Magnesium alloy, preparation method thereof, battery and electric device

By adding zinc, rare earth elements, zirconium and calcium oxide to magnesium alloys to control their mass percentage, the problem of insufficient flame retardant performance of magnesium alloys is solved, the ignition point and flame retardant performance are improved, and it is suitable for new energy vehicles in high-temperature environments. Application reduces production costs.

CN119020649AActive Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310594226.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing magnesium alloys have insufficient flame retardant performance, which limits its further development and application in the fields of aviation, aerospace, chemicals, etc.

Method used

By adding zinc (Zn), rare earth elements, zirconium (Zr) and calcium oxide (CaO) to the magnesium alloy, its mass percentage is controlled, the ignition point and flame retardant properties of magnesium alloy are improved, and the ignition point and flame retardant properties of magnesium alloy are processed through reasonable component matching and process , alleviate the thermal cracking and sticking phenomenon during casting and extrusion.

Benefits of technology

It significantly improves the flame retardant performance of magnesium alloy, ensures its stability and safety at high temperatures, is suitable for vehicles such as new energy vehicles and other electrical devices, reduces the impact of impurities on performance, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020649A_ABST
    Figure CN119020649A_ABST
Patent Text Reader

Abstract

The magnesium alloy comprises the following components in percentage by mass: 2%-6.5% of Zn, 0.01%-3% of rare earth elements, 0.01%-1% of Zr, 0.5%-2% of CaO and the balance of Mg and impurities. The invention further provides a preparation method of the magnesium alloy, a battery and an electric device. The magnesium alloy disclosed by the invention has relatively good flame retardant property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a magnesium alloy and a preparation method thereof, a battery and an electrical device. Background Art

[0002] Magnesium alloys have the advantages of low density, high strength, large elastic modulus, good heat dissipation, good shock absorption, and high recycling rate. Magnesium alloys are mainly used in aviation, aerospace, transportation, chemical industry, rocket and other industrial sectors. However, the existing magnesium alloys still have the problem of insufficient flame retardancy, which limits the further development and application of magnesium alloys. Therefore, it is of great significance to provide a magnesium alloy with good flame retardancy. Summary of the invention

[0003] In view of the above problems, the present application provides a magnesium alloy and a preparation method thereof, a battery and an electrical device to solve the above technical problems existing in magnesium alloys.

[0004] In a first aspect, the present application provides a magnesium alloy, comprising:

[0005] Zinc (Zn), the mass percentage of Zn is 2%-6.5%;

[0006] Rare earth elements, the mass percentage of rare earth elements is 0.01%-3%;

[0007] Zirconium (Zr), the mass percentage of Zr is 0.01%-1%;

[0008] Calcium oxide (CaO), wherein the mass percentage of CaO is 0.5%-2%; and

[0009] The rest is Mg and impurities.

[0010] In the technical solution of the embodiment of the present application, Zn, rare earth elements, Zr, CaO and Mg are combined and the percentages of the above components are controlled. CaO can significantly increase the ignition point of the magnesium alloy, and by controlling the mass percentage of CaO to 0.5%-2%, the thermal cracking phenomenon that is prone to occur in the casting process of the magnesium alloy and the mold sticking phenomenon that is prone to occur during extrusion are alleviated, thereby significantly improving the flame retardant properties of the magnesium alloy without affecting the casting performance and extrusion performance of the magnesium alloy.

[0011] In some embodiments, the rare earth element includes at least one of lanthanum (La) and cerium (Ce).

[0012] In the technical solution of the embodiment of the present application, La and Ce are both rare earth metals with relatively low prices. Therefore, on the basis of controlling the mechanical properties of the alloy, the cost of the magnesium alloy is also reduced, which is conducive to industrial production.

[0013] In some embodiments, the mass percentage of Zn is 5%-6.5%; the mass percentage of rare earth elements is 2%-3%; the mass percentage of Zr is 0.5%-1%; the mass percentage of CaO is 1%-2%; and the rest is Mg and impurities.

[0014] In the technical solution of the embodiment of the present application, by controlling the mass percentage of each component, the flame retardant properties of the magnesium alloy are improved without significantly increasing the cost. At the same time, it is not easy to oxidize during the smelting process, which can reduce the use of protective atmosphere and covering agent and improve the quality of magnesium liquid.

[0015] In some embodiments, the average grain size of the magnesium alloy is 6-10 μm.

[0016] In the technical solution of the embodiment of the present application, the grains of the magnesium alloy are fully refined and have a fine and uniform microstructure.

[0017] In some embodiments, the mass percentage of impurities is less than or equal to 0.075%.

[0018] In some embodiments, the impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than or equal to 0.004%, the mass percentage of Cu in the magnesium alloy is less than or equal to 0.02%, the mass percentage of Ni in the magnesium alloy is less than or equal to 0.001%, and the mass percentage of Si in the magnesium alloy is less than or equal to 0.05%.

[0019] In the technical solution of the embodiment of the present application, the content of impurity elements in the magnesium alloy is low, which reduces the impact of impurities on the performance of the magnesium alloy.

[0020] In some embodiments, the magnesium alloy has a flash point greater than or equal to 750°C, optionally, a flash point greater than or equal to 800°C.

[0021] In the technical solution of the embodiment of the present application, the ignition point of the magnesium alloy is above 750° C., which is conducive to safe use in vehicles such as new energy vehicles or other electrical devices.

[0022] In a second aspect, the present application provides a method for preparing the magnesium alloy of any of the above embodiments, comprising:

[0023] Providing pure Mg, pure Zn, Mg-rare earth element master alloy, CaO and Mg-Zr master alloy according to the mass percentage of Mg, Zn, rare earth elements, Zr and CaO in the magnesium alloy;

[0024] Mixing pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy and smelting to obtain magnesium alloy liquid, and smelting is performed in a protective gas;

[0025] The magnesium alloy liquid is poured, extruded and heat treated in sequence.

