6.00h. The low-boiling point volatile impurities in the raw cadmium are volatilized and removed in the form of steam. Then, the raw cadmium removed by the first vacuum volatilization is subjected to the second vacuum volatilization smelting, and the vacuum degree is 1.0-9.0×10 -4 Pa, the temperature range is 800-900℃, the metal main body cadmium is volatilized, the volatilization time is 6h, the high boiling point difficult to volatilize impurities remain in the crucible, the metal cadmium vapor is condensed and collected to obtain 6N high-purity cadmium.

[0038] Example 3

[0039] A method for preparing 6N high-purity cadmium comprises the following steps:

[0040] The raw material industrial grade cadmium is placed in the crucible of the vacuum distillation equipment at a vacuum degree of 2.0-9.0×10 -3 Pa, the temperature range is 500-700℃, and the volatile smelting is carried out for 6.00h. The low-boiling point volatile impurities in the raw cadmium are volatilized and removed in the form of steam. Then, the raw cadmium removed by the first vacuum volatilization is subjected to the second vacuum volatilization smelting, and the vacuum degree is 1.0-9.0×10 -4 Pa, the temperature range is 800-900℃, the metal main body cadmium is volatilized, the volatilization time is 6h, the high boiling point difficult to volatilize impurities remain in the crucible, the metal cadmium vapor is condensed and collected to obtain 6N high-purity cadmium.

[0041] The following Table 1 shows the impurity contents of crude cadmium in Example 1, refined cadmium in Example 2 and industrial-grade cadmium in Example 3 after two vacuum volatilization smeltings, in ppm.

[0042] Table 1

[0043]

[0044]

[0045] It can be seen from the above table that after the first vacuum volatilization smelting, the content of low-boiling-point volatile impurities in the crude cadmium, refined cadmium and industrial-grade cadmium of Example 1, Example 2 or Example 3 is significantly reduced, while the content of high-boiling-point difficult-to-volatile impurities remains basically unchanged or increases slightly. The reason is that the content of metallic cadmium is reduced after the first vacuum volatilization smelting; after the subsequent second vacuum volatilization smelting, the high-boiling-point difficult-to-volatile impurities in the cadmium are significantly reduced, and the impurity content in the high-purity cadmium obtained by the raw material cadmium in Example 1, Example 2 and Example 3 after two vacuum volatilization smelting is significantly lower than the impurity content in the 6N high-purity cadmium specified in the national standard. For the impurity Tl not specified in the national standard, its content in the high-purity cadmium obtained in Example 1, Example 2 and Example 3 is also significantly reduced, indicating that the 6N high-purity cadmium obtained by the preparation method of high-purity cadmium provided by the present invention can meet the market demand.

[0046] The above are only preferred examples of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have many changes. Within the principles of the present invention, all modifications and substitutions made should be included in the protection scope of the present invention.

Claims

1. A method for preparing ultra-high purity cadmium, characterized in that Here are the steps: Step 1: subjecting the raw material cadmium to a first vacuum volatilization smelting at 500 to 700°C to remove low-boiling-point volatile impurities in the raw material cadmium in the form of metal vapor; Step 2: subjecting the raw material cadmium treated in step 1 to a second vacuum volatilization smelting at 800-900° C., so that the main metal cadmium in the raw material cadmium is volatilized to obtain metal cadmium vapor; Step 3: Condensing and collecting the metallic cadmium vapor obtained in step 2 to obtain 6N ultra-high purity cadmium.

2. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The vacuum degree of the vacuum volatilization in step 1 and step 2 is 1.0-9.0×10 -3 -10 -5 Pa.

3. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The vacuum volatilization time in step 1 is 2.00-6.00 hours.

4. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The vacuum volatilization time of step 1 is 6.00-12.00 hours.

5. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The raw material cadmium includes one or more of crude cadmium and refined cadmium.

6. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The heating process of step 1 uses induction heating to gradually increase the temperature: the raw cadmium is placed in a mold and preheated at 200° C.-400° C. for 0.50-1.00 h, and then heated at 500° C.-700° C. for 2.00-6.00 h to perform the first vacuum volatilization melting.

7. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The heating process in step 2 uses induction heating to gradually increase the temperature: the raw cadmium obtained in step 1 is heated at 800° C.-900° C. for 6.00-12.00 hours, and a second vacuum volatilization smelting is performed to obtain metallic cadmium vapor.

8. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The low-boiling-point volatile impurities in step 1 include one or more of zinc, aluminum, magnesium, lead, and thallium.

9. The method for preparing ultra-high purity cadmium according to claim 1, characterized in that: The high boiling point and non-volatile impurities in step 2 include one or more of copper, iron, tin, silicon and sulfur.

10. A method for using the ultra-high purity cadmium prepared by the method according to any one of claims 1 to 9, characterized in that: The ultra-high purity cadmium is used in semiconductors, optoelectronic materials and electronic devices, and energy materials are used in energy storage and nuclear energy high-tech fields.