Regulation and control method for component distribution of hard alloy column nail

By controlling the component distribution and sintering process of cemented carbide column nails, the precise adjustment of the material properties of cemented carbide column nails is achieved, and the problem of inaccurate material performance regulation in the existing technology is solved, and the comprehensiveness of cemented carbide column nails is improved. Performance and service life.

CN119020654APending Publication Date: 2024-11-26ZIGONG CEMENTED CARBIDE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411084969.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing performance control methods of cemented carbide column nail materials cannot achieve small and clear differences in material properties, resulting in performance fluctuations within an excessively large range and cannot meet the high-precision needs under different working conditions.

Method used

By controlling the component distribution of cemented carbide column nails, including 80-88 wt% tungsten carbide and 12-20 wt% bonding phase, adjusting the sintering temperature and dewaxing insulation time, combined with liquid phase sintering fluidity control, the bonding phase uniformity is achieved Distribution, specific components such as 84.8 wt% tungsten carbide powder, 13 wt% cobalt powder, 2 wt% nickel powder, sintering temperature is 1390-1450°C, dewaxing insulation time is 60-500 minutes, and sintering pressure is 0-10MPa.

Benefits of technology

It realizes accurate adjustment of the material properties of cemented carbide column nails, reduces the fluctuation range of material properties, improves the comprehensive service performance and service life of cemented carbide column nails, and reduces the use of additives, avoiding the complexity of alloy components. change.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020654A_ABST
    Figure CN119020654A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hard alloy, and discloses a method for regulating and controlling component distribution of a hard alloy column nail, the components of the hard alloy column nail comprise 80-88 wt% of tungsten carbide and 12-20 wt% of a bonding phase, and the carbon content of the hard alloy column nail is 6.08-6.20%; when the hard alloy column nail is prepared, the sintering temperature is controlled to be 1390-1450 DEG C, the dewaxing heat preservation time is 60-500 min, and the sintering pressure is 0-10 MPa. According to the method for regulating and controlling the component distribution of the hard alloy column nail, the distribution condition of the bonding phase in the hard alloy column nail is regulated and controlled by regulating and controlling the component difference of the bonding phase, the sintering process and the like, so that the hard alloy column nail has better comprehensive use performance on the whole, the cost can be effectively controlled, and the service life of the hard alloy column nail is prolonged. And the use content of the additive is reduced, complexity of alloy components is avoided, and component distribution is effectively regulated and controlled on the premise that the components are not changed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide, and in particular to a method for regulating and controlling the distribution of cemented carbide column components. Background Art

[0002] Tungsten Carbide Dowel Pin is a fixed connection element made of cemented carbide in engineering and mechanical applications. It is mostly used in rolling crushing in the fields of mining, cement, chemical industry, etc. In actual use, Tungsten Carbide Dowel Pin is mainly installed on the roller surface of the roller press to crush the material, which can effectively promote the formation of the material layer and control the loss of the roller surface base material.

[0003] The application conditions of roller presses are complex and varied. Different application scenarios have strict requirements on the hardness, bending strength and other properties of cemented carbide studs, but the differences are small, which leads to further improvement and development of cemented carbide studs. At present, the cemented carbide studs are mainly improved by adding grain growth inhibitors or controlling the particle size of raw materials to meet different performance requirements.

[0004] However, when the above two methods are used for improvement and adjustment, it is very easy for the number of alloy grain boundaries to change too much, and grain boundaries are one of the key factors affecting material properties. Too many grain boundaries will increase the brittleness of the material, while reducing toughness and wear resistance. In short, according to different working conditions, the material properties of cemented carbide studs need to be regulated within a small range, but the existing regulation methods all have the problem of inaccurate regulation, resulting in the material properties of cemented carbide studs fluctuating within a too large range.

[0005] Based on the current situation of regulating the performance of cemented carbide stud materials, there is an urgent need for a regulation method that can more accurately regulate the performance of cemented carbide stud materials. Summary of the invention

[0006] The technical problems to be solved by the present invention are:

[0007] Since the performance requirements of cemented carbide studs are closely related to the working conditions, the material performance requirements of cemented carbide studs are extremely high and the differences are small for different working conditions. Therefore, when producing different cemented carbide studs for different working conditions, it is necessary to control the material performance of different cemented carbide studs to have small and clear differences. However, the existing cemented carbide stud material performance control method has the problem of low adjustment accuracy, that is, it is impossible to effectively achieve the effect of small and clear differences in the performance of cemented carbide studs.

