Gradient structure Tip / VW94 composite material containing ultra-fine grains and preparation method of gradient structure Tip / VW94 composite material
By adding Ti particles to the Tip/VW94 composite material and performing sliding friction treatment, an ultrafine crystal gradient structure was prepared, which solved the problem of insufficient material strength and plasticity, achieved strength improvement and plasticity maintenance, and was simple in process and low in cost. .
Patent Information
- Application Number
- CN202411144367.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The strength and plastic properties of the existing Tip/VW94 composite materials fail to meet the requirements for structural materials application, and the existing gradient structure preparation methods have problems such as large investment in equipment, high pollution, and poor surface quality.
By adding Ti particles to the cast alloy, homogenized heat treatment and hot extrusion, combined with sliding friction treatment, a gradient structure Tip/VW94 composite material containing ultrafine crystals was prepared.
It significantly improves the strength of the composite material, while maintaining good plastic properties, simple process and low cost, and has good application prospects.
Smart Images

Figure CN119020709A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a gradient structure Tip / VW94 composite material containing ultrafine grains and a preparation method thereof. Background Art
[0002] At present, magnesium-based composite materials have received more attention due to their excellent performance, and they also have better application prospects in the aerospace, automotive and electronics industries. Composite materials can generally be classified according to the different reinforcements, and they can be divided into fiber reinforcement, whisker reinforcement and particle reinforcement. Among them, particle reinforced composite materials have simpler preparation processes and lower costs, and are more promising at present.
[0003] Pu et al. used Ti particles to reinforce high-strength rare earth magnesium alloy and prepared Tip / Mg-8.7Gd-4Y-1Zn-1Mn (VW94) composite materials by semi-solid stirring assisted ultrasonic vibration. The mechanical properties of the composite material were improved to varying degrees on the basis of the alloy, with yield strength and tensile strength of 162MPa and 240MPa respectively, and elongation increased to 7.7%. Tip / VW94 composite materials have successfully further improved their mechanical properties, however, their performance still does not meet the requirements for application as structural materials. How to continue to improve its strength and maintain plasticity on this basis is a problem worthy of attention.
[0004] Generally speaking, the methods to improve material strength include homogenization heat treatment, adding rare earth elements, building gradient structures, adding reinforcing particles, etc. It is worth noting that the introduction of gradient structures in these methods can usually maintain a balance between strength and plasticity, which is critical for the practical application of materials.
[0005] Introducing gradient structures into metals can improve various properties of materials. There are many methods for preparing gradient structures, which can be divided into three types according to their preparation principles: chemical / physical coating or deposition method, plastic deformation method and hybrid surface nano-processing. Among them, chemical / physical coating or deposition technology requires large equipment investment, high pollution during the production process, and the combination between the coating and the substrate of the gradient layer is often not stable enough to meet the actual production application; while in the plastic deformation method, the material treated with surface nano-processing generally undergoes severe plastic deformation to form a gradient structure with the average grain size gradually decreasing from the surface to the core. The most widely used hybrid surface nano-processing technologies today are surface mechanical attrition treatment (SMAT), ultrasonic rolling extrusion (USRP) and ultrasonic shot peening (USSP). However, the surface quality of the material treated by SMAT is too rough, which affects the practical application; USRP technology also has defects. Since the static pressure is applied to the tool head and the vibration frequency is low, the nanolayer formed is very thin and the strengthening effect is not good enough; the operation of ultrasonic shot peening technology (USSP) is based on the use of high-power ultrasound to vibrate the steel ball. Since it is ultrasonic, the frequency of the entire device is very high, which enables the material surface to obtain very high-frequency impact shot peening treatment in a short period of time, thereby obtaining a surface nanolayer; however, because its principle is dynamic impact, the surface of the material after treatment is not smooth enough and has a high roughness, which leads to a decrease in the material's fatigue resistance; and the hybrid preparation method involves the transformation of the structural layer, and cannot guarantee that the nano-ization effect is stable enough, so the material performance cannot be guaranteed. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the main purpose of the present invention is to provide a gradient structure Tip VW94 composite material containing ultrafine grains and a preparation method thereof, aiming to solve the problem of strength and plasticity inversion of existing Tip / VW94 composite materials.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a gradient structure Tip / VW94 composite material containing ultrafine grains, comprising the following steps: 1) adding Ti particles to a cast alloy and dispersing them uniformly to prepare a Tip / VW94 magnesium-based composite material;
[0009] 2) performing homogenization heat treatment and hot extrusion on the Tip / VW94 magnesium-based composite material obtained in step 1) to obtain a composite plate;
[0010] 3) The composite plate material in step 2) is subjected to sliding friction treatment to obtain a gradient structure Tip / VW94 composite material containing ultrafine grains.
