Cold-formed high-strength steel for automobile and preparation method of cold-formed high-strength steel

By adding specific chemical components to automotive steel and using smelting, hot rolling, pickling, cold rolling and hood annealing processes, cold-formed high-strength steel with high strength and elongation are prepared, and the existing medium and high-strength steel plates are solved. The problems of difficulty in cold forming and complex thermal forming have achieved efficient forming and cost reduction of automotive steel, supporting the development of lightweight automobiles.

CN119020693AInactive Publication Date: 2024-11-26HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226604.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively cold-form the automotive steel plate with a high strength of more than 1200MPa, and the thermoforming process is complex and the cost is high, and the mold design and manufacturing are complex, which affects production efficiency and cost.

Method used

Chemical components are C: 0.07-0.18%, Si: 0.22-0.80%, Mn: 1.8-2.6%, P≤0.02%, S≤0.01%, Al: 0.01-0.06%, Ti: 0.01-0.06%, Cr : 0.6~1.0%, B: 0.002~0.005%, V: 0.05~0.12% of cold-formed high-strength steel for automobiles, prepared by smelting, hot rolling, pickling, cold rolling and hood annealing processes, and the steel plate is heated to Aoste After body building, it cools naturally in the air, and the microstructure is converted into martensite to achieve hardening.

Benefits of technology

Cold-formed high-strength steel for automobiles with high strength and elongation has the capability of precision forming, simplifying stamping equipment, reducing mold damage, improving the tensile strength and elongation of parts, reducing production costs, and complying with automotive lightweight Quantitative demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020693A_ABST
    Figure CN119020693A_ABST
Patent Text Reader

Abstract

The invention discloses cold-formed high-strength steel for an automobile and a preparation method thereof, and belongs to the technical field of automobile material preparation. The cold-rolled steel comprises the following chemical components in percentage by mass: 0.07 to 0.18 percent of C, 0.22 to 0.80 percent of Si, 1.8 to 2.6 percent of Mn, less than or equal to 0.02 percent of P, less than or equal to 0.01 percent of S, 0.01 to 0.06 percent of Al, 0.01 to 0.06 percent of Ti, 0.6 to 1.0 percent of Cr, 0.002 to 0.005 percent of B, 0.05 to 0.12 percent of V and the balance of Fe and inevitable impurity elements. The preparation method comprises the procedures of smelting, hot rolling, acid pickling, cold rolling and cover annealing. The cover annealing process is adopted, the obtained cold-formed high-strength steel structure has dispersively distributed nanoscale carbides, the ferrite grain size is small and uniform, the plasticity is good, the performance is excellent, the strength is high after heat treatment, the production process is simple, and the cold-formed high-strength steel structure has remarkable significance for achieving light weight of automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile material preparation, and relates to a cold-formed high-strength steel for automobiles and a preparation method thereof. Background Art

[0002] Lightweighting of automobiles is one of the important directions for the future development of the automobile industry. Lightweighting plays a vital role in reducing automobile fuel consumption and reducing emission pollution. Experiments have shown that if the weight of the entire vehicle is reduced by 10%, the fuel efficiency can be improved by 6% to 8%; for every 100 kg reduction in the curb weight of the vehicle, the fuel consumption per 100 kilometers can be reduced by 0.3 to 0.6 liters, and carbon dioxide emissions can be reduced by about 5g / kilometer. The use of high-strength steel is an effective way to achieve lightweighting of automobiles. On the premise of ensuring the safety performance of the vehicle, the thickness of the components can be effectively reduced to achieve weight reduction of the vehicle body. Compared with traditional 340MPa materials, the theoretical weight reduction potential of 600MPa-grade steel is about 20%, and the weight reduction potential of 800MPa materials will increase to more than 30%.