[0026] In the technical solution of the embodiment of the present application, Zn, rare earth elements, Zr, CaO and Mg are combined and the percentages of the above components are controlled. CaO can significantly increase the ignition point of the magnesium alloy, and by controlling the mass percentage of CaO to 0.5%-2%, the thermal cracking phenomenon that is prone to occur in the casting process of the magnesium alloy and the mold sticking phenomenon that is prone to occur during extrusion are alleviated, thereby significantly improving the ignition point of the magnesium alloy without affecting the casting performance and extrusion performance of the magnesium alloy.

[0027] In some embodiments, the steps of mixing and smelting pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy to obtain a magnesium alloy liquid include: adding pure Mg into a smelting furnace for melting, adding pure Zn after the pure Mg is melted, and performing mechanical stirring while maintaining the temperature of the smelting furnace; controlling the temperature of the smelting furnace to 650-680°C, adding CaO after 10-20 minutes and stirring; heating, and when the temperature of the smelting furnace reaches 680-690°C, adding the Mg-rare earth element master alloy and stirring, and finally adding the Mg-Zr master alloy and stirring to obtain a magnesium alloy liquid.

[0028] In the technical solution of the embodiment of the present application, the temperature of the smelting furnace is controlled to be 650-680° C., which can reduce the oxidation of the magnesium melt and at the same time, make CaO evenly distributed in the melt.

[0029] In the technical solution of the embodiment of the present application, Mg-rare earth element intermediate alloy is added at 680-690°C, so that the burnout of the alloy elements is small and the yield is high. At the same time, the dissolution rate of the alloy elements is fast and they can be completely dissolved.

[0030] In some embodiments, after the step of adding Mg-rare earth element master alloy at 680-690° C. and stirring, the step further includes: maintaining the temperature of the smelting furnace at 680-690° C. and standing for 10-15 minutes to obtain magnesium alloy liquid.

[0031] In the technical solution of the embodiment of the present application, the temperature of the smelting furnace is lowered to a temperature suitable for subsequent pouring operations by standing still for 10-15 minutes.

[0032] In a third aspect, the present application provides a battery, the battery comprising the magnesium alloy as described above or a magnesium alloy prepared by the method for preparing the magnesium alloy as described above.

[0033] In the technical solution of the embodiment of the present application, the battery includes a magnesium alloy, which has an ignition point of above 750°C and has high mechanical properties, and can be safely used in vehicles such as new energy vehicles or other electrical devices.

[0034] In some embodiments, a battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and a magnesium alloy is used for the end plate.

[0035] The magnesium alloy provided in the present application is used as an end plate of a battery, and due to its high ignition point and good mechanical properties, it can increase the stability of the battery.

[0036] In a fourth aspect, the present application provides an electrical device, comprising a battery according to any of the above embodiments.

[0037] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific embodiments of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0039] Figure 1 A schematic diagram of the structure of an electric device in some embodiments of the present application;

[0040] Figure 2 A schematic diagram of the exploded structure of a battery according to some embodiments of the present application;

[0041] Figure 3 This is a schematic diagram of the exploded structure of a battery module according to some embodiments of the present application;

[0042] Figure 4 A schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application;

[0043] Figure 5 This is a flow chart of a method for preparing magnesium alloys according to some embodiments of the present application. DETAILED DESCRIPTION

[0044] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0046] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0047] The “mass percentage” mentioned herein refers to the percentage of the mass of the element to the total mass of the magnesium alloy.

[0048] Existing magnesium alloys have the problem of insufficient flame retardancy, which limits the further development and application of magnesium alloys.

[0049] In order to solve the problem that the existing magnesium alloy has insufficient flame retardant performance, the present invention designs a magnesium alloy, including: zinc (Zn), the mass percentage of Zn is 2%-6.5%; rare earth elements, the mass percentage of the rare earth elements is 0.01%-3%; zirconium (Zr), the mass percentage of Zr is 0.01%-1%; calcium oxide (CaO), the mass percentage of CaO is 0.5%-2%; and the rest is Mg and impurities.

[0050] CaO can significantly increase the ignition point of magnesium alloys, and by controlling the mass percentage of CaO to 0.5%-2%, it can alleviate the thermal cracking phenomenon of magnesium alloys during the casting process and the mold sticking phenomenon during extrusion, thereby significantly improving the flame retardant properties of magnesium alloys without affecting the casting and extrusion properties of magnesium alloys.

[0051] The magnesium alloy disclosed in the embodiments of the present application can be used in, but not limited to, the automotive field, the electronics industry field, the aerospace field, etc. For example, the shell material of the battery pack in new energy vehicles, other shell materials and bracket materials in automobiles, computers, mobile phones, cameras, airplanes, etc. Any product using magnesium alloy can use the magnesium alloy provided in the embodiments of the present application.

[0052] For the convenience of description, the following embodiments are described by taking an electric device 1000 of an embodiment of the present application as a vehicle as an example.

[0053] Please refer to Figure 1, Figure 1 A schematic diagram of the structure of an electric device 1000 provided for some embodiments of the present application. The electric device 1000 may be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is arranged inside the electric device 1000, and the battery 100 may be arranged at the bottom, head or tail of the electric device 1000. The battery 100 may be used to power the electric device 1000. For example, the battery 100 may be used as an operating power source for the electric device 1000. The electric device 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the electric device 1000.

[0054] In some embodiments of the present application, the battery 100 can not only serve as an operating power source for the electrical device 1000, but also serve as a driving power source for the electrical device 1000, replacing or partially replacing fuel or natural gas to provide driving power for the electrical device 1000.

[0055] Please refer to Figure 2 , Figure 2 Schematic diagram of the exploded structure of the battery 100 provided for some embodiments of the present application. The battery 100 includes a box 10 and a battery module 20, and the battery module 20 is accommodated in the box 10. Among them, the box 10 is used to provide a storage space for the battery module 20, and the box 10 can adopt a variety of structures. In some embodiments, the box 10 may include a first part 11 and a second part 12, the first part 11 and the second part 12 cover each other, and the first part 11 and the second part 12 jointly define a storage space for accommodating the battery module 20. The second part 12 can be a hollow structure with one end open, the first part 11 can be a plate-like structure, and the first part 11 covers the open side of the second part 12, so that the first part 11 and the second part 12 jointly define a storage space; the first part 11 and the second part 12 can also be hollow structures with one side open, and the open side of the first part 11 covers the open side of the second part 12. Of course, the box 10 formed by the first part 11 and the second part 12 can be in a variety of shapes, such as a cylinder, a cuboid, etc.

