Variable-temperature hot extrusion magnesium alloy preparation method
By using a multi-stage variable-temperature hot extrusion process, the temperature change of the extrusion die is controlled, which promotes the dynamic recrystallization and precipitation strengthening of magnesium alloys, forming a bimodal grain structure. This solves the problem of insufficient formability of magnesium alloys and significantly improves their mechanical properties.
Patent Information
- Application Number
- CN202411153413.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
Magnesium alloys have a limited number of slip systems at room temperature, which restricts their formability, and existing hot extrusion techniques are insufficient to significantly improve their strength and toughness.
A multi-stage variable-temperature hot extrusion process is adopted. By controlling the temperature of the extrusion die between 275℃, 250℃ and 225℃, dynamic recrystallization and precipitation strengthening of magnesium alloy are promoted, forming a bimodal grain structure.
It significantly improves the tensile strength and yield strength of magnesium alloys, with the ultimate tensile strength approaching 400 MPa, which is far higher than that of conventional preparation processes, and the elongation is also relatively high.
Smart Images

Figure CN119020623A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium alloy preparation, and in particular to a method for preparing a magnesium alloy by variable temperature hot extrusion. Background Art
[0002] Magnesium alloy is a lightweight metal structural material with a density of only 23% of steel and 66% of aluminum. They are increasingly valued in the field of energy conservation and emission reduction, especially in the aerospace and automotive industries. However, due to its hexagonal close-packed crystal structure, magnesium alloys have a small number of slip systems at room temperature and limited formability, which hinders their widespread commercial application. Therefore, improving the formability of magnesium alloys by improving the strength and toughness of the material has always been the eternal focus of magnesium alloy research.
[0003] Hot extrusion technology is an effective deformation process that can simultaneously improve the strength and toughness of magnesium alloys, and has been used to manufacture high-performance magnesium alloy parts. By controlling the extrusion temperature, the critical decomposition shear stress of the magnesium alloy can be effectively reduced, the sliding system of the magnesium alloy can be activated, the formation of a bimodal grain structure can be promoted, and the mechanical properties of the magnesium alloy can be improved, thereby enhancing the formability of the magnesium alloy. Chinese patent CN 108728707 A discloses a method for preparing a high-strength deformed magnesium alloy by rapid extrusion. The alloy product obtained by extrusion in a mold temperature environment of 400°C can achieve a good tensile strength of about 300MPa, but in fact, compared with the current common magnesium alloy mechanical properties, it does not show too obvious advantages. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a magnesium alloy by hot extrusion at a variable temperature, so as to significantly improve the mechanical properties of the magnesium alloy.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for preparing a magnesium alloy by hot extrusion at a variable temperature, comprising the following steps:
[0006] (a) melting a magnesium alloy ingot in an argon atmosphere, homogenizing the magnesium alloy ingot, quenching the magnesium alloy ingot, and cooling the magnesium alloy ingot at room temperature;
[0007] (b) removing the surface layer of the cooled magnesium alloy ingot and processing it into a magnesium alloy workpiece with a cylindrical structure, inserting the magnesium alloy workpiece into a hot extrusion die, and filling metal spherical particles between the magnesium alloy workpiece and the push rod;
[0008] (c) preheating the hot extrusion die to 275°C, then moving the push rod forward and pushing the metal spherical particles to move the magnesium alloy workpiece forward until the magnesium alloy workpiece is completely extruded into the conical cavity, then stopping the extrusion and cooling the hot extrusion die to 250°C, continuing to push the magnesium alloy workpiece so that it is extruded to the end of the conical cavity, then stopping the extrusion and cooling the extrusion die to 225°C, continuing to push the magnesium alloy workpiece so that it is completely extruded from the conical cavity, and stopping the extrusion to obtain the variable temperature hot extruded magnesium alloy.
[0009] Preferably, in step (a), industrial grade pure Mg, Bi, Zn and Mg-20wt%Ca alloy are used to prepare a Mg-2Bi-0.5Zn-0.3Ca alloy ingot in an induction melting furnace under an argon atmosphere, and the alloy ingot is melted for 45 minutes to achieve thermal stability.
[0010] More preferably, in step (a), the homogenization treatment is carried out at 500° C. for 12 hours, followed by rapid quenching in water and cooling at room temperature.
[0011] More preferably, in step (c), the speed of the push rod is 1 mm / s.
