Catalyst ink as well as preparation method and application thereof

Through catalyst ink of aqueous polyurethane and modified silver nanopowder, combined with air plasma treatment and electroless plating technology, the high cost and complex steps in the preparation of flexible metal conductors are solved, and rapid curing and efficient preparation of highly conductive and flexible metals are achieved. Conductors are green and environmentally friendly and widely applicable.

CN119020765APending Publication Date: 2024-11-26NORTHWESTERN POLYTECHNICAL UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411114377.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art has problems of high costs, waste of materials and complex steps in the preparation of flexible metal conductors, especially when using traditional electrodeposition methods, the need for expensive palladium metal catalysts, and the curing time is too long and often involves organic solvents. .

Method used

Using water-based polyurethane as an auxiliary agent and binder to prepare catalyst ink, combined with air plasma treatment and electroless plating technology, the preparation of flexible metal conductors can be achieved quickly cured and patterned at low temperatures, avoiding the use of organic solvents, and using modifications silver nanopowder to reduce costs.

Benefits of technology

It realizes efficient preparation of patterned metal conductors with high conductivity and good flexibility on a variety of flexible substrates, shortens curing time and reduces costs, and the catalyst ink has green and environmentally friendly characteristics, and is suitable for many types of substrates, and the preparation process Simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020765A_ABST
    Figure CN119020765A_ABST
Patent Text Reader

Abstract

The invention provides catalyst ink as well as a preparation method and application thereof, and belongs to the technical field of preparation of flexible electronic devices. The catalyst ink is prepared from the following components in percentage by mass: 25 to 33 percent of waterborne polyurethane, 50 to 65 percent of metal nano powder, 1 to 5 percent of waterborne cross-linking agent, 0 to 3 percent of waterborne thickening agent, 0 to 3 percent of waterborne defoaming agent and the balance of water, and the total mass percent is 100 percent. The prepared catalyst ink does not need to use an organic solvent, and the curing time is short when the catalyst ink is used for preparing a patterned flexible metal conductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flexible electronic device preparation, and more specifically to a catalyst ink and a preparation method and application thereof. Background Art

[0002] With the rapid development of science and technology and the continuous progress of society, flexible electronic devices and wearable electronic products have emerged rapidly, which has driven the demand for flexible, lightweight and intelligent electronic products. As this demand grows, flexible metal conductors, as a key material, have received increasing attention. Compared with other conductive materials such as carbon materials and conductive polymers, metal materials have excellent conductivity and stability, so they are more popular and are widely used in flexible sensors, flexible circuits, electromagnetic shielding and other fields. However, integrating metals onto flexible substrates remains a challenge, especially considering the flexibility of the substrate and the preparation efficiency of flexible conductors.

[0003] Traditional methods for preparing metal conductors, such as photolithography and vacuum deposition, require expensive equipment and serious material waste when preparing flexible metals. In order to overcome these defects, a series of chemical methods have been developed to directly grow metals on flexible substrates to achieve a combination of high conductivity and flexibility. Among these methods, electroless deposition technology has attracted much attention due to its ability to continuously grow metal films. However, the current common electroless deposition methods usually include multiple steps, such as surface pretreatment, catalyst sensitization and activation, etc. These steps are not only complicated but also often involve expensive palladium metal catalysts. Chinese invention patent CN115910481A patent discloses a method for preparing flexible metal conductors based on resin binders, but the catalyst ink prepared by this invention has a too long curing time of 1h to 24h, and the preparation process often involves the use of organic solvents. Summary of the invention

[0004] In view of the above problems, the present invention provides a catalyst ink and a preparation method and application thereof. The catalyst ink prepared by the present invention does not require the use of organic solvents and has a short curing time when used to prepare patterned flexible metal conductors.

[0005] The first object of the present invention is to provide a catalyst ink, which is composed of the following components in percentage by mass:

[0006] 25% to 33% water-based polyurethane, 50% to 65% metal nanopowder, 1% to 5% water-based cross-linking agent, 0% to 3% water-based thickener, 0% to 3% water-based defoaming agent, and the rest is water, totaling 100%.

[0007] The present invention uses water-based polyurethane as an auxiliary agent and a binder to prepare catalyst ink. The water-based polyurethane can be quickly cured at low temperatures, shortening the curing time of the catalyst ink and saving time costs. In addition, since the water-based polyurethane has good dispersibility in water, water can be used when preparing the catalyst ink and cleaning the printing equipment, thereby avoiding the use of organic solvents. The prepared catalyst ink is green and environmentally friendly.