[0056] In the battery 100, there may be multiple battery modules 20, and the multiple battery modules 20 may be connected in series, in parallel, or in mixed connection. Mixed connection means that the multiple battery modules 20 are both connected in series and in parallel. The multiple battery modules 20 may be directly connected in series, in parallel, or in mixed connection, and then the whole formed by the multiple battery modules 20 is accommodated in the box 10; of course, the battery 100 may also be a battery module formed by connecting multiple battery modules 20 in series, in parallel, or in mixed connection, and then the multiple battery modules are connected in series, in parallel, or in mixed connection to form a whole, and then accommodated in the box 10. The battery 100 may also include other structures, for example, the battery 100 may also include a converging component for realizing electrical connection between the multiple battery modules 20.

[0057] In the battery 100 , there may be one or more battery modules 20 , and each battery module 20 may be fixed to the housing 10 by a corresponding fastener (such as a bolt), or each battery module 20 may be fixed to the housing 10 by bonding.

[0058] Figure 3 A schematic diagram of the exploded structure of a battery module 20 provided for some embodiments of the present application. The battery module 20 includes a plurality of stacked battery cells 20a, an end plate 30, and a connector (not shown in the figure). Two end plates 30 are arranged at both ends of the battery module 20 along the stacking direction of the battery cells 20a, and the two end plates 30 are connected by a connector. The end plates 30 and the connector provide a clamping force to the battery cells 20a, and the battery cells 20a are fastened to form a battery module 20 with a certain structural strength. The multiple battery cells 20a in the battery module 20 can be electrically connected through a busbar component (not shown in the figure) to achieve parallel, series or mixed connection of the multiple battery cells 20a in the battery module 20. There may be one or more busbar components, and each busbar component is used to electrically connect at least two battery cells 20a.

[0059] Each battery cell 20a may be a secondary battery, a lithium-sulfur battery, a lithium-ion battery or a lithium metal battery, but is not limited thereto. The battery cell 20 may be cylindrical, flat, rectangular or in other shapes.

[0060] Please refer to Figure 4 , Figure 4 The schematic diagram of the decomposed structure of a battery cell 20a provided in some embodiments of the present application. The battery cell 20a refers to the smallest unit that constitutes a battery. Figure 4 The battery cell 20a includes an end cover 21, a shell 22, a battery cell assembly 23 and other functional components.

[0061] The end cap 21 refers to a component that covers the opening of the shell 22 to isolate the internal environment of the battery cell 20a from the external environment. Without limitation, the shape of the end cap 21 can be adapted to the shape of the shell 22 to match the shell 22. The end cap 21 can be made of a material with a certain hardness and strength (such as aluminum alloy), so that the end cap 21 is not easily deformed when squeezed and collided, so that the battery cell 20a can have a higher structural strength and the safety performance can also be improved. Functional components such as electrode terminals 21a can be provided on the end cap 21. The electrode terminal 21a can be used to electrically connect to the battery cell assembly 23 for outputting or inputting electrical energy of the battery cell 20a. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for releasing the internal pressure when the internal pressure or temperature of the battery cell 20a reaches a threshold. The material of the end cap 21 can also be a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose special restrictions on this. In some embodiments, an insulating member may be provided inside the end cap 21, and the insulating member may be used to isolate the electrical connection components in the housing 22 from the end cap 21 to reduce the risk of short circuit. For example, the insulating member may be plastic, rubber, or the like.

[0062] The shell 22 is a component used to cooperate with the end cover 21 to form the internal environment of the battery cell 20a, wherein the formed internal environment can be used to accommodate the battery cell assembly 23, electrolyte and other components. The shell 22 and the end cover 21 can be independent components, and an opening can be set on the shell 22, and the internal environment of the battery cell 20a is formed by covering the opening with the end cover 21 at the opening. Without limitation, the end cover 21 and the shell 22 can also be integrated. Specifically, the end cover 21 and the shell 22 can form a common connection surface before other components are put into the shell, and when the interior of the shell 22 needs to be encapsulated, the end cover 21 covers the shell 22. The shell 22 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 22 can be determined according to the specific shape and size of the battery cell assembly 23. The material of the shell 22 can be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiment of the present application does not impose any special restrictions on this.

[0063] The battery cell assembly 23 is a component in the battery cell 100 where electrochemical reactions occur. One or more battery cell assemblies 23 may be included in the housing 22. The battery cell assembly 23 is mainly formed by winding or stacking cathode sheets and anode sheets, and a separator is usually provided between the cathode sheets and the anode sheets. The parts of the cathode sheets and the anode sheets with active substances constitute the main body of the battery cell assembly, and the parts of the cathode sheets and the anode sheets without active substances each constitute a tab 23a. The cathode tab and the anode tab may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the cathode active substance and the anode active substance react with the electrolyte, and the tab 23a connects the electrode terminals to form a current loop.

[0064] According to some embodiments of the present application, the present application provides a magnesium alloy, including: zinc (Zn), the mass percentage of Zn is 2%-6.5%; rare earth elements, the mass percentage of rare earth elements is 0.01%-3%; zirconium (Zr), the mass percentage of Zr is 0.01%-1%; calcium oxide (CaO), the mass percentage of CaO is 0.5%-2%; and the rest is Mg and impurities.

[0065] As an example, the mass percentage of Zn can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, etc., or 2%-2.5%, 2.5%-3%, 3%-3.5%, 3.5%-4%, 4%-4.5%, 4.5%-5%, 5%-5.5%, 5.5%-6%, 6%-6.5%, etc. It can be understood that the mass percentage of Zn is not limited to the mass percentages listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of Zn is 2%-6.5%.