[0008] The technical solution adopted by the present invention is:

[0009] The invention provides a method for regulating the distribution of components of a cemented carbide column nail. The components of the cemented carbide column nail include 80-88wt% of tungsten carbide and 12-20wt% of a bonding phase, and the carbon content of the cemented carbide column nail is 6.08-6.20%. When preparing the cemented carbide column nail, the sintering temperature is controlled to be 1390-1450°C, the dewaxing and heat preservation time is 60-500min, and the sintering pressure is 0-10MPa.

[0010] Preferably, the bonding phase comprises one or more of cobalt powder, nickel powder and iron powder.

[0011] Preferably, the bonding phase comprises 10.4-17.3 wt % cobalt powder and 1.6-2.7 wt % nickel powder.

[0012] Preferably, the difference in bonding phase content at both ends of the cemented carbide stud is 0.1-1.2%.

[0013] Preferably, in the cemented carbide stud, the solid solubility of tungsten in the bonding phase is 1-10%.

[0014] Preferably, the cemented carbide stud comprises 84.8wt% tungsten carbide powder, 13wt% cobalt powder, 2wt% nickel powder and 0.2wt% chromium carbide powder, and the carbon content of the cemented carbide stud is 6.13%.

[0015] The beneficial effects of the present invention are as follows:

[0016] The present invention has found that liquid phase sintering will occur in the bonding phase during the sintering process. Due to the effects of the tray loading process, boat coating, gravity, etc., there are obvious differences in the distribution of the bonding phase in the vertical direction. Such non-uniform component distribution will cause the material properties of different parts of the cemented carbide studs to be also quite different, thus affecting their normal operation and use. In this regard, the present invention effectively adjusts the fluidity of the liquid phase sintering of the bonding phase by regulating the differences in bonding phase components, carbon content, and sintering process, thereby regulating the distribution of the bonding phase in the cemented carbide studs, so that the cemented carbide studs have better overall comprehensive performance, so as to promote the efficiency of the stud roller material crushing and extend the service life of the studs. The cemented carbide stud component distribution control method proposed by the present invention can not only effectively control costs, but also reduce the use content of additives, avoid the complication of alloy components, and achieve effective and precise control of component distribution under the premise of unchanged components. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is an electron microscope image (1000 times) of the top cross section of the cemented carbide stud in Example 1;

[0018] Figure 2This is an electron microscope image (1000 times) of the bottom cross section of the cemented carbide stud in Example 1;

[0019] Figure 3 This is an electron microscope image (1000 times) of the top cross section of the cemented carbide stud in Example 2;

[0020] Figure 4 This is an electron microscope image (1000 times) of the bottom cross section of the cemented carbide stud in Example 2. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0022] The present invention provides a method for regulating the distribution of cemented carbide stud components, wherein the cemented carbide stud components include 80-88wt% tungsten carbide and 12-20wt% bonding phase, and the carbon content of the cemented carbide stud is 6.08-6.20%;

[0023] Preferably, the powder is 84.8wt% tungsten carbide powder, 0.2wt% chromium carbide powder, 13wt% cobalt powder and 2wt% nickel powder, and the carbon content of the cemented carbide stud is 6.13%;

[0024] When preparing the hard alloy column nail, the sintering temperature is controlled to be 1390-1450° C., the dewaxing and heat preservation time is 60-500 minutes, and the sintering pressure is 0-10 MPa.

[0025] In the present invention, the bonding phase includes one or more of cobalt powder, nickel powder and iron powder; preferably 10.4-17.3wt% of cobalt powder and 1.6-2.7wt% of nickel powder.

[0026] In the present invention, in the cemented carbide stud, the solid solubility of tungsten in the bonding phase is 1-10%, and the difference in bonding phase content between the top and both ends of the cemented carbide stud is 0.1-1.2%.