[0008] In a preferred embodiment of the present invention, the metal nanopowder is modified silver obtained by silanization of silver nanoparticles with a particle size of 60nm to 120nm. Silver is much cheaper than traditional palladium metal catalysts, and silver has good chemical stability and high catalytic activity.

[0009] In a preferred embodiment of the present invention, the water-based crosslinking agent is an aziridine crosslinking agent or a polycarbodiimide crosslinking agent. Taking the aziridine water-based crosslinking agent as an example, the reason why the present invention selects the aziridine water-based crosslinking agent is that the aziridine compound has a high reactivity and can effectively undergo a crosslinking reaction with the hydroxyl or amino group in the waterborne polyurethane. Secondly, the use of the aziridine crosslinking agent can provide good softness and elasticity. This type of crosslinking agent can make the catalyst ink maintain good flexibility after curing.

[0010] In a preferred embodiment of the present invention, the aqueous thickener is one or more of bentonite, attapulgite, aluminum silicate, cellulose thickener and acrylic thickener. Taking acrylic thickener as an example, the present invention selects acrylic thickener because it can be well integrated with water, and secondly, acrylic thickener can effectively control the rheological behavior of ink.

[0011] In a preferred embodiment of the present invention, the water-based defoamer is polyethylene glycol dimethyl ether or polyether-siloxane copolymer. Taking polyether-siloxane copolymer as an example, the present invention selects polyether-siloxane type water-based defoamers because the siloxane group has extremely low surface tension, can quickly diffuse to the interface between air and liquid, and can break the tiny bubbles formed on the interface. Secondly, the polyether-siloxane water-based defoamer has good chemical stability and resistance to temperature changes.

[0012] A second object of the present invention is to provide a method for preparing the above catalyst ink, comprising the following steps:

[0013] Weigh the components according to the following mass percentages: 25% to 33% water-based polyurethane, 50% to 65% metal nanopowder, 1% to 5% water-based crosslinking agent, 0% to 3% water-based thickener, 0% to 3% water-based defoaming agent, and the rest is water, totaling 100%;

[0014] The catalyst ink is obtained by uniformly mixing water-based polyurethane, metal nanopowder, water-based crosslinking agent, water-based thickener, water-based defoaming agent and water.

[0015] The third object of the present invention is to provide an application of the above catalyst ink in preparing a patterned flexible metal conductor. The preparation of the patterned flexible metal conductor comprises the following steps:

[0016] Printing the catalyst ink on a flexible substrate and curing it at room temperature to obtain a cured ink;

[0017] performing air plasma treatment on the cured ink to obtain treated ink;

[0018] The treated ink is moved to a metal salt solution containing a reducing agent for chemical plating to obtain a patterned flexible metal conductor.

[0019] The present invention moves the treated ink to a metal salt solution containing a reducing agent for chemical plating. During the chemical metal plating, the metal cations are reduced to elemental metals under the action of the reducing agent. The nano-metal in the ink itself is a good catalyst that can adsorb the metal cations in the metal salt solution containing the reducing agent and accelerate the transfer of electrons, thereby growing metal in the place where the ink is printed to obtain a patterned flexible metal conductor.

[0020] The catalyst ink prepared by the present invention can be printed on both a flat and dense substrate and a rough and porous substrate. The ink surface cured by air plasma treatment can greatly improve the catalytic efficiency and prepare a flexible metal conductor with high conductivity and strong adhesion.

[0021] In a preferred embodiment of the present invention, the curing time is 10 min to 30 min.

[0022] In a preferred embodiment of the present invention, the air plasma treatment has a treatment time of 1 min to 10 min and a power of 20 W to 90 W.

[0023] In a preferred embodiment of the present invention, the chemical plating is chemical copper plating or chemical gold plating.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses water-based polyurethane as an auxiliary agent and a binder. This resin can be cured at a relatively fast speed at a low temperature. Since water-based polyurethane has good dispersibility in water, water can be used when preparing catalyst ink or cleaning printing equipment, thereby avoiding the use of organic solvents.

[0026] By using the catalyst ink of the present invention, the efficient preparation of patterned metals can be achieved on various types of flexible substrates using an electroless deposition process, and has good application prospects in the field of flexible electronic devices.

[0027] (2) The catalyst ink prepared in the present invention is a water-based ink, and the entire preparation process does not involve the use of organic solvents. Therefore, the catalyst ink is green and environmentally friendly. In addition, the catalyst ink does not need to be heated during the curing process, and can be cured at room temperature for 10 minutes to 30 minutes, which effectively shortens the curing time. In addition, in subsequent use, it can ensure that the flexible patterned metal has good bending performance and conductivity.