[0011] In some specific embodiments, the cast alloy is prepared by the following method: heating and melting the VW94 prefabricated alloy under an inert atmosphere, and after the VW94 prefabricated alloy is completely melted, cooling to a semi-solid temperature, and adding the preheated aluminum foil wrapped with Ti particles into the melt and starting mechanical stirring; after the mechanical stirring is completed, heating the melt, and when the temperature rises to 700°C, ultrasonic dispersion is performed, and then rapid water cooling is performed to obtain a Tip / VW94 magnesium-based composite material.
[0012] Furthermore, the specific method of the dispersion is: the dispersion is uniformly dispersed by combining mechanical stirring and ultrasonic dispersion, wherein the speed of mechanical stirring is 250-350r / min for the first 3-5 minutes, and the speed is 550-750r / min for the next 1-3 minutes; the power of ultrasonic dispersion is 1-3kw, and the ultrasonic dispersion is 5-15min.
[0013] In step 1), the mass fraction of the Ti particles in the cast alloy is 1-5%, and the particle size of the Ti particles is 5-10 μm.
[0014] In some specific embodiments, the process parameters of the homogenization heat treatment in step 2) are: firstly treat at a temperature of 510-550° C. for 4-6 hours, then cool to 450-550° C. with the furnace and continue homogenization for 2-4 hours.
[0015] In some specific embodiments, the process parameters of the hot extrusion in step 2) are: extrusion temperature is 400-600°C, and extrusion ratio is (15-25):1.
[0016] In some specific embodiments, the sliding friction treatment in step 3) is specifically: load 300-500N, sliding speed 0.2m / s, and sliding friction parameters repeated 30 times.
[0017] In some specific embodiments, the cast alloy is VW94 cast magnesium alloy.
[0018] The object of the present invention is to provide a gradient structure Tip / VW94 composite material containing ultrafine grains.
[0019] In some specific embodiments, a gradient deformation layer with a thickness of 300-500 μm is constructed on the surface of the ultrafine-grained gradient-structured Tip / VW94 composite material, and the grain size in the deformation layer in the high-strain region is refined to 80-95 nm.
[0020] Compared with the prior art, the present invention has at least the following advantages:
[0021] 1) The gradient structure Tip / VW94 composite material containing ultrafine grains provided by the present invention selects Ti particles as the reinforcement of the high-strength rare earth magnesium alloy composite material, and evenly disperses the Ti particles in the VW94 magnesium alloy, so that the composite material not only has the good comprehensive mechanical properties of the rare earth elements, but also has better strength and toughness due to the reinforced particles; and then the Ti particle reinforced composite material is subjected to sliding friction treatment to construct a gradient structure, thereby significantly improving the strength of the gradient structure TipVW94 composite material while slightly reducing the plasticity of the composite material, and it is expected to achieve the improvement of the mechanical properties of magnesium alloys and magnesium-based composite materials.