[0027] By adopting the method for controlling the distribution of cemented carbide column components of the present invention, the cemented carbide powder can control the difference in the content of the top and bottom bonding phases of 30-40 mm cemented carbide column to fluctuate between 0.1% and 1.5% by controlling the sintering process and the carbon content, etc., combined with the control of the fluidity of liquid phase sintering, so that the hardness difference at the ends of the cemented carbide column can be controlled within 2HRA, and the solid solubility of tungsten in the bonding phase can be controlled within 1%-10%, thereby achieving a degree of accuracy that cannot be achieved by traditional control methods, and making the material properties of the cemented carbide column controllable and adjustable within a small range.

[0028] <Example>

[0029] Example 1

[0030] The following cemented carbide raw material powders were weighed in weight percentage: 84.8wt% WC20, 0.2wt% chromium carbide powder, 13wt% cobalt powder, and 2wt% nickel powder; and the total carbon content in the cemented carbide raw material powder was 6.13wt%.

[0031] First, the cobalt powder and nickel powder are placed in a desktop double-motion mixer and mixed for 1 hour to obtain a bonding phase, and then the WC20, chromium carbide powder and bonding phase are added to a ball mill;

[0032] Take 2wt% paraffin and 0.04wt% stearic acid (the content here refers to the weight percentage of the material in the cemented carbide raw material powder), add them to a ball mill, use WC-6wt%Co cemented carbide balls with a diameter of φ6.35mm as grinding bodies, the ball-to-material ratio is 4:1, add 360mL / kg ethane as grinding media, and perform ball milling. The ball mill uses a 1L cantilever ball mill, the ball milling speed is controlled to 72r / min, and the ball milling time is 30h;

[0033] After the ball milling is completed, the slurry is sieved and then vacuum dried at 75°C to obtain a dry powder. The dry powder is granulated and molded at a pressure of 7MPa. The pressed green body is vacuum sintered at 1390°C for 90 minutes. After sintering, positive pressure cooling is performed with the pressure maintained at 0.9MPa. The green body is taken out of the furnace after the temperature in the furnace is lower than 50°C to obtain a cemented carbide stud.

[0034] Example 2

[0035] The difference between this embodiment and embodiment 1 is that the sintering temperature is 1430° C., the pressure during sintering is 0.9 MPa, and the holding time is 150 min.

[0036] Example 3

[0037] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 82.8wt% WC20, 0.2wt% chromium carbide powder, 15.6wt% cobalt powder, and 2.4wt% nickel powder; and the total carbon content in the cemented carbide raw material powder is 6.11wt%.

[0038] Example 4

[0039] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 80.8wt% WC20, 0.2wt% chromium carbide powder, 16.5wt% cobalt powder, and 2.5wt% nickel powder; and the total carbon content in the cemented carbide raw material powder is 6.09wt%.

[0040] Example 5

[0041] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 86.8wt% WC20, 0.2wt% chromium carbide powder, 11.3wt% cobalt powder, and 1.7wt% nickel powder; and the total carbon content in the cemented carbide raw material powder is 6.17wt%.

[0042] Example 6

[0043] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 82.8wt% WC20, 0.2wt% chromium carbide powder, 12.9wt% cobalt powder, and 2.1wt% nickel powder.

[0044] Example 7

[0045] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 82.8wt% WC20, 0.2wt% chromium carbide powder, 13.35wt% cobalt powder, and 1.65wt% nickel powder.

[0046] Example 8

[0047] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 82.8wt% WC20, 0.2wt% chromium carbide powder, 12.3wt% cobalt powder, and 2.7wt% nickel powder.

[0048] Example 9

[0049] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 86.8wt% WC20, 0.2wt% chromium carbide powder, 10.4wt% cobalt powder, and 2.6wt% nickel powder.

[0050] Example 10

[0051] The difference between this embodiment and embodiment 1 is that the cemented carbide raw material powder includes 80.8wt% WC20, 0.2wt% chromium carbide powder, 17.2wt% cobalt powder, and 1.8wt% nickel powder.

[0052] <Comparative Example>

[0053] Comparative Example 1

[0054] The difference between this comparative example and Example 1 is that the sintering temperature is 1465° C., the sintering pressure is 12 MPa, and the holding time is 270 min.

[0055] Comparative Example 2

[0056] The difference between this comparative example and Example 1 is that the sintering temperature is 1380° C. and the holding time is 50 min.