[0028] (3) The present invention provides a method for preparing a patterned flexible metal conductor. No pretreatment of the flexible substrate is required. Metal nanoparticles are directly fixed on various types of flexible substrates by printing. The ink surface is cured by air plasma treatment and then chemically plated on the flexible substrate to form a patterned metal conductor with high adhesion, high conductivity and flexibility.

[0029] (4) The process flow of the present invention is simple. Different from the previous process of grafting polymers onto flexible substrates to load catalysts, the present invention can prepare highly conductive and flexible patterned metals through simple printing and solution processing.

[0030] (5) The present invention is universally applicable to most substrates, whether they are rough and porous substrates or flat and dense substrates. For rough and porous substrates, the catalyst ink can penetrate into the interior of the substrate, so that a mechanical locking relationship is formed between the catalyst ink and the flexible substrate, thereby enhancing the bonding strength. For most flat and dense substrates, the groups on their surfaces can form physical or chemical adsorption with the waterborne polyurethane, thereby ensuring the bonding strength between the catalyst ink and the flexible substrate.

[0031] (6) The method of the present invention is compatible with most printing methods. Depending on the shape of the metal pattern, the produced flexible metal can be used as a conductive circuit or as a metal electrode in a flexible device.

[0032] (7) The printed circuit or printed electrode of the present invention has good flexibility and can withstand relatively large deformations, such as bending, folding, curling, and twisting. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the three-layer structure of the present invention, wherein a shows a schematic diagram on a flat and dense substrate, and b shows a schematic diagram on a rough and porous substrate.

[0034] Figure 2 : are static water contact angle diagrams, wherein a is the static water contact angle diagram of the product printed on PET in Example 1 before air plasma treatment of the catalyst ink, and b is the static water contact angle diagram of the product printed on PET in Example 1 after air plasma treatment of the catalyst ink.

[0035] Figure 3 This is a diagram revealing the mechanism of improving the catalytic efficiency by treating the ink surface with air plasma in Example 1 of the present invention.

[0036] Figure 4 This is a bar graph of the surface resistance of the copper layer of the catalyst ink before and after air plasma treatment in Example 1 of the present invention.

[0037] Figure 5 These are optical microscope images and electron microscope images of the catalyst ink printed on the PET surface and after chemical copper plating in Example 1 of the present invention, wherein a is an optical microscope image of the catalyst ink printed on the PET surface, b is an electron microscope image of the catalyst ink printed on the PET surface with a scale of 30 μm, c is an electron microscope image of the catalyst ink printed on the PET surface with a scale of 5 μm, d is an optical microscope image after chemical copper plating, e is an electron microscope image after chemical plating with a scale of 30 μm, and f is an electron microscope image after chemical copper plating with a scale of 5 μm.

[0038] Figure 6 The PET in Example 1 of the present invention, the catalyst ink printed on the PET, and the XRD spectrum after chemical copper plating.

[0039] Figure 7 The bending test of the flexible copper metal prepared on PET in Example 5 of the present invention is performed, wherein Figure a is a relationship diagram between the normalized resistance value and the number of bending times, and Figure b is a partial enlarged diagram of Figure a.

[0040] Figure numerals: 1-flexible substrate material, 2-waterborne polyurethane-assisted catalyst layer, 3-chemically plated metal layer, 4-waterborne polyurethane, 5-modified silver, 6-chemically plated metal. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In the following specific embodiments, unless otherwise specified, all raw materials can be commercially available. The aqueous polyurethane used in the present invention was purchased from Sansheng Trading Co., Ltd., model PU-3407; the particle size of the silver nanoparticles is 60nm to 120nm; the aziridine crosslinker was purchased from Sansheng Trading Co., Ltd., model 150B; the acrylic acid aqueous thickener was purchased from Guanlin Chemical Technology Co., Ltd., model PTF; the polyether-siloxane aqueous defoamer was purchased from Zhonglian Federation Fine Chemical Co., Ltd., model B0626. The methacrylic acid aqueous thickener was purchased from Shandong Shoucheng Chemical Co., Ltd., model A28 thickener. Polyethylene terephthalate is denoted as PET, poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) is denoted as PEDOT:PSS, and the two-dimensional transition metal titanium carbide is denoted as Ti 3 C 2 T x .