[0022] 2) The method for preparing the gradient structure Tip / VW94 composite material containing ultrafine grains provided by the present invention uses readily available raw materials, has a simple process, low cost, strong reproducibility, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0024] Figure 1 The IPF diagram (a) and grain size statistics diagram (b) of the VW94 prefabricated alloy in Example 1 of the present invention; and the histogram of the proportion of small-angle grain boundaries (c);
[0025] Figure 2 The structure scan of the VW94 alloy material subjected to SFT in Comparative Example 1 of the present invention is performed, wherein the plan view before SFT (a); the plan view after SFT deformation (b); the cross-sectional view before SFT (c); the cross-sectional view after SFT deformation (d);
[0026] Figure 3 (a) IPF diagram of the plate in Example 1; (b) grain size statistical histogram; (c) small angle grain boundary proportion histogram;
[0027] Figure 4 The metallographic cross-section comparison diagram of the composite materials in the embodiment of the present invention and the comparative example, wherein (a) the original 3.5wt.% Ti / VW94 composite material; (b) the 3.5wt.% Ti / VW94 composite material after SFT deformation;
[0028] Figure 5The tensile properties of the gradient structure Tip / VW94 composite material prepared in Example 1 and the VW94 prefabricated alloy (Comparative Example 1) in step 1) are compared in a bar chart: (a) VW94 alloy material; (b) 3.5wt.% Ti / VW94 composite material;
[0029] Figure 6 The high strain TEM morphology image (a), selected area electron diffraction pattern image (b), average grain size distribution histogram (c), and stacking fault diagram (d) of the gradient structure Tip / VW94 composite material in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0031] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0032] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0033] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0034] The test methods used in the following embodiments include:
[0035] The mechanical strength and plasticity of the composite material are reflected by testing the main properties of each test sample respectively; the main properties tested in this application include microstructure, mechanical properties, etc.
[0036] 1. Microstructure characterization equipment
[0037] 1) X-ray diffractometer
[0038] X-ray diffraction (XRD) can be used to analyze the phase structure. Before testing, the sample surface needs to be gently polished with 200#, 400#, 800#, and 1200# sandpaper. It should be noted that the sample with a nanolayer on the surface after SFT only needs to grind off the surface oxide layer. This experiment uses Empyrean multifunctional high-resolution X-ray diffractometer, the target material is Cu target, and the maximum output power is 4kW. In this experiment, XRD was used to detect the phase of alloys and composite materials before and after sliding friction treatment, and the phase was determined by combining MDI Jade6 software, and the data was imported into the X-ray spectrum drawn by OriginPro2016; the detection parameters are: scanning speed 1° / min, scanning range 0~90°.
[0039] 2) Metallographic microscope
[0040] Optical microscopy (OM) uses the principle of geometric optical imaging to analyze the microstructure of metal materials. Since the microstructure of VW94 alloy and 3.5wt.% Ti / VW94 composite material will change significantly after the surface is treated by sliding friction, and a gradient structure layer with a gradient change in grain size will be produced, it is necessary to use a metallographic microscope to observe the microstructure of the material before and after SFT. This experiment uses an ICX41M-T / R metallographic microscope, and the samples observed are all longitudinal sections before and after SFT; the sample preparation method is as follows: 3×5×7mm samples are cut by wire cutting, and then 200#, 400#, 800#, 1200#, 2000# sandpaper are used to grind the sample under flowing water, and finally nitric acid alcohol and picric acid solution are used for corrosion, and ethanol is used for rinsing; the corrosion time is controlled at 15~30s according to different materials.
[0041] 3) Scanning electron microscopy
[0042] Scanning electron microscope (SEM) is a new type of electron optical instrument with high image resolution and large depth of field. SEM can be used to conduct preliminary analysis of the morphology and composition of samples. It is generally divided into secondary electron scanning and backscattering scanning. This experiment uses JEOL JSM-7800 field emission scanning electron microscope with an operating voltage of 20kV to compare and observe the differences in morphology and second phase distribution before and after SFT. Electron backscatter diffraction (EBSD) is a crystal orientation analysis method using the backscattered electron diffraction cell in the SEM electron microscope. This experiment uses EBSD to shoot the real grain size and texture strength of the material before and after SFT, and analyzes the results in combination with Channel5. software.