[0066] Zinc has solid solution strengthening and aging strengthening effects in magnesium alloys, thereby improving the strength of magnesium alloys; zinc can also weaken the adverse effects of impurities such as iron and nickel in magnesium alloys on the corrosion resistance of magnesium alloys, thereby improving the corrosion resistance of magnesium alloys. If the Zn content is too high, for example, the mass percentage is greater than 6.5%, the mechanical properties of the magnesium alloy will decrease, and it will also cause microporosity and increase the tendency of hot cracking in the magnesium alloy; if the Zn content is too low, for example, the mass percentage is less than 2%, the strength and corrosion resistance of the magnesium alloy will not be significantly improved. The embodiment of the present application improves the strength and corrosion resistance of the magnesium alloy without affecting the mechanical properties of the magnesium alloy by controlling the mass percentage of Zn to 2%-6.5%.

[0067] As an example, the mass percentage of Zr can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 1%, etc., or 0.01%-0.02%, 0.02%-0.03%, 0.03%-0.04%, 0.04%-0.05%, 0.05%-0.06%, 0.06%-0.07%, 0.06%-0.08%, 0.08%-0.09%, 0.09%-1%, etc. It can be understood that the mass percentage of Zr is not limited to the mass percentages listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of Zr is 0.01%-1%.

[0068] Zr has a significant grain refining effect. If the mass percentage of Zr is too large, for example, higher than 1%, it will make the magnesium alloy difficult to process and cast; if the mass percentage of Zr is too small, the effect on grain refining is not obvious. The embodiment of the present application controls the mass percentage of Zr to 0.01%-1%, which has a significant grain refining effect without affecting the processing and casting of the magnesium alloy.

[0069] As an example, the mass percentage of CaO can be 0.5%, 0.65%, 0.7%, 0.85%, 0.9%, 1.0%, 1.15%, 1.2%, 1.35%, 1.4%, 1.55%, 1.6%, 1.75%, 1.8%, 1.95%, 2%, etc., and can also be 0.5%-0.65%, 0.65%-0.7%, 0.7%-0. .85%, 0.85%-0.9%, 0.9%-1.0%, 1.0%-1.15%, 1.15%-1.2%, 1.2%-1.35%, 1.35%-1.4%, 1.4%-1.55%, 1.55%-1.6%, 1.6%-1.75%, 1.75%-1.8%, 1.8%-1.95%, 1.95%-2%, etc. It can be understood that the mass percentage of CaO is not limited to the mass percentages listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of CaO is 0.5%-2%.

[0070] CaO can significantly increase the ignition point of magnesium alloys, and CaO can refine the microstructure of magnesium alloys, and the grain size of the obtained magnesium alloys is smaller. When the mass percentage of CaO is too small, for example, less than 0.5%, the effect of improving the ignition point of magnesium alloys is small, and it cannot meet the use requirements of new energy vehicle batteries, etc.; when the mass percentage of CaO is too large, for example, greater than 2%, the casting performance of magnesium alloys is reduced, and thermal cracking is prone to occur during the casting process. At the same time, the extrusion performance is also reduced, and mold sticking is prone to occur during extrusion. In the technical solution of the embodiment of the present application, by controlling the mass percentage of CaO to 0.5%-2%, the flame retardant properties of magnesium alloys are significantly improved, and the microstructure of magnesium alloys is refined, and a magnesium alloy with a smaller grain size is obtained without affecting the casting performance and extrusion performance of magnesium alloys.

[0071] As an example, the mass percentage of the rare earth element may be 0.01%, 0.05%, 0.08%, 0.1%, 0.15%, 0.17%, 0.2%, 0.25%, 0.26%, 3%, etc., or 0.01%-0.05%, 0.05%-0.08%, 0.08%-0.1%, 0.1%-0.15%, 0.15%-0.17%, 0.17%-0.2%, 0.2%-0.25%, 0.25%-0.26%, 0.26%-3%, etc. It can be understood that the mass percentage of the rare earth element is not limited to the mass percentage listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of the rare earth element is 0.01%-3%.

[0072] Adding rare earth elements to magnesium alloys can refine the structure of magnesium alloys and improve the mechanical properties of magnesium alloys. After the rare earth elements are added, they can purify the melt in the process of preparing magnesium alloys to play a role in degassing and deslagging, thereby improving the quality of the melt. During the smelting process, rare earth elements easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thus improve the corrosion resistance of the magnesium alloy. At the same time, rare earth elements can react with the main impurity elements in magnesium alloys such as Fe, Cu, Ni, and Si to generate high-melting-point binary or multi-component rare earth compounds, reduce the content of impurity elements in the matrix, and further improve the mechanical properties and corrosion resistance of the magnesium alloy.

[0073] When the mass percentage of rare earth elements is too small, for example, less than 0.01%, it cannot achieve the effect of grain refinement, and the mechanical properties of magnesium alloys are slightly improved; when the mass percentage of rare earth elements is too large, for example, greater than 3%, the cost of magnesium alloys will be greatly increased, which is not conducive to industrial production. The embodiment of the present application controls the mass percentage of rare earth elements to 0.01%-3%, thereby significantly improving the mechanical properties of magnesium alloys while controlling the cost of magnesium alloys.

[0074] Rare earth elements can be selected according to actual needs, for example, rare earth elements can be at least one of lanthanum (La) and cerium (Ce) but not limited thereto. In other embodiments, rare earth elements can also include praseodymium (Pr), gadolinium (Gd), neodymium (Nd), yttrium (Y), etc. In some embodiments, the rare earth elements are cheap rare earth elements, and cheap rare earth elements refer to relatively cheap rare earth elements known to those skilled in the art, such as La, Ce, Pr, Y, etc.

[0075] In some optional embodiments, the rare earth element includes at least one of La and Ce.

[0076] Both La and Ce are cheap rare earth metals. Therefore, on the basis of improving the mechanical properties of the alloy, the cost of the magnesium alloy is also reduced, which is conducive to industrial production.

[0077] In some other optional embodiments, the rare earth elements include only Ce.

[0078] CaO and Ce are added to the existing Mg-Zn-Zr magnesium alloy. The magnesium alloy is simple to prepare and has low cost. The obtained magnesium alloy has good flame retardant properties and mechanical properties.