[0012] More preferably, the extrusion ratio of the hot extrusion die is 3:1.
[0013] Compared with the prior art, the present invention innovatively prepares magnesium alloys through multi-stage variable temperature hot extrusion, so that the prepared magnesium alloy has significantly higher tensile strength and yield strength. Its ultimate tensile strength can be close to 400MPa, which is much higher than the magnesium alloy products produced by conventional preparation processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic diagram of the structure before hot extrusion in the embodiment;
[0015] Figure 2 is a schematic diagram of the first hot extrusion of a magnesium alloy workpiece in an embodiment;
[0016] Figure 3 is a schematic diagram of a magnesium alloy workpiece being hot extruded for the second time in an embodiment;
[0017] Figure 4 is a schematic diagram of the magnesium alloy workpiece being hot extruded for the third time in the embodiment;
[0018] Figure 5 SEM images of magnesium alloy samples: temperature-variable magnesium alloy (a)-(c), non-temperature-variable magnesium alloy (d) and (f);
[0019] Figure 6EBSD and corresponding grain size distribution histogram of magnesium alloy samples: variable temperature magnesium alloy (a) and (b), non-variable temperature magnesium alloy (c) and (d);
[0020] Figure 7 This is the tensile stress-strain curve of the magnesium alloy sample.
[0021] In the figure:
[0022] 1——Magnesium alloy workpiece 2——Push rod 3——Metal spherical particles
[0023] 4——Hot extrusion die. DETAILED DESCRIPTION
[0024] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments and drawings. The contents mentioned in the implementation modes are not intended to limit the present invention.
[0025] Example
[0026] A method for preparing a magnesium alloy by hot extrusion at a variable temperature, comprising the following steps:
[0027] (a) Mg-2Bi-0.5Zn-0.3Ca alloy ingots were prepared using industrial-grade pure Mg, Bi, Zn and Mg-20wt%Ca alloy in an induction melting furnace under argon atmosphere. The alloy ingots were smelted for 45 minutes to achieve thermal stability, homogenized at 500°C for 12 hours, and then rapidly quenched in water and cooled at room temperature.
[0028] (b) removing the surface layer of the cooled magnesium alloy ingot and processing it into a magnesium alloy workpiece with a diameter of 60 mm × 20 mm, inserting the magnesium alloy workpiece into a hot extrusion die with an extrusion ratio of 3:1, and filling metal spherical particles (such as Figure 1 As shown), the hardness of the metal spherical particles is close to the hardness of the magnesium alloy workpiece.
[0029] (c) The hot extrusion die is preheated to 275°C and kept warm for 1 hour to ensure that the temperature of the outside and inside of the magnesium alloy workpiece is 275°C, and then the push rod is moved forward at a speed of 1 mm / s to push the metal spherical particles to move the magnesium alloy workpiece forward until the magnesium alloy workpiece is completely extruded into the conical cavity (such as Figure 2 Then stop the extrusion and cool the hot extrusion die to 250℃ and keep it warm for 1 hour to ensure that the temperature of the outside and inside of the magnesium alloy workpiece is 250℃. Continue to push the magnesium alloy workpiece at a speed of 1mm / s to extrude it to the end of the conical cavity (as shown in Figure 2). Figure 3As shown in the figure, at this time, part of the metal spherical particles enter the conical cavity and adapt to the shape of the conical cavity to fill it, then stop extrusion and cool the extrusion die to 225℃ for 1 hour to ensure that the temperature of the outside and inside of the magnesium alloy workpiece is 225℃. Continue to push the magnesium alloy workpiece at a speed of 1mm / s to make it completely extruded from the conical cavity (as shown in the figure). Figure 4 As shown), at this time, the conical cavity is completely filled with metal spherical particles, and extrusion is stopped to obtain variable temperature hot extruded magnesium alloy.
[0030] Comparative Example
[0031] The difference between this comparative example and the embodiment is that in step (c), the temperature of the hot extrusion die is kept at 225° C. throughout the process to extrude the magnesium alloy workpiece, thereby obtaining a non-temperature-variable hot extruded magnesium alloy.