[0043] In particular, the secondary electron scanning samples in this experiment are all planes and longitudinal sections of the materials before and after SFT, while the samples used for EBSD shooting are planes at different gradient positions before and after SFT. Before using secondary electron scanning and backscattering scanning, the materials need to be ground with 200#, 400#, 800#, 1200#, and 2000 sandpaper. The ground secondary electron scanning samples need to be corroded with 1ml of nitric acid alcohol for 15 to 30s depending on the sample, and backscattering scanning also requires electrolytic polishing of the sample. The polishing method is as follows: First, use AC-II as the polishing liquid, use liquid nitrogen to cool the surface of the material, the electrolytic voltage is 20V, add enough liquid nitrogen to the polishing liquid, control the current and polish the sample when the temperature is low enough, and the time is controlled at about one minute depending on the sample.
[0044] 4) Transmission electron microscopy
[0045] Compared with OM and SEM, transmission electron microscope (TEM) can see more tiny microstructures, especially for the morphology of nanoparticles and the measurement of particle size. Therefore, in this experiment, TEM can help observe the image of the microstructure in the deformed layer after deformation treatment. This experiment uses FEITechnai F20 transmission electron microscope. The TEM absorption contrast image can be used for morphological observation; the material phase can be determined by diffraction techniques such as electron diffraction; and due to the high resolution of TEM, the defects in the crystal can be observed, the defect type can be determined, and the defect density can be estimated; high-angle annular dark field image-scanning transmission electron microscopy technology is used to characterize the dispersion at the atomic level. The samples in this experiment were prepared by mechanical polishing and ion beam thinning at room temperature using a Gatan precision ion polishing system. The samples after SFT treatment were prepared as cross-sectional gradient samples, and the samples after aging treatment were prepared as the treated plane.
[0046] 2. Mechanical properties testing equipment
[0047] 1) Microhardness tester
[0048] The micro Vickers hardness tester can measure the Vickers hardness of the sample based on the indentation by pressing the surface of the material. It has better accuracy than other hardness testers. This experiment needs to measure the changes in hardness of the sample at different depths before and after SFT deformation, so the HVS-1000Z digital micro hardness tester is used. The force applied to measure the hardness in this experiment is 100gf, and the holding time is 10s. Since there is a hardness gradient in the sample in this experiment, it is necessary to accurately measure the hardness multiple times at different depths and take the average value. The hardness measurement surface of all samples used is the longitudinal section.
[0049] 2) Tensile testing machine
[0050] The tensile testing machine can measure the strength, elongation and other properties of the material by applying a tensile load to the material. Generally, there are room temperature stretching and high temperature stretching. This experiment uses room temperature stretching. The tensile testing machine used is the CMT-5105 universal tensile testing machine, and the stretching speed is 1.5mm / min. In order to better compare, the tensile samples before and after SFT need to be of the same size, and they need to be polished with 1000#, 1500#, and 3000# sandpaper before stretching. The size of the tensile sample is: gauge length 10mm, middle diameter 4mm, and end diameter 10mm.
[0051] In addition, it is important to note that since the material samples after SFT deformation in this experiment are double-sided treated samples, the preparation of the tensile sample also needs to ensure that both sides have complete gradient deformation layers. Therefore, the thickness of the tensile sample after SFT treatment depends on the actual situation.