[0079] The magnesium alloy in the embodiment of the present application has a reasonable combination of Mg, Zn, Zr, rare earth elements and CaO, and controls the range of mass percentage, so that the ignition point of the magnesium alloy is above 750°C, and at the same time has high mechanical properties, and can be safely used in vehicles such as new energy vehicles and other electrical devices.

[0080] According to some optional embodiments of the present application, the mass percentage of Zn is 5%-6.5%; the mass percentage of rare earth elements is 2%-3%; the mass percentage of Zr is 0.5%-1%; the mass percentage of CaO is 1%-2%; and the rest is Mg and impurities.

[0081] In the technical solution of the embodiment of the present application, by controlling the mass percentage of each component, the flame retardant properties of the magnesium alloy are improved without significantly increasing the cost. At the same time, it is not easy to oxidize during the smelting process, which can reduce the use of protective atmosphere and covering agent and improve the quality of magnesium liquid.

[0082] According to some optional embodiments of the present application, the average grain size of the magnesium alloy is 6-10 μm.

[0083] As an example, the average grain size of the magnesium alloy can be 6μm, 6.2μm, 6.43μm, 6.5μm, 6.9μm, 7μm, 7.26μm, 7.5μm, 7.85μm, 8μm, 8.3μm, 8.4μm, 8.5μm, 8.85μm, 9μm, 9.2μm, 9.1μm, 9.2μm, 9.5μm, 9.7μm, 9.9μm, 10μm, etc., or it can be 6-8.4μm, 6.43-7μm, 7.26-9.9μm, 7.5-8μm, 8.3-9μm, 7.85-9.5μm, 6.5-10μm, etc. It can be understood that the average grain size of the magnesium alloy is not limited to the values ​​and value ranges listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of CaO is 6-10 μm.

[0084] The grains of the magnesium alloy are fully refined, and the grain size of the magnesium alloy is small. The mechanical properties of the magnesium alloy can be controlled by controlling the grain size. Therefore, the grain size can be controlled according to actual needs, thereby improving the practicability of the magnesium alloy.

[0085] According to some embodiments of the present application, the mass percentage of impurities is less than or equal to 0.075%.

[0086] As an example, the mass percentage of impurities may be less than or equal to 0.075%, 0.07%, 0.065%, 0.06%, 0.05%, 0.0326%, 0.03%, 0.02%, 0.01%, 0.005%, 0.001%, etc. It can be understood that the mass percentage of impurities is not limited to the numerical range listed in the above examples, and can be adjusted according to actual needs, as long as the mass percentage of impurities is less than or equal to 0.075%.

[0087] According to some other embodiments of the present application, the impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than or equal to 0.004%, the mass percentage of Cu in the magnesium alloy is less than or equal to 0.02%, the mass percentage of Ni in the magnesium alloy is less than or equal to 0.001%, and the mass percentage of Si in the magnesium alloy is less than or equal to 0.05%.

[0088] As an example, the mass percentage of Fe in the magnesium alloy may be less than or equal to 0.004%, 0.003%, 0.0025%, 0.002%, 0.001%, 0.0001%, etc.

[0089] As an example, the mass percentage of Cu in the magnesium alloy may be less than or equal to 0.02%, 0.018%, 0.015%, 0.01%, 0.001%, 0.0001%, etc.

[0090] As an example, the mass percentage of Ni in the magnesium alloy may be less than or equal to 0.001%, 0.0008%, 0.0005%, 0.0002%, 0.0001%, 0.00001%, etc.

[0091] As an example, the mass percentage of Si in the magnesium alloy may be less than or equal to 0.05%, 0.04%, 0.03%, 0.025%, 0.02%, 0.01%, 0.001%, 0.0001%, etc.

[0092] Rare earth elements added to magnesium alloys, especially rare earth elements such as La and Ce, can react with the main impurity elements in magnesium alloys such as Fe, Cu, Ni, and Si to generate binary or multi-component rare earth compounds with high melting points, thereby reducing the content of impurity elements in magnesium alloys. Therefore, the content of impurity elements in magnesium alloys is low, and the effect on the performance of magnesium alloys is small.

[0093] According to some embodiments of the present application, the ignition point of the magnesium alloy is greater than or equal to 750°C, and optionally, the ignition point is greater than or equal to 800°C.

[0094] As an example, the ignition point of the magnesium alloy may be greater than or equal to 750° C., 770° C., 780° C., 800° C., 850° C., etc.

[0095] The ignition point of magnesium alloy is above 750°C, so the magnesium alloy provided in the present application can be safely used in vehicles such as new energy vehicles or other electrical devices.

[0096] See also Figure 5 According to some embodiments of the present application, the present application also provides a method for preparing the magnesium alloy in any of the above embodiments, comprising:

[0097] Providing pure Mg, pure Zn, Mg-rare earth element master alloy, CaO and Mg-Zr master alloy according to the mass percentage of Mg, Zn, rare earth elements, Zr and CaO in the magnesium alloy;

[0098] Mixing pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy and smelting to obtain magnesium alloy liquid, and smelting is performed in a protective gas;

[0099] The magnesium alloy liquid is poured, extruded and heat treated in sequence.

[0100] By combining Zn, rare earth elements, Zr, CaO and Mg and controlling the percentages of the above components, CaO can significantly increase the ignition point of the magnesium alloy, and by controlling the mass percentage of CaO to 0.5%-2%, the thermal cracking phenomenon of the magnesium alloy during the casting process and the mold sticking phenomenon during the extrusion can be alleviated, thereby significantly improving the flame retardant properties of the magnesium alloy without affecting the casting performance and extrusion performance of the magnesium alloy.

[0101] The preparation method of the magnesium alloy provided in the embodiment of the present application is simple and low-cost. By adding CaO and controlling the mass percentage of CaO to 0.5%-2%, the ignition point of the magnesium alloy can be significantly improved and the flame retardant performance can be improved; CaO can also refine the microstructure of the magnesium alloy, and the obtained magnesium alloy has a smaller grain size and better mechanical properties.