[0043] The modified silver used in the present invention is obtained by silanization treatment of silver nanoparticles as raw materials, and the specific treatment steps are as follows:

[0044] An ethanol solution containing 5% deionized water was prepared, and 10 g of silver nanoparticles and 3-aminopropyltriethoxysilane accounting for 5% of the mass of the silver nanoparticles were added to 100 mL of the ethanol solution, and magnetic stirring was performed at 25° C. for 12 h. After stirring, vacuum filtration was performed, and the product obtained by filtration was placed in an oven at 90° C. in a vacuum environment and dried for 6 h to obtain modified silver.

[0045] Example 1

[0046] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0047] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0048] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0049] Step 2: Print the prepared catalyst ink on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm to form an interdigitated electrode pattern, and cure at room temperature for 30 minutes to obtain a PET printed with the catalyst ink.

[0050] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 6 minutes at a power of 50 W.

[0051] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 120 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0052] After chemical plating, the plating solution remaining on the pattern surface is washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, wherein chemical deposition can only occur in the area printed with catalyst ink to obtain PET after chemical copper plating, that is, the copper interdigital electrode prepared on PET.

[0053] Step 5: Prepare a flexible pressure sensor using the copper interdigital electrode prepared on PET as the bottom electrode and PEDOT:PSS spin-coated on the microstructured PDMS film as the top electrode. It should be noted that the patterned metal layer on PET is the copper interdigital electrode prepared on PET.

[0054] Example 2

[0055] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0056] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0057] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0058] Step 2: Print a large-area catalyst ink pattern of 5 cm in length and 5 cm in width on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm. Curing was carried out at room temperature for 30 minutes to obtain a PET printed with catalyst ink.

[0059] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 9 minutes at a power of 50 W.

[0060] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 30 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0061] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0062] Example 3

[0063] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0064] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0065] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0066] Step 2: Print a large-area catalyst ink pattern of 5 cm in length and 5 cm in width on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm. Curing was carried out at room temperature for 30 minutes to obtain a PET printed with catalyst ink.

[0067] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 9 minutes at a power of 50 W.

[0068] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 60 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0069] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0070] Example 4

[0071] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0072] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0073] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0074] Step 2: Print a large-area catalyst ink pattern of 5 cm in length and 5 cm in width on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm. Curing was carried out at room temperature for 30 minutes to obtain a PET printed with catalyst ink.

[0075] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 9 minutes at a power of 50 W.

[0076] Step 4, immersing the catalyst ink after air plasma treatment into a chemical copper plating solution, and performing chemical copper plating for 90 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0077] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0078] Example 5

[0079] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0080] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0081] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0082] Step 2: Print a large-area catalyst ink pattern of 5 cm in length and 5 cm in width on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm. Curing was carried out at room temperature for 30 minutes to obtain a PET printed with catalyst ink.

[0083] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 9 minutes at a power of 50 W.

[0084] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 120 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0085] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0086] Example 6

[0087] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0088] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0089] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0090] Step 2: Print a large-area catalyst ink pattern of 5 cm in length and 5 cm in width on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm. Curing was carried out at room temperature for 30 minutes to obtain a PET printed with catalyst ink.

[0091] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 9 minutes at a power of 50 W.

[0092] Step 4, immersing the catalyst ink after air plasma treatment into a chemical copper plating solution, and performing chemical copper plating for 150 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0093] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0094] Example 7

[0095] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0096] Step 1: 32.2% aqueous polyurethane, 64.3% modified silver, 1.6% aziridine crosslinking agent, 0.6% acrylic acid aqueous thickener and 1.3% polyether-siloxane aqueous defoaming agent are mixed according to mass percentage and then magnetically stirred to prepare catalyst ink.

[0097] Specifically, 1 g of waterborne polyurethane was weighed, and then 2 g of modified silver was weighed according to a mass ratio of waterborne polyurethane to modified silver of 1:2, 0.05 g of aziridine crosslinker was weighed according to a content of 5% of the mass of waterborne polyurethane, 0.02 g of waterborne thickener was weighed according to a content of acrylic acid waterborne thickener of 2% of the mass of waterborne polyurethane, and 0.04 g of polyether-siloxane defoamer was weighed according to a content of 4% of the content of waterborne polyurethane.

[0098] Step 2: Print the prepared catalyst ink on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm to form an interdigitated electrode pattern, and cure at room temperature for 30 minutes to obtain a PET printed with the catalyst ink.

[0099] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 6 minutes at a power of 50 W.