[0052] Example 1
[0053] This embodiment provides a method for preparing a gradient structure Tip VW94 composite material containing ultrafine grains, comprising the following steps:
[0054] 1) Preparation of 3.5wt.% Tip / VW94 composite material
[0055] 11) First, the VW94 prefabricated alloy is polished to make the surface of the VW94 prefabricated alloy smooth and oxidized, then an appropriate amount of VW94 prefabricated alloy raw material is weighed and put into a cleaned stainless steel crucible, and the crucible is placed in a resistance furnace at 740° C. and heated for 1 hour until it melts. During the heating process, the air is isolated to ensure the purity of the melt, and CO2-SF6 inert gas protection is introduced throughout the process, with a ratio of 99:1; at the same time, the required mass of Ti particles is weighed and wrapped with Al foil, and the air on the surface of the particles is isolated, and the particles are placed in a drying oven at 200° C. for preheating for 35 minutes to obtain aluminum foil wrapped with Ti particles;
[0056] 12) After the VW94 prefabricated alloy is completely melted at 720°C, a colander is used to remove slag and the temperature is lowered to the semi-solid temperature of 620°C. The preheated aluminum foil wrapped with Ti particles is quickly thrown into the melt. The speed is controlled within 300r / min in the first 4min and adjusted to 650r / min in the last 2min. The whole process is under a protective gas environment and the Ti particles are instantly immersed in the melt.
[0057] 13) After mechanical stirring, the melt is heated. When the temperature reaches 700°C, it is lightly stirred with a mechanical stirrer and taken out. A colander is used to remove slag. An ultrasonic probe is placed in a crucible and immersed 3-4 cm below the liquid surface. The melt is heated together with the furnace temperature. The ultrasonic device is turned on. The smelting furnace is heated and the temperature is controlled at 700°C. The ultrasonic parameters are set to a power of about 2 kW. The ultrasonic dispersion is maintained for 10 minutes, and the ultrasonic probe is then taken out. After the ultrasonic dispersion treatment is completed, the melt is lightly stirred at the lowest speed with a mechanical stirrer, and then quickly placed in cold water for cooling to obtain a cast Ti particle reinforced VW94 composite material, and the middle 1 / 3 of the melt is taken to obtain a Tip / VW94 composite material.
[0058] 14) The Tip / vw94 composite material of step 13) was homogenized at 520° C. for 5 hours, cooled to 500° C. in the furnace and then homogenized for 3 hours, taken out and quickly water-cooled to obtain a homogenized composite material;
[0059] 15) extruding the homogenized composite material into a 4 mm thick plate at 450° C. with an extrusion ratio of 23:1;
[0060] 2) Preparation method of gradient structure Tip / VW94 composite material containing ultrafine grains
[0061] 21) The plate prepared in step 1) is placed on a sliding friction treatment device at room temperature for sliding friction treatment. The sliding friction treatment method is: a friction pair with a load of 300N is placed on the plate, the sliding speed is set to 0.2m / s, and the sliding friction parameters are repeated 30 times on the surface of the plate to be treated; during the experiment, the two ends of the plate need to be clamped, and the ground debris is removed in time to ensure the flatness of the treated surface. At the same time, in order to prevent bending due to high-speed sliding, 1.5mm is required at both ends of the plate, and two treatment areas are selected for the same treatment surface; the width of a treatment area is 15mm and the length is 130mm, and then the same area is rubbed again after 1mm. After treating one surface, the plate is turned over and the sliding friction treatment with the same parameters is performed at the same position to obtain a gradient structure Tip / VW94 composite material containing ultrafine grains on both sides.
[0062] Comparative Example 1
[0063] This comparative example provides a method for preparing a VW94 composite material, wherein the components and proportions thereof are substantially the same as those of Example 2; the steps and process parameters thereof are substantially the same as those of Example 1, except that Ti particle reinforcement is not performed, but the VW94 alloy is directly subjected to sliding friction treatment, specifically comprising the following steps:
[0064] 1) Surface treatment of VW94 prefabricated alloy
[0065] 11) grinding the VW94 prefabricated alloy to make the surface of the VW94 prefabricated alloy smooth and oxidized;
[0066] 12) extruding the pretreated VW94 prefabricated alloy into a 4 mm thick plate at 450°C with an extrusion ratio of 23:1;
[0067] 2) Preparation method of VW94 composite material
[0068] 21) The plate prepared in step 1) is placed on a sliding friction treatment device at room temperature for sliding friction treatment. The sliding friction treatment method is: a friction pair with a load of 500N is placed on the plate, the sliding speed is set to 0.2m / s, and the sliding friction parameters are repeated 30 times on the surface of the plate to be treated; during the experiment, the two ends of the plate need to be clamped, and the ground debris is removed in time to ensure the flatness of the treated surface. At the same time, in order to prevent bending due to high-speed sliding, 1.5mm needs to be left at both ends of the plate, and two treatment areas need to be selected for the same treatment surface; the width of a treatment area is 15mm and the length is 130mm, and then the same area is slid and rubbed again after 1mm. After treating one surface, the plate is turned over and the sliding friction treatment with the same parameters is performed at the same position to obtain a VW94 composite material with a gradient structure on both sides.