[0032] Structural characterization
[0033] The microstructure evolution mechanism of the magnesium alloy samples obtained by extrusion of the embodiment and the comparative example at 20 kV was observed using a Carl Zeiss EVO-18 scanning electron microscope (SEM) equipped with an energy dispersive spectrometer (EDS). Figure 5 Figure 2 is the SEM image of the longitudinal section of the Mg-2Bi-0.5Zn-0.3Ca alloy at different extrusion temperatures. The change of hot extrusion temperature leads to different microstructural characteristics. The variable temperature hot extruded magnesium alloy samples in the embodiment show a clear bimodal grain structure, with obvious non-dynamic crystallization (unDRXed) regions along the extrusion direction and uniformly distributed fine equiaxed dynamically crystallized (DRXed) grains, such as Figure 5 (a)-5(c) However, the non-temperature-varied hot extruded magnesium alloy sample in the comparative example is composed only of coarse DRXed grains without any identifiable bimodal grain structure, such as Figure 5 (d)-5(f) shown.
[0034] The microstructure of the variable temperature hot extruded magnesium alloy of the comparative example and the 225℃ non-variable temperature hot extruded magnesium alloy of the comparative example. The magnesium alloy samples were ground with sandpaper of different grits in sequence, from coarse to fine, until #2000, and etched with ethyl acetate solution. The grain size and grain boundary were characterized by TSL EBSD, and the corresponding data were processed by OIM software to obtain the corresponding EBSD microstructure image and grain size distribution histogram, as shown in Figure 2. Figure 6 As shown. Among them, Figure 6 a and 6b correspond to the EBSD characterization results of the variable temperature hot extruded magnesium alloy in the embodiment. Figure 6c and 6d correspond to the EBSD characterization results of the non-variable temperature hot extruded magnesium alloy in the comparative example. It can be seen that the variable temperature hot extruded magnesium alloy has finer dynamic recrystallized grains than the non-variable temperature hot extruded magnesium alloy. The average grain size of the variable temperature hot extruded magnesium alloy is 1.1μm, while the average grain size of the non-variable temperature hot extruded magnesium alloy is 2.4μm. The average grain size of the variable temperature hot extruded magnesium alloy is significantly smaller than that of the non-variable temperature hot extruded magnesium alloy. At the same time, it can be seen that a large number of non-dynamic crystallization regions are formed in the variable temperature hot extruded magnesium alloy. These non-dynamic crystallization regions and fine dynamic recrystallization grains contribute to a typical bimodal grain structure, while there is no bimodal grain structure in the non-variable temperature hot extruded magnesium alloy. It can be seen that the magnesium alloy has a more complex microstructure after variable temperature hot extrusion.
[0035] Performance Testing
[0036] The mechanical properties of magnesium alloy samples were tested using a CMT-5205 electronic universal testing machine at a constant speed of 1 mm / min at room temperature. The strain measurement of all samples was performed using an installed XTDIC-VG-60 video extensometer with a resolution of 0.1 μm. The values of tensile properties, including yield strength, ultimate tensile strength and elongation, were determined by calculating the average of three repeated tests performed under each experimental condition. The tensile stress-strain curves of variable temperature hot extruded magnesium alloy and non-variable temperature hot extruded magnesium alloy are shown in Figure 2. Figure 7 As shown. The yield strength, ultimate tensile strength and elongation of the variable temperature hot extruded magnesium alloy are 382.5MPa, 392.4MPa and 13.7% respectively, while the yield strength, ultimate tensile strength and elongation of the non-variable temperature hot extruded magnesium alloy are 232.5MPa, 269MPa and 23.6% respectively. By comparison, the yield strength and ultimate tensile strength of the variable temperature hot extruded magnesium alloy are much higher than those of the non-variable temperature hot extruded magnesium alloy, which are 64.5% and 45.9% higher respectively, but the elongation is less than that of the non-variable temperature hot extruded magnesium alloy, which is caused by the mutual restriction of the strength and toughness of the alloy material. At the same time, by comparing the tensile properties of other hot extruded magnesium alloys, it can be seen that the variable temperature hot extruded magnesium alloy prepared in the embodiment has excellent yield strength and ultimate tensile strength, and the elongation is also at a high level, as shown in Table 1. It can be seen that the magnesium alloy prepared by variable temperature hot extrusion has excellent mechanical properties.
[0037] Table 1 Comparison of tensile mechanical properties of magnesium alloys with similar compositions under similar hot extrusion process conditions.