[0003] The steel plate undergoes plastic deformation under the action of the stamping die through the stamping mechanical equipment to obtain the required shape and size. At present, there are two main technical routes for stamping high-strength automotive steel, cold forming and hot forming. The cold forming process has many advantages, cold stamping parts have stable quality, high dimensional accuracy, simple operation and high productivity. However, with the increase in the strength of automotive steel plates, it is inevitable that it will be difficult to form, mainly manifested in forming cracks, severe springback and die wear. At present, automotive steel plates with a strength of more than 1200MPa are almost impossible to cold form. Hot forming is to heat a steel plate with a strength of 500-600MPa to above the austenite temperature range, then stamp the steel plate into the required shape, and then quench it in the die at a cooling rate of 20-30℃. After quenching, the part strength can reach 1500MPa. However, compared with cold forming, hot stamping presses need to be customized, taking into account the rapid mold closing capability of mechanical presses and the pressure holding capability of hydraulic presses. In addition, the mold design and manufacturing are relatively complex, and the mold cost is high. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a cold-formed high-strength steel for automobiles and a preparation method thereof. The obtained high-strength steel has extremely strong hardenability. After being heated to complete austenitization, it is naturally cooled in the air, and the microstructure can be completely transformed into a martensitic structure to achieve hardening, with a tensile strength of ≥1000MPa and an elongation A80 of ≥7%.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions: A cold-formed high-strength steel for automobiles, whose chemical composition and mass percentage are C: 0.07-0.18%, Si: 0.22-0.80%, Mn: 1.8-2.6%, P≤0.02%, S≤0.01%, Al: 0.01-0.06%, Ti: 0.01-0.06%, Cr: 0.6-1.0%, B: 0.002-0.005%, V: 0.05-0.12%, and the balance is Fe and unavoidable impurity elements.

[0006] Furthermore, the mass percentage of Ti and V in the cold-formed high-strength steel satisfies: Ti+V≤0.15%.

[0007] Furthermore, the thickness of the cold-formed high-strength steel is 1.0-2.5 mm; the microstructure is a ferrite structure, and fine and dispersed carbide precipitation is distributed in the crystal.

[0008] Furthermore, the cold-formed high-strength steel has a yield strength of 280-400 MPa, a tensile strength of 440-550 MPa, an elongation after fracture A80≥25%, a work hardening index n≥0.14, no cracking after 180° bending 0T, and an average limiting hole expansion rate λ≥50%.

[0009] Furthermore, after the cold-formed high-strength steel is heated to be completely austenitized and then naturally cooled in the air, the microstructure is completely transformed into a martensitic structure, the tensile strength is ≥1000MPa, and the elongation A80 is ≥7%.

[0010] The present invention also provides a method for preparing the above-mentioned cold-formed high-strength steel for automobiles, which comprises the steps of smelting, hot rolling, pickling, cold rolling, and hood annealing; In the hood annealing process, the cold hardened coil obtained by cold rolling is placed in a hood furnace for heating. During the heating process, the heating speed is not controlled before 400°C, the heating time at 400-750°C is not less than 12h, the holding temperature is 670-750°C, the holding time is 8-18h, and then slowly cooled to room temperature to obtain cold-formed high-strength steel.

[0011] Furthermore, in the hot rolling process, the heating temperature is 1200-1250°C, the start rolling temperature is 1050-1120°C, the final rolling temperature is 750-880°C, the coiling temperature is 620-710°C, and the hot-rolled steel coil structure is lamellar ferrite and bainite structure.

[0012] Furthermore, in the cold rolling process, the reduction rate is 60 to 70%.

[0013] Furthermore, in the hood annealing process, the temperature difference between the hot spot and the cold spot of the steel coil is ≤60°C, and the hood cooling time is not less than 8 hours.

[0014] The composition design principle of the present invention is as follows: The carbon element is the most important element that determines the mechanical properties of steel. The carbon element mainly exists in the form of carbides in steel, which can significantly improve the strength and hardness of steel. Carbon can also improve the hardenability of steel, but too much C will reduce the plasticity and welding properties of steel. In order to ensure good plasticity and weldability, the present invention requires that the C content be controlled at 0.07-0.18%.

[0015] The Si element has a strong solid solution strengthening effect in steel, which can improve the hardness and strength of ferrite and inhibit the precipitation of carbides. Too high Si content will reduce the plasticity of the steel and deteriorate the corrosion resistance and weldability of the steel. Therefore, the present invention requires that the Si content be controlled at 0.22-0.80%.

[0016] The Mn element can improve the hardness, strength and wear resistance of steel. However, excess manganese will significantly increase the supercooling ability of austenite, increase the formation of cold cracks, and deteriorate the welding performance of steel. Therefore, the Mn content of the present invention is controlled to 1.8-2.6%.

[0017] The Al element has a strong solid solution strengthening effect, can refine the grains, and significantly improve the oxidation resistance of the steel. However, too much Al will affect the welding performance and cutting performance of the steel. Therefore, the Al content of the present invention is controlled at 0.01-0.06%.