[0069] Performance Testing:
[0070] The present application performs performance tests on the gradient structure Tip / VW94 composite material prepared in Example 1, the VW94 prefabricated alloy in step 1) (Comparative Example 1), the plate in step 1) (Comparative Example 2), and the VW94 alloy material after SFT in Comparative Example 1, specifically:
[0071] 1. Microstructure
[0072] 1) The VW94 prefabricated alloy in Comparative Example 1 was subjected to electron backscatter diffraction (EBSD) testing using a JEOL JSM-7800 field emission scanning electron microscope. The results are as follows: Figure 1 As shown, Figure 1 (a) IPF diagram of VW94 prefabricated alloy. Figure 1 (b) Grain size statistics and Figure 1 (c) Histogram of the proportion of small-angle grain boundaries. The grain size was calculated using the intercept method using Nano Measurer software. The average grain size of the original VW94 alloy is 8.1 μm. The white lines in the IPF diagram are small-angle grain boundaries, and their orientation difference is between 2 and 15°. According to statistics, the proportion of small-angle grain boundaries is 8%.
[0073] The present application uses a JEOL JSM-7800 field emission scanning electron microscope to perform secondary electron scanning and backscattering scanning on the VW94 alloy material after SFT in Comparative Example 1, with an operating voltage of 20KV. The results are as follows: Figure 2 As shown, the SFT front plane diagram of the VW94 alloy material is as follows Figure 2 (a); Plane diagram of SFT after deformation Figure 2 (b); SFT front cross-section Figure 2 (c); The cross-sectional view of SFT after deformation Figure 2(d), as can be seen from the figure, under the action of strain, the second phase as a whole is finer and more evenly distributed in the matrix. The blocky LPSO phase is elongated or even broken, and the layered LPSO phase is also twisted and broken under the action of large strain to coordinate the strain; in addition, the LPSO phase that was previously broken during extrusion is broken into smaller pieces under the action of stress and distributed at the grain boundaries; the fine β particles are still stably dispersed at the grain boundaries and in the grains. Studies have shown that the fine β-Mg5(Gd, Y) phase can have a dragging effect in the grain and hinder the growth of grains. In addition, in the sliding friction treatment, these second phase particles have a significant hindering effect on the movement of dislocations, resulting in dislocation pile-up. Therefore, the fine LPSO phase and β-Mg5(Gd, Y) phase dispersed at the grain boundaries both promote grain refinement. At the same time, the stress concentration at the interface between the α-Mg phase and the LPSO phase under stress can accelerate the grain refinement; in terms of mechanical properties, it is reported that when the elongated LPSO phase is consistent with the direction of load loading, it can act as a short fiber reinforcement phase to improve the strength of the alloy through load transfer.
[0074] The present application conducted an electron backscatter diffraction test (EBSD) on the plate in Comparative Example 2 using a JEOL JSM-7800 field emission scanning electron microscope. The results are as follows: Figure 3 As shown, Figure 3 (a) is the IPF diagram of the original composite material. Figure 3 (b) is the grain size distribution histogram. Figure 3 (c) is the distribution diagram of the proportion of small-angle grain boundaries. The grain size was counted by Nano Measurer software using the intercept method. According to statistics, the average grain size is 3.1μm; the white line in the IPF diagram is the small-angle grain boundary, and the orientation difference of the small-angle grain boundary is between 2 and 15°; according to statistics, the proportion of small-angle grain boundaries is 13%.