[0038]
[0039] The variable temperature hot extrusion magnesium alloy preparation method provided by the present invention promotes the generation of a large number of bimodal grain structures in the low Ca content Mg-2Bi-0.5Zn-0.3Ca magnesium alloy, obtains excellent yield strength, ultimate tensile strength and good elongation, indicating that the prepared magnesium alloy has excellent mechanical properties and can enhance the formability of the magnesium alloy. This is due to the fact that in the variable temperature hot extrusion process, the microstructure of the magnesium alloy can be affected by controlling the temperature of the extrusion die. In the initial stage, the die is preheated to 275°C, which helps the plastic deformation of the magnesium alloy workpiece and reduces the deformation resistance. As the extrusion proceeds, the die temperature gradually decreases to 250°C, which helps to promote the occurrence of dynamic recrystallization, refine the grains, and thus improve the strength and toughness of the material. When the die temperature is reduced to 225°C, the deformation area of the magnesium alloy material may undergo a more significant dynamic recrystallization process, because the lower die temperature helps to form more nucleation points, thereby promoting the occurrence of recrystallization, which helps to obtain finer grains and improve the strength and toughness of the material.
[0040] Compared with the prior art that directly uses 400℃ high temperature one-time extrusion to prepare magnesium alloy, the present invention innovatively adopts the technical idea of variable temperature hot extrusion. The dynamic recrystallization and precipitation strengthening during the variable temperature hot extrusion process can significantly improve the mechanical properties of the alloy. These strengthening mechanisms help to obtain ultrafine grains and high-density precipitation phases at lower temperatures, so that the present invention can prepare magnesium alloys with better mechanical properties. Moreover, the preparation method is simple and low-cost. It is a convenient method that can effectively improve the mechanical properties of magnesium alloys, which has great significance and value for the research and development of high-performance magnesium alloys.
[0041] In order to make it easier for ordinary technicians in the field to understand the improvements of the present invention over the prior art, some drawings and descriptions of the present invention have been simplified, and the above-mentioned embodiments are preferred implementation schemes of the present invention. In addition, the present invention can also be implemented in other ways. Any obvious replacement without departing from the concept of the present technical solution is within the protection scope of the present invention.
Claims
1. A method for preparing a magnesium alloy by hot extrusion at a variable temperature, characterized in that: The following steps are involved: (a) melting a magnesium alloy ingot in an argon atmosphere, homogenizing the magnesium alloy ingot, quenching the ingot, and cooling the ingot at room temperature; (b) removing the surface layer of the cooled magnesium alloy ingot and processing it into a magnesium alloy workpiece with a cylindrical structure, inserting the magnesium alloy workpiece into a hot extrusion die, and filling metal spherical particles between the magnesium alloy workpiece and the push rod; (c) preheating the hot extrusion die to 275°C, then moving the push rod forward and pushing the metal spherical particles to move the magnesium alloy workpiece forward until the magnesium alloy workpiece is completely extruded into the conical cavity, then stopping the extrusion and cooling the hot extrusion die to 250°C, continuing to push the magnesium alloy workpiece so that it is extruded to the end of the conical cavity, then stopping the extrusion and cooling the extrusion die to 225°C, continuing to push the magnesium alloy workpiece so that it is completely extruded from the conical cavity, and stopping the extrusion to obtain the variable temperature hot extruded magnesium alloy.
2. The method for preparing magnesium alloy by variable temperature hot extrusion according to claim 1, characterized in that: In step (a), industrial-grade pure Mg, Bi, Zn and Mg-20wt%Ca alloy are used to prepare a Mg-2Bi-0.5Zn-0.3Ca alloy ingot in an induction melting furnace under an argon atmosphere. The alloy ingot is melted for 45 minutes to achieve thermal stability.
3. The method for preparing magnesium alloy by variable temperature hot extrusion according to claim 1, characterized in that: In step (a), the homogenization treatment is carried out at 500°C for 12 hours, followed by rapid quenching in water and cooling at room temperature.
4. The method for preparing magnesium alloy by variable temperature hot extrusion according to claim 1, characterized in that: In step (c), the speed of the push rod is 1 mm / s.
5. The method for preparing magnesium alloy by variable temperature hot extrusion according to claim 1, characterized in that: The extrusion ratio of the hot extrusion die is 3:
1.
6. A variable temperature hot extruded magnesium alloy, characterized in that: The magnesium alloy is prepared by the variable temperature hot extrusion magnesium alloy preparation method described in any one of claims 1 to 5.