[0102] Adding rare earth elements to magnesium alloys can refine the structure of magnesium alloys and improve the mechanical properties of magnesium alloys. After the rare earth elements are added, they can purify the melt in the process of preparing magnesium alloys to play a role in degassing and deslagging, thereby improving the quality of the melt. During the smelting process, rare earth elements easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thus improve the corrosion resistance of the magnesium alloy. At the same time, rare earth elements can react with the main impurity elements in magnesium alloys such as Fe, Cu, Ni, and Si to generate high-melting-point binary or multi-component rare earth compounds, reduce the content of impurity elements in the matrix, and further improve the mechanical properties and corrosion resistance of the magnesium alloy.

[0103] According to some embodiments of the present application, the step of mixing pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy and smelting to obtain a magnesium alloy liquid includes: adding pure Mg into a smelting furnace for melting, adding pure Zn after the pure Mg is melted, and performing mechanical stirring while maintaining the temperature of the smelting furnace; controlling the temperature of the smelting furnace to 650-680°C, adding CaO after 10-20 minutes and stirring; heating, and when the temperature of the smelting furnace reaches 680-690°C, adding the Mg-rare earth element master alloy and stirring, and finally adding the Mg-Zr master alloy and stirring to obtain a magnesium alloy liquid.

[0104] The type of the smelting furnace can be selected according to actual needs. In some optional embodiments, the smelting furnace is a protective gas smelting furnace, and a protective gas can be introduced into the smelting furnace.

[0105] The melting point of pure Mg is 649° C. In some optional embodiments, pure Mg is added into a smelting furnace and the temperature is raised to 650-680° C. to completely melt the pure Mg.

[0106] In some optional embodiments, the stirring methods include but are not limited to natural convection stirring, manual stirring, steel flow impact stirring, mechanical stirring, electromagnetic stirring and gas stirring, etc., which can be selected according to actual needs.

[0107] As an example, when CaO is added to the smelting furnace, the temperature in the smelting furnace may be but is not limited to 650°C, 655°C, 660°C, 665°C, 670°C, 675°C, 680°C, etc.; it may also be but is not limited to 650-655°C, 655-660°C, 660-665°C, 665-670°C, 670-675°C, 675-680°C, etc.

[0108] If the CaO addition temperature is too high, for example, above 680°C, the magnesium melt is easily oxidized; if the CaO addition temperature is too low, for example, below 650°C, the fluidity of the magnesium melt is low, which will cause uneven distribution of CaO. In the technical solution of the embodiment of the present application, the temperature of the smelting furnace is controlled to be 650-680°C, which can reduce the oxidation of the magnesium melt and make the CaO evenly distributed in the melt.

[0109] As an example, when Mg-rare earth element master alloy is added to the smelting furnace, the temperature in the smelting furnace may be, but is not limited to, 680°C, 681°C, 682°C, 683°C, 684°C, 685°C, 686°C, 687°C, 688°C, 689°C, 690°C, etc., and may also be, but is not limited to, 680-681°C, 681-682°C, 682-683°C, 683-684°C, 684-685°C, 685-686°C, 686-687°C, 687-688°C, 688-689°C, 689-690°C, etc.

[0110] If the addition temperature of the Mg-rare earth element master alloy is too high, for example, the addition temperature of the Mg-rare earth element master alloy is higher than 690°C, the burnout of the alloy elements will increase and the recovery rate of the alloy elements will decrease; if the addition temperature of the Mg-rare earth element master alloy is too low, for example, lower than 680°C, the dissolution rate of the alloy elements will slow down or even fail to dissolve completely.

[0111] In the embodiment of the present application, Mg-rare earth element master alloy is added at 680-690° C., so that the alloy element burnout is small and the recovery rate is high. At the same time, the alloy element dissolves quickly and can be completely dissolved.

[0112] According to some embodiments of the present application, after the step of adding Mg-rare earth element master alloy at 680-690° C. and stirring, the step further includes: maintaining the temperature of the smelting furnace at 680-690° C. and standing for 10-15 minutes to obtain magnesium alloy liquid.

[0113] As an example, the standing time may be, but not limited to, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, etc., or may be, but not limited to, 10-11 min, 11-12 min, 12-13 min, 13-14 min, 14-15 min, etc. Standing for 10-15 min allows the temperature of the smelting furnace to drop to a temperature suitable for subsequent pouring operations.

[0114] According to some optional embodiments of the present application, the shielding gas may include but is not limited to a mixed gas of sulfur hexafluoride (SF6) and nitrogen (N2), a mixed gas of argon and SF6, a mixed gas of SF6 and carbon dioxide (CO2), etc. The volume ratio of SF6 to N2 in the mixed gas of SF6 and N2, and the volume ratio of SF6 to CO2 in the mixed gas of SF6 and CO2 can be selected according to actual needs.

[0115] According to some optional embodiments of the present application, the protective gas is a mixed gas of sulfur hexafluoride (SF6) and nitrogen (N2).

[0116] By introducing protective gas, the contact time between the magnesium alloy liquid and the atmosphere during the smelting process can be reduced, thereby preventing the magnesium alloy liquid from being oxidized.

[0117] The material of the casting mold in the pouring can be selected according to the material of the casting. According to some embodiments of the present application, the casting mold used in the casting can be but not limited to a metal mold, a metal alloy mold, a ceramic mold, a synthetic material mold, etc. For example, aluminum, H13 steel, ferrosilicon alloy, graphite, alumina ceramics, potassium borate glass fiber, etc. According to some optional embodiments of the present application, the casting mold used in the pouring is a metal film. The size of the casting mold can be selected according to the shape, size, etc. of the casting.

[0118] Metal molds, metal alloy molds, ceramic molds, or synthetic material molds are relatively low in price and have good high temperature resistance, toughness and strength.

[0119] In some optional embodiments, after pouring, the process further comprises subjecting the poured ingot to homogenization treatment at 390-410° C. for 10 h-14 h.

[0120] According to some embodiments of the present application, the billet obtained by casting is peeled after removing the head and tail to obtain an extruded billet, and the extruded billet is placed in an extrusion barrel and extruded to obtain an extruded rod.