[0075] 2) Grain size
[0076] This application uses optical microscopy (OM) to analyze the microstructure of metal materials using the principle of geometric optical imaging. The prepared ultrafine-grained gradient structure Tip / VW94 composite material was observed for microstructure. The results are as follows: Figure 4 As shown in the figure, it can be seen that the surface grains of the gradient structure Tip / VW94 composite material are refined to 87nm, and a gradient deformation layer with a thickness of about 400μm is produced; according to the evolution law of the microstructure, its grain refinement mechanism is: after the start of SFT, a large number of dislocations are activated and promote the formation of small-angle grain boundaries, there are a small number of twins coordinated deformation, the twin boundaries divide the coarse grains, and the small-angle grain boundaries transform into large-angle grain boundaries under the action of strain. Under the synergistic effect of shear bands and stacking faults, the material grains are significantly refined.
[0077] 3) Mechanical properties test
[0078] The present application uses a tensile testing machine (CMT-5105 universal tensile testing machine) to test the mechanical properties (strength, elongation, etc.) of the gradient structure Tip / VW94 composite material prepared in Example 1, the VW94 prefabricated alloy in step 1) (Comparative Example 1), the plate in step 1) (Comparative Example 2), and the VW94 alloy material after SFT in Comparative Example 1 (this test is a room temperature test). The specific test data are shown in Table 1, and the engineering stress-strain curve and tensile performance bar graph are shown in Table 1. Figure 5 (a) and 5(b):
[0079] Table 1 Mechanical properties test results of different samples
[0080] Sample performance Tensile strength / MPa Yield strength / MPa Elongation / % Example 1 383 309 8.7 Comparative Example 1 307 220 15.8 Comparative Example 2 329 254 10.6 Comparative Example 1 334 253 15.4
[0081] From Table 1 Figure 5 It can be seen that the tensile strength (UTS) and yield strength (YS) of the gradient structure Tip / VW94 composite material have been improved to a certain extent, among which the tensile strength (UTS) has increased from 329MPa to 383MPa, an increase of 54MPa; the yield strength (YS) has increased from 254MPa to 309MPa, an increase of 55MPa; in addition, while the strength has increased, the elongation after fracture (EL) has not been significantly affected, only decreasing from 10.6% of the Ti-reinforced sheet (Comparative Example 2) to 8.7%. From the data of Example 1 and the data of Comparative Example 1, Comparative Example 2 and Comparative Example 1, it can be seen that the present application adopts the method of first reinforcing the VW94 prefabricated alloy with Ti particles, and then constructing a gradient structure by sliding friction (SFT), which significantly enhances the ultimate tensile strength and yield strength of the composite material, and only slightly decreases in elongation, that is, to a certain extent, the purpose of simultaneously improving mechanical strength and elongation is achieved.
[0082] 4) Hardness test
[0083] The present application uses a microhardness tester to test the hardness of the VW94 prefabricated alloy (Comparative Example 1) in step 1) on the gradient structure Tip / VW94 composite material prepared in Example 1. The cross-sectional hardness of the gradient structure Tip VW94 composite material also shows a gradient change, wherein the near-surface hardness value reaches 131.1 HV, which is 23.1% higher than the original state.