[0057] Comparative Example 3

[0058] The difference between this comparative example and Example 1 is that the cemented carbide raw material powder includes 77.8wt% WC20, 0.2wt% chromium carbide powder, 19.0wt% cobalt powder, and 3.0wt% nickel powder; and the total carbon content in the cemented carbide raw material powder is 6.0wt%.

[0059] Comparative Example 4

[0060] The difference between this comparative example and Example 1 is that the cemented carbide raw material powder includes 89.8wt% WC20, 0.2wt% chromium carbide powder, 8.5wt% cobalt powder, and 1.5wt% nickel powder; and the total carbon content in the cemented carbide raw material powder is 6.23wt%.

[0061] <Test example>

[0062] Samples: Examples 1-10, Comparative Examples 1-4

[0063] The cemented carbide studs prepared in Examples 1-10 and Comparative Examples 1-4 were respectively taken, and the bonding phase distribution at the top and bottom thereof was observed and detected. Figures 1 to 4 Shown are electron microscope images of the top and bottom of the cemented carbide stud in Example 1 and electron microscope images of the top and bottom of the cemented carbide stud in Example 2, respectively.

[0064] Furthermore, the composition analysis of the bottom of the cemented carbide studs of Example 1 and Example 2 was performed, and the results are shown in Table 1 below:

[0065] Table 1 Composition analysis results of the bottom of cemented carbide studs of different samples

[0066]

[0067] Through the above electron microscope images and composition analysis results, it can be seen that a cobalt layer appears on the bottom surface of the cemented carbide column nail, indicating that the present invention can effectively adjust the fluidity of the bonding phase during liquid phase sintering, thereby regulating the distribution of the bonding phase in the cemented carbide column nail, so that the cemented carbide column nail has better comprehensive performance as a whole.

[0068] The alloy grain size, strength of different parts and bonding phase content distribution of the samples were then measured, and the results are summarized in Table 2:

[0069] Table 2 Material properties of different samples

[0070]

[0071]

[0072] Through the performance test of the cemented carbide studs prepared in the above-mentioned embodiments 1-10 and comparative examples 1-4, it can be found that the cemented carbide studs prepared according to the control method of embodiments 1-10 have a more uniform and controllable bonding phase distribution, and the control accuracy is high, and can be controlled within a small difference range. Therefore, it can be explained that the cemented carbide stud component distribution control method proposed in the present invention can achieve a degree of accuracy that cannot be achieved by traditional control methods, so that the material properties of the cemented carbide studs can be controlled and adjusted within a small range, so that the cemented carbide studs have better comprehensive performance as a whole, and the composition of the alloy is not changed or increased.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for regulating the distribution of cemented carbide stud components, characterized in that: The cemented carbide stud comprises 80-88 wt% tungsten carbide and 12-20 wt% bonding phase, and the carbon content of the cemented carbide stud is 6.08-6.20%; When preparing the hard alloy column nail, the sintering temperature is controlled to be 1390-1450° C., the dewaxing and heat preservation time is 60-500 minutes, and the sintering pressure is 0-10 MPa.

2. The method for controlling the composition distribution of cemented carbide studs according to claim 1, characterized in that: The bonding phase includes one or more of cobalt powder, nickel powder and iron powder.

3. The method for controlling the composition distribution of cemented carbide studs according to claim 2, characterized in that: The bonding phase includes 10.4-17.3 wt % of cobalt powder and 1.6-2.7 wt % of nickel powder.

4. The method for controlling the composition distribution of cemented carbide studs according to any one of claims 1 to 3, characterized in that: The difference in the content of the bonding phase at both ends of the hard alloy column nail is 0.1-1.2%.

5. The method for controlling the composition distribution of cemented carbide studs according to any one of claims 1 to 3, characterized in that: In the cemented carbide stud, the solid solubility of tungsten in the bonding phase is 1-10%.

6. The method for controlling the composition distribution of cemented carbide studs according to claim 1, characterized in that: The cemented carbide column nail comprises 84.8wt% tungsten carbide powder, 13wt% cobalt powder, 2wt% nickel powder and 0.2wt% chromium carbide powder, and the carbon content of the cemented carbide column nail is 6.13%.