[0121] In the embodiment of the present application, the extruded billet obtained by removing the head and tail of the billet obtained by casting and then peeling the billet has better quality and is more conducive to extrusion molding.

[0122] According to some embodiments of the present application, the extrusion parameters may be, but are not limited to: an extrusion ratio of 18-35, an extrusion temperature of 380-420° C., and an extrusion rod speed of 0.5-2 mm / s.

[0123] The extrusion temperature may be, but is not limited to, 380°C, 385°C, 390°C, 395°C, 400°C, 405°C, 410°C, 415°C, 420°C, etc.; it may also be, but is not limited to, 380-385°C, 385-390°C, 390-395°C, 395-400°C, 400-405°C, 405-410°C, 410-415°C, 415-420°C, etc.

[0124] The extrusion rod speed can be but not limited to 0.5mm / s, 0.7mm / s, 0.9mm / s, 1.1mm / s, 1.3mm / s, 1.5mm / s, 1.7mm / s, 1.9mm / s, 2mm / s, etc., and can also be but not limited to 0.5-0.7mm / s, 0.7-0.9mm / s, 0.9-1.1mm / s, 1.1-1.3mm / s, 1.3-1.5mm / s, 1.5-1.7mm / s, 1.7-1.9mm / s, 1.9-2mm / s, etc.

[0125] The extrusion parameters in the embodiments of the present application result in better forming quality of the magnesium alloy.

[0126] According to some embodiments of the present application, the heat treatment may be performed by, but not limited to, an aging treatment, and the aging treatment may be performed at room temperature or at a higher temperature.

[0127] In some optional embodiments, the heat treatment temperature is 150-200° C., and the time is 6-16 hours.

[0128] The temperature of the aging treatment may be, but is not limited to, 150°C, 165°C, 170°C, 175°C, 178°C, 180°C, 185°C, 190°C, 193°C, 195°C, 200°C, etc.; and may be, but is not limited to, 150-170°C, 175-185°C, 190-200°C, etc.

[0129] The time of aging treatment can be but not limited to 6 hours, 7 hours, 7.5 hours, 8 hours, 9 hours, 10 hours, 10.2 hours, 10.5 hours, 11 hours, 12 hours, 13 hours, 13.5 hours, 14 hours, 15 hours, 16 hours, etc., and can also be but not limited to 6-15 hours, 7.5-9 hours, 10.2-11 hours, 10 hours-13 hours, 13.5-16 hours, etc.

[0130] After the above heat treatment, the magnesium alloy has good strength and hardness.

[0131] According to some embodiments of the present application, the present application also provides a battery, the battery comprising the magnesium alloy as described above or a magnesium alloy prepared by the method for preparing the magnesium alloy as described above.

[0132] In the technical solution of the embodiment of the present application, the battery includes a magnesium alloy, which has an ignition point of above 750°C and has high mechanical properties, and can be safely used in vehicles such as new energy vehicles or other electrical devices.

[0133] In some embodiments, a battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and a magnesium alloy is used for the end plate.

[0134] The magnesium alloy provided in the present application can be used for the end plate 30 of the battery 100. The end plate 30 is located at the end of the battery module 20. The end plate 30 can be fixedly connected to the battery module 20. The end plate 30 can be used to fix and squeeze the battery cells 20a after grouping. The end plate 30 can be a plate-shaped structural member located at the end of the battery module 20, or a bracket structural member constituting the frame of the battery module 20.

[0135] The magnesium alloy provided in the present application is used as the end plate 30 of the battery 100. Due to its high ignition point and good mechanical properties, it can increase the stability of the battery.

[0136] According to some embodiments of the present application, the present application further provides an electrical device, comprising a battery provided by any of the embodiments described above, and the battery is used to provide electrical energy to the electrical device.

[0137] The electrical device may be, but is not limited to, any of the aforementioned devices or systems using batteries.

[0138] The preparation process and test data are introduced as follows:

[0139] Embodiment 1:

[0140] The composition of the magnesium alloy provided in Example 1 is: 5.5% by mass of Zn, 0.1% by mass of Zr, 1% by mass of Ce, 1.5% by mass of CaO, impurities Fe<0.004%, Cu<0.02%, Ni<0.001%, Si<0.05%; the rest is magnesium.

[0141] The preparation method of the magnesium alloy in this embodiment includes:

[0142] Providing corresponding pure Mg, pure Zn, Mg-30Ce master alloy, CaO and Mg-20Zr master alloy according to the mass percentages of Mg, Zn, Zr, Ce and CaO in the above magnesium alloy;

[0143] Introduce SF6+N2 mixed gas into the smelting furnace, add the pure Mg into the smelting furnace for melting, add pure Zn after the pure Mg is melted, maintain the temperature of the smelting furnace and perform mechanical stirring at the same time, maintain the temperature of the smelting furnace at 650-680°C, add CaO after 10min-20min and stir; increase the temperature, add the Mg-30Ce master alloy and stir when the temperature of the smelting furnace reaches 680-690°C, finally add the Mg-Zr master alloy and stir, maintain the temperature of the smelting furnace and stand for 10min-15min to obtain the magnesium alloy liquid;

[0144] Use a metal mold for pouring, the size of the metal mold is Φ65*250mm;

[0145] The cast billet was homogenized at 400℃ for 12h, and then the head and tail were removed and peeled to obtain an extrusion billet of Φ50mm*120. The prepared extrusion billet was put into an extrusion barrel and extruded to obtain an extrusion rod of Φ10mm. The extrusion parameters were: extrusion ratio 25, extrusion temperature 400℃, and extrusion rod speed 1mm / s.

[0146] The extruded bars were subjected to aging treatment, and the aging parameters were 175°C and 8 hours.

[0147] Examples 2-11 and Comparative Examples 1-2:

[0148] Examples 2-11 and Comparative Examples 1-2 are substantially the same as Example 1, the only difference being the mass percentage of each element in the composition providing the magnesium alloy.

[0149] The flame retardant properties of the magnesium alloys of Examples 1-11 and Comparative Examples 1-2 were tested respectively:

[0150] The ignition point test of the magnesium alloy was conducted by using the Differential Thermal Analysis (DTA) method, with a heating rate of 30°C / min.