[0084] 5) The present application uses a FEI Technai F20 transmission electron microscope to observe the morphology using TEM absorption contrast images; use electron diffraction and other diffraction techniques to determine the material phase; and due to the high resolution of TEM, it is possible to observe the defects in the crystal, determine the defect type, estimate the defect density, etc.; and use high-angle annular dark field imaging-scanning transmission electron microscopy technology to characterize the dispersion at the atomic level. The gradient structure Tip / VW94 composite material prepared in Example 1 and the VW94 alloy material after SFT in Comparative Example 1 were tested by transmission electron microscope (TEM), and the results are as follows: Figure 6 As shown, the high strain TEM morphology of the gradient structure Tip / VW94 composite material Figure 6 (a), Selected area electron diffraction pattern Figure 6 (b), average grain size distribution histogram Figure 6 (c), and stacking faults Figure 6 (d); from Figure 6 It can be seen that after sliding friction treatment, the grain refinement degree of the composite material is less than that of the alloy; this is because a large number of rare earth-rich phases with a size less than 20 nm in the gradient structure Tip / VW94 composite material will pin the subgrain boundaries, hinder the transformation of subgrain boundaries to high-angle grain boundaries, and inhibit grain refinement ( Figure 5 ); and the strengthening effect of the gradient structure on the 3.5wt.% Ti / VW94 composite material is better than that of the VW94 alloy. This is because the stress mismatch between the Ti particles and the matrix in the gradient structure Tip / VW94 composite material under strain leads to the formation of a strain mismatch field, which hinders dislocation migration and promotes strengthening while providing energy for twin nucleation and inducing twin boundary strengthening.
[0085] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a gradient structure Tip / VW94 composite material containing ultrafine grains, characterized in that: The method comprises the following steps: 1) adding Ti particles to the cast alloy and dispersing the particles uniformly to prepare a Tip / VW94 magnesium-based composite material; 2) performing homogenization heat treatment and hot extrusion on the Tip / VW94 magnesium-based composite material obtained in step 1) to obtain a composite plate; 3) The composite plate material in step 2) is subjected to sliding friction treatment to obtain a gradient structure Tip / VW94 composite material containing ultrafine grains.
2. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 1, characterized in that: The step 1) is specifically as follows: in an inert atmosphere, the VW94 prefabricated alloy is heated and melted, and after the VW94 prefabricated alloy is completely melted, the temperature is lowered to a semi-solid temperature, and at the same time, the preheated aluminum foil wrapped with Ti particles is added to the melt and mechanical stirring is started; after the mechanical stirring is completed, the melt is heated, and when the temperature rises to 700° C., ultrasonic dispersion is performed, and then rapid water cooling is performed to obtain the Tip / VW94 magnesium-based composite material.
3. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 1, characterized in that: The specific method of the dispersion is: the dispersion is uniformly dispersed by combining mechanical stirring and ultrasonic dispersion, wherein the speed of mechanical stirring is 250-350r / min for the first 3-5 minutes and the speed is 550-750r / min for the last 1-3 minutes; the power of ultrasonic dispersion is 1-3kw and the ultrasonic dispersion is 5-15min.
4. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 1, characterized in that: In step 1), the mass fraction of the Ti particles in the cast alloy is 1-5%, and the particle size of the Ti particles is 5-10 μm。 5. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 4, characterized in that: The process parameters of the homogenization heat treatment in step 2) are: firstly treat at a temperature of 510-550° C. for 4-6 hours, then cool to 450-550° C. with the furnace and continue homogenization for 2-4 hours.
6. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 1, characterized in that: The process parameters of the hot extrusion in step 2) are: extrusion temperature is 400-600°C, and extrusion ratio is (15-25):
1.
7. The method for preparing the gradient structure Tip / VW94 composite material containing ultrafine grains according to claim 1, characterized in that: The sliding friction treatment in step 3) is specifically as follows: load 300-500N, sliding speed 0.2m / s, and sliding friction parameters repeated 30 times.
8. The method for preparing the ultrafine-grained gradient structure Tip / VW94 composite material according to claim 4, characterized in that: The cast alloy is VW94 cast magnesium alloy.
9. A gradient structure Tip / VW94 composite material containing ultrafine grains prepared by the preparation method according to any one of claims 1 to 8.
10. The ultrafine-grained gradient structure Tip / VW94 composite material according to claim 9, characterized in that: The surface of the ultrafine-grained gradient-structure Tip / VW94 composite material constructs a gradient deformation layer with a thickness of 300-500 μm, and the grain size in the deformation layer in the high-strain region is refined to 80-95 nm.
Citation Information
Cited By
Preparation method and application of metal surface nanocrystalline based on controllable fretting friction
CN121250042A