[0018] Cr can improve the hardenability of steel, improve the oxidation resistance of steel, form a passivation film on the surface of steel, and significantly improve the corrosion resistance of steel. However, too much Cr will hinder bainite transformation, so the Cr content of the present invention is controlled at 0.6-1.0%.

[0019] Ti element in steel easily forms carbide TiC with carbon, has strong solid solution strengthening effect, and can also refine grains. However, Ti is expensive, and adding too much will lead to increased costs. Therefore, the Ti content of the present invention is controlled at 0.01-0.06%.

[0020] The B element can significantly improve the hardenability of austenite. Generally, the effect of alloying elements in improving hardenability increases with the increase of their content in steel, but boron has an optimal content range. Too much or too little is not conducive to improving hardenability. Therefore, the B content of the present invention is controlled at 0.002-0.005%.

[0021] The V element exists in the steel mainly in the form of carbides, which can refine the steel structure, improve the strength and toughness of the steel, and also improve the heat treatment performance and corrosion resistance of the steel. However, when there is too much vanadium, the unevenness and brittleness of the steel will increase, so the V content of the present invention is controlled at 0.05-0.12%.

[0022] The inventive principle of the technical solution of the present invention is as follows: In order to overcome the antagonistic relationship between strength and elongation, the present invention performs heat treatment after the steel plate is cold-formed into the final part shape and size. The annealed steel plate itself has low strength and good plasticity, and can achieve the deformation of complex parts. After forming, the parts are austenitized in a heating furnace and then taken out and cooled in the air to complete the hardening of the parts, and the strength is improved without the need for a cooling system, thereby achieving the steel plate with both complex deformation ability and hardening ability. The cold-formed high-strength steel obtained by the present invention has better forming performance than DP, DH, and CP steels of the same strength level after hardening.

[0023] In order to simplify the stamping equipment, the present invention adds a large amount of elements that improve hardenability, so that the hardenability of the high-strength steel is extremely strong. After complete austenitization, the structure can be transformed into martensite by natural cooling in the air. Therefore, a relatively slow cooling rate should be maintained in the annealing process to prevent the formation of martensite. The slowest cooling rate of the continuous annealing production line is still too fast for this high-strength steel. Therefore, the technical solution of the present invention uses hood annealing, which is continuously kept warm at 650℃~750℃ for 8~18h. Keeping warm at this temperature is conducive to the precipitation of nano-scale carbides, and the grain size is small and uniform. If the temperature is too low and the time is too short, the recrystallization of the steel plate structure is incomplete, and the banded structure is residual, and the performance is uneven. If the temperature is too high and the time is too long, the grains are too coarse, which seriously affects the strength of the steel plate, and at the same time, the carbides will aggregate and grow, which is not conducive to the improvement of the mechanical properties of the material.

[0024] The beneficial effects of adopting the above technical solution are: (1) The cold-formed high-strength steel for automobiles provided by the present invention has precision forming capability. By adding appropriate amounts of alloy elements and strictly controlling the temperature during rolling to ensure that the hot rolling final rolling temperature and the coiling temperature are within the range of the hole and, by adopting a hood annealing process, the production is flexible, the steel coil has uniform performance, the steel plate structure has dispersedly distributed nano-scale carbides, the ferrite grain size is small and uniform, the steel plate has good plasticity, and the work hardening index is high, thereby achieving excellent forming capability, and can be used to prepare complex deformed parts.

[0025] (2) The high-strength steel described in the present invention has simple equipment in the production process of parts. The parts are stamped and formed by cold forming process. Compared with hot forming, ordinary presses can be used for stamping. The mold does not need a circulating water system, and cold stamping causes less damage to the mold, and the part size accuracy is high.

[0026] (3) After the high-strength steel of the present invention is cold-formed to obtain the shape of the part, it is subjected to complete austenitization heat treatment in a heating furnace and then taken out and cooled in air to achieve through hardening, which greatly improves the strength of the part. Due to cooling in air, the internal stress of the part is small and zero deformation can be achieved. The strength and size of the part are further guaranteed.