[0151] Table 1 Mass percentage of each element in the magnesium alloy of the embodiment and the comparative example and the performance parameters of the magnesium alloy

[0152] sample Zn Zr CaO Ce La Flash point / ℃ Example 1 5.5% 0.1% 1.5% 1% 0 760 Example 2 3.8% 0.1% 0.5% 3% 0 750 Example 3 2.5% 0.2% 2% 0.01% 0 820 Example 4 4.5% 0.2% 1% 0 2% 755 Example 5 5.2% 0.2% 1.5% 1% 1.5% 780 Example 6 2% 0.01% 0.5% 0.01% 0 770 Example 7 6.5% 1% 2% 1% 2% 800 Example 8 5% 0.5% 1% 1% 1% 805 Example 9 5.5% 0.8% 1.2% 1% 1.5% 810 Example 10 6% 0.8% 1.5% 0 2.5% 820 Embodiment 11 6.5% 1% 2% 1% 2% 840 Comparative Example 1 5.8% 0.2% 0 0 0 505 Comparative Example 2 4.5% 0.2% 0 5% 0 600

[0153] By comparing Examples 1-11 with Comparative Examples 1-2, the present application combines Zn, Zr, CaO, rare earth elements, magnesium, etc., and controls the mass percentage of Zn to 2%-6.5%, the mass percentage of rare earth elements to 0.01%-3%, the mass percentage of Zr to 0.01%-1%, the mass percentage of CaO to 0.5%-2%, and the rest to Mg and impurities, so that the ignition point of the magnesium alloy is above 750°C.

[0154] By comparing Examples 1-7 with Examples 8-11, the present application further controls the mass percentage of Zn to 5%-6.5%, the mass percentage of rare earth elements to 2%-3%, the mass percentage of Zr to 0.5%-1%, the mass percentage of CaO to 1%-2%, and the rest to Mg and impurities, so that the ignition point of the magnesium alloy is further improved.

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A magnesium alloy, characterized in that: include: Zinc (Zn), wherein the mass percentage of Zn is 2%-6.5%; Rare earth elements, wherein the mass percentage of the rare earth elements is 0.01%-3%; Zirconium (Zr), wherein the mass percentage of Zr is 0.01%-1%; Calcium oxide (CaO), wherein the mass percentage of CaO is 0.5%-2%; and The rest is Mg and impurities.

2. The magnesium alloy according to claim 1, characterized in that The rare earth element includes at least one of lanthanum (La) and cerium (Ce).

3. The magnesium alloy according to claim 1 or 2, characterized in that: The mass percentage of Zn is 5%-6.5%; the mass percentage of the rare earth element is 2%-3%; the mass percentage of Zr is 0.5%-1%; the mass percentage of CaO is 1%-2%; and The rest is Mg and impurities.

4. The magnesium alloy according to any one of claims 1 to 3, characterized in that: The average grain size of the magnesium alloy is 6-10 μm.

5. The magnesium alloy according to any one of claims 1 to 4, characterized in that: The mass percentage of the impurities is less than or equal to 0.075%.

6. The magnesium alloy according to any one of claims 1 to 5, characterized in that: The impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than or equal to 0.004%, the mass percentage of Cu in the magnesium alloy is less than or equal to 0.02%, the mass percentage of Ni in the magnesium alloy is less than or equal to 0.001%, and the mass percentage of Si in the magnesium alloy is less than or equal to 0.05%.

7. The magnesium alloy according to any one of claims 1 to 6, characterized in that: The magnesium alloy has a ignition point greater than or equal to 750°C, and optionally, a ignition point greater than or equal to 800°C.

8. A method for preparing a magnesium alloy according to any one of claims 1 to 7, characterized in that: include: Providing pure Mg, pure Zn, Mg-rare earth element master alloy, CaO and Mg-Zr master alloy according to the mass percentages of Mg, Zn, rare earth elements, Zr and CaO in the magnesium alloy; The pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy are mixed and smelted to obtain a magnesium alloy liquid, wherein the smelting is performed in a protective gas; The magnesium alloy liquid is poured, extruded and heat treated in sequence.

9. The method for preparing a magnesium alloy according to claim 8, characterized in that: The step of mixing and smelting the pure Mg, pure Zn, CaO, Mg-rare earth element master alloy, and Mg-Zr master alloy to obtain a magnesium alloy liquid comprises: The pure Mg is added into a smelting furnace for melting, and after the pure Mg is melted, pure Zn is added, and the temperature of the smelting furnace is maintained while mechanical stirring is performed, and the temperature of the smelting furnace is maintained at 650-680° C. After 10-20 minutes, CaO is added and stirred; The temperature is raised, and when the temperature of the smelting furnace reaches 680-690° C., the Mg-rare earth element master alloy is added and stirred, and finally the Mg-Zr master alloy is added and stirred to obtain the magnesium alloy liquid.

10. The method for preparing a magnesium alloy according to claim 9, characterized in that: After the step of adding the Mg-rare earth element master alloy at 680-690° C. and stirring, the method further comprises: maintaining the temperature of the smelting furnace at 680-690° C. and standing for 10 min-15 min to obtain the magnesium alloy liquid.

11. A battery, characterized in that: The invention comprises a magnesium alloy as described in any one of claims 1 to 7 or a magnesium alloy prepared by the method for preparing a magnesium alloy as described in any one of claims 8 to 10.

12. The battery according to claim 11, characterized in that The battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and the magnesium alloy is used for the end plate.

13. An electrical device, characterized in that: Comprising a battery as claimed in claim 11 or 12.

Citation Information

Patent Citations

  • High-plasticity heat-conducting magnesium alloy and preparation method thereof

    CN104046867A

  • Magnesium alloy casting technology

    CN105779797A

  • High-flame-retardant high-yield-ratio wrought magnesium alloy and preparation method thereof

    CN112481532A

  • High Thermal Conductive and Flame Retardant Wrought Magnesium Alloy

    KR101600590B1

  • Mg casting alloy having High thermal conductivity and method of manufacturing the same