[0027] (4) The cold-formed high-strength steel for automobiles described in the present invention has a yield strength of 280-400MPa, a tensile strength of 440-550MPa, an elongation after fracture A80 ≥ 25%, a work hardening index n ≥ 0.14, 180° bending 0T without cracking, and an average ultimate hole expansion rate λ ≥ 50%. After heat treatment, the tensile strength is ≥ 1000MPa, and the elongation A80 is ≥ 7%. The high-strength steel of the present invention has strong plasticity, excellent deep drawing performance, high strength after heat treatment, simple production equipment and process, and is in line with the development direction of automobile steel. It is of great significance to achieve lightweight automobiles. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the metallographic structure diagram of the steel coil after hot rolling in Example 1 of the present invention; Figure 2 This is a metallographic structure diagram of a steel plate after bell annealing in Example 1 of the present invention; Figure 3 This is a SEM microstructure image of the steel plate after bell annealing in Example 1 of the present invention; Figure 4 This is a metallographic structure diagram of the cold-formed high-strength steel after austenitization and air cooling according to Example 1 of the present invention; Figure 5 This is the SEM microstructure diagram of Example 1 of the present invention after cold forming, high-strength austenitization and air cooling. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with the embodiments and drawings.

[0030] Examples 1 to 9 A method for preparing cold-formed high-strength steel for automobiles, comprising smelting, hot rolling, pickling, cold rolling, and hood annealing processes; (1) Smelting: The slab is cast after smelting according to the set chemical composition range. The chemical composition by mass percentage is: C: 0.07-0.18%, Si: 0.22-0.80%, Mn: 1.8-2.6%, P≤0.02%, S≤0.01%, Al: 0.01-0.06%, Ti: 0.01-0.06%, Cr: 0.6-1.0%, B: 0.002-0.005%, V: 0.05-0.12%, and the balance is Fe and unavoidable impurity elements.

[0031] (2) Hot rolling: The slab is heated and kept at 1200-1250°C for 160-200 min, followed by dephosphorization and rolling at a temperature of 1050-1120°C. After multiple passes of rolling, the final rolling temperature is controlled at 750-880°C, air-cooled to 620-710°C for coiling, and cooled to room temperature to obtain a hot-rolled coil. The hot-rolled coil has a lamellar ferrite and bainite structure.

[0032] (3) Pickling: The hot-rolled steel coil is pickled, rinsed and dried to obtain the pickled plate.

[0033] (4) Cold rolling: The pickled steel plate is cold rolled with a reduction rate of 60-70% to obtain a cold-hardened coil with a thickness of 1.0-2.5 mm.

[0034] (5) Hood annealing: The cold hardened coil is placed in a hood furnace for annealing. During the heating process, the heating speed is not controlled before 400°C. The heating time at 400-750°C is not less than 12 hours. The holding temperature is 670-750°C, the holding time is 8-18 hours, the temperature difference between the hot spot and the cold spot of the steel coil is ≤60°C, and the cooling time with a hood is not less than 8 hours. During the heating and cooling process of the steel coil in the hood annealing furnace, the temperature of different parts of the steel coil is different. The highest and lowest temperature points of the steel coil are usually called the hot spot and the cold spot.

[0035] Comparative Examples 1 to 3 (1) Smelting: Smelting is performed according to the set chemical composition range and then cast into slabs.

[0036] (2) Hot rolling: The slab is heated and kept at 1200-1250°C for 160-200 min, followed by dephosphorization and rolling at a temperature of 1050-1120°C. After multiple passes of rolling, the final rolling temperature is controlled at 750-880°C, air-cooled to a coiling temperature of 620-710°C, and then cooled to room temperature to obtain a hot-rolled coil.

[0037] (3) Pickling: The hot-rolled steel coil is pickled, rinsed and dried to obtain the pickled plate.

[0038] (4) Cold rolling: The pickled steel plate is cold rolled with a reduction rate of 60-70% to obtain a cold-hardened coil with a thickness of 1.0-2.5 mm.

[0039] (5) Hood annealing: The cold hard coil is placed in a hood furnace for annealing. The heating speed is not controlled before 400°C. The heating time at 400-750°C is not less than 12h. For comparative example 1, the insulation temperature is controlled at 650-670°C and the insulation time is 13h; for comparative example 2, the insulation temperature is controlled at 670-750°C and the insulation time is 6h; for comparative example 3, the insulation temperature is controlled at 670-750°C and the insulation time is 20h.

[0040] The compositions of the cold-formed high-strength steels of Examples 1-9 and Comparative Examples 1-3 are shown in Table 1, and the production process parameter controls are shown in Tables 2 and 3.

[0041] The high-strength steel obtained in Examples 1-9 and Comparative Examples 1-3 was kept in a 930° C. heating furnace for 6 minutes, taken out after being completely austenitized, and placed in the air for cooling. The mechanical properties of the steel plates were measured. The mechanical properties are shown in Table 4.

[0042] Table 1. Chemical composition of cold-formed high-strength steel of various embodiments and comparative examples (wt%)

[0043] Table 2 Hot rolling and cold rolling process parameters of various embodiments and comparative examples

[0044] Table 3. Hood annealing process parameters for each embodiment and comparative example

[0045] Table 4 Mechanical properties of high-strength steel in various embodiments and comparative examples

[0046] In Comparative Example 1, the hood annealing holding temperature is lower than the lower limit of the control temperature, which is 660°C, and the holding time is 13h. Within the range, the tensile strength after annealing is 593MPa, the yield strength is 507MPa, and the elongation is only 15.2%.

[0047] In Comparative Example 2, the hood annealing temperature was controlled within the range of 730°C, and the insulation time was lower than the lower limit of the controlled insulation time, only 6 hours. After annealing, the tensile strength was 552 MPa, the yield strength was 470 MPa, and the elongation was only 22.0%.

[0048] In comparative example 3, the hood annealing temperature was controlled within the range of 720°C, the insulation time was as long as 24h, the tensile strength after annealing was 463MPa, the yield strength was only 220MPa, and the elongation was 19.0%.

[0049] The high-strength steel in Examples 1-9 of the present invention strictly controls the holding temperature and holding time of the hood annealing process, so that the steel plate structure is fine and uniform ferrite, the precipitated carbides are nano-scale and dispersed inside the ferrite, so that the steel plate has good formability.

Claims

1. A cold-formed high-strength steel for automobiles, characterized in that: Its chemical composition and mass percentage are C: 0.07~0.18%, Si: 0.22~0.80%, Mn: 1.8~2.6%, P≤0.02%, S≤0.01%, Al: 0.01~0.06%, Ti: 0.01~0.06%, Cr: 0.6~1.0%, B: 0.002~0.005%, V: 0.05~0.12%, and the balance is Fe and unavoidable impurity elements.

2. The cold-formed high-strength steel for automobiles according to claim 1, characterized in that: The mass percentage of Ti and V meets the requirement of Ti+V≤0.15%.

3. The cold-formed high-strength steel for automobiles according to claim 2, characterized in that: The thickness of the cold-formed high-strength steel is 1.0-2.5 mm; the microstructure is a ferrite structure, and fine dispersed carbide precipitation is distributed in the crystal.

4. The cold-formed high-strength steel for automobiles according to claim 3, characterized in that: The cold-formed high-strength steel has a yield strength of 280-400 MPa, a tensile strength of 440-550 MPa, an elongation after fracture A80≥25%, a work hardening index n≥0.14, no cracking after 180° bending 0T, and an average limiting hole expansion rate λ≥50%.

5. The cold-formed high-strength steel for automobiles according to claim 4, characterized in that: After the cold-formed high-strength steel is heated to be completely austenitized and then naturally cooled in the air, the microstructure is completely transformed into a martensite structure, the tensile strength is ≥1000MPa, and the elongation A80 is ≥7%.

6. The method for preparing cold-formed high-strength steel for automobiles according to any one of claims 1 to 5, characterized in that: It includes smelting, hot rolling, pickling, cold rolling and hood annealing processes; In the hood annealing process, the cold hardened coil obtained by cold rolling is placed in a hood furnace for heating. During the heating process, the heating speed is not controlled before 400°C, the heating time at 400-750°C is not less than 12h, the holding temperature is 670-750°C, the holding time is 8-18h, and then slowly cooled to room temperature to obtain cold-formed high-strength steel.

7. The method for preparing cold-formed high-strength steel for automobiles according to claim 6, characterized in that: In the hot rolling process, the heating temperature is 1200-1250°C, the starting rolling temperature is 1050-1120°C, and the final rolling temperature is 750-880°C.

8. The method for preparing cold-formed high-strength steel for automobiles according to claim 7, characterized in that: In the hot rolling process, the coiling temperature is 620-710°C, and the hot rolled steel coil structure is lamellar ferrite and bainite structure.

9. The method for preparing cold-formed high-strength steel for automobiles according to claim 8, characterized in that: In the cold rolling process, the reduction rate is 60-70%.

10. The method for preparing cold-formed high-strength steel for automobiles according to any one of claims 1 to 9, characterized in that: In the hood annealing process, the temperature difference between the hot spot and the cold spot of the steel coil is ≤60℃, and the cooling time with hood is not less than 8h.