[0100] Step 4, immersing the catalyst ink after air plasma treatment into a chemical gold plating solution, and performing chemical gold plating for 150 minutes in an environment of 30°C, wherein the components of the chemical gold plating solution are: 3.39 g / L tetrachloroauric acid, 0.4 g / L sodium hydroxide, 6.95 g / L hydroxylamine hydrochloride, 11 g / L disodium hydrogen phosphate, 16 g / L sodium thiosulfate pentahydrate and 40 g / L sodium sulfite, and dissolving tetrachloroauric acid, sodium hydroxide, hydroxylamine hydrochloride, disodium hydrogen phosphate, sodium thiosulfate pentahydrate and sodium sulfite in deionized water to obtain a chemical gold plating solution.

[0101] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area printed with the catalyst ink, thereby obtaining a gold interdigital electrode prepared on PET.

[0102] Example 8

[0103] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0104] Step 1: Mix 30% waterborne polyurethane, 60% modified silver, 1% polycarbodiimide crosslinker, 2% waterborne thickener, 2% polyethylene glycol dimethyl ether and 5% water according to mass percentage and stir them magnetically to prepare catalyst ink. The polycarbodiimide crosslinker used in this embodiment is called Ucarlnk TM XL-29SE, the water-based thickener is a mixture of bentonite and aluminum silicate in a mass ratio of 1:1.

[0105] Step 2: Print the prepared catalyst ink on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm to form an interdigitated electrode pattern, and cure at room temperature for 15 minutes to obtain a PET printed with the catalyst ink.

[0106] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 6 minutes at a power of 50 W.

[0107] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 30 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0108] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0109] The C-layer resistance obtained after chemical plating is 268.3mΩ / □.

[0110] Example 9

[0111] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0112] Step 1: Mix 25% aqueous polyurethane, 50% modified silver, 5% aziridine crosslinking agent, 3% polyethylene glycol dimethyl ether and 17% water according to mass percentage and stir magnetically to prepare catalyst ink.

[0113] Step 2: Print the prepared catalyst ink on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm to form an interdigitated electrode pattern, and cure at room temperature for 10 minutes to obtain a PET printed with the catalyst ink.

[0114] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 1 minute at a power of 90 W.

[0115] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 60 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0116] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0117] The C-layer resistance obtained after chemical plating is 28.1mΩ / □.

[0118] Example 10

[0119] This embodiment provides a method for preparing a patterned flexible metal conductor, which comprises the following steps:

[0120] Step 1: 33% aqueous polyurethane, 65% modified silver, 1% aziridine crosslinker and 1% aqueous thickener are mixed according to mass percentage and then stirred magnetically to prepare catalyst ink. In this embodiment, the aqueous thickener is a mixture of attapulgite and hydroxymethyl cellulose in a mass ratio of 1:2.

[0121] Step 2: Print the prepared catalyst ink on a PET transparent film through a screen with a hollow line width of 500 μm and a line spacing of 500 μm to form an interdigitated electrode pattern, and cure at room temperature for 30 minutes to obtain a PET printed with the catalyst ink.

[0122] Step 3: Treat the PET printed with the catalyst ink with air plasma to improve the catalytic efficiency. The treatment conditions are: 10 minutes at a power of 20 W.

[0123] Step 4, immersing the catalyst ink after air plasma treatment into the chemical copper plating solution, and performing chemical copper plating for 60 minutes in an environment of 30°C, wherein the components of the chemical copper plating solution are: 15g / L copper sulfate pentahydrate, 14g / L potassium sodium tartrate, 19.5g / L disodium ethylenediaminetetraacetic acid, 14.5g / L sodium hydroxide, 0.02g / L 2,2-bipyridine, 0.01g / L potassium ferrocyanide and 15mL / L formaldehyde, and dissolving copper sulfate pentahydrate, potassium sodium tartrate, disodium ethylenediaminetetraacetic acid, sodium hydroxide, 2,2-bipyridine, potassium ferrocyanide and formaldehyde in deionized water to obtain a chemical copper plating solution.

[0124] After chemical plating, the plating solution remaining on the pattern surface was washed with deionized water, and then dried in an oven at 40°C for 15 minutes to obtain a patterned metal layer on PET, in which chemical deposition could only occur in the area where the catalyst ink was printed.

[0125] The C-layer resistance obtained after chemical plating is 27.1mΩ / □.

[0126] The schematic diagram of the three-layer structure of the patterned flexible metal layer prepared by the present invention is as follows Figure 1 As shown, Figure 1 a in the figure is a schematic diagram on a flat and dense substrate. Figure 1 b is a schematic diagram on a rough porous substrate. The prepared patterned flexible metal conductor is characterized and tested below.

[0127] like Figure 2 As shown in a, the static water contact angle of the ink surface in Example 1 before the air plasma treatment is 73°, and the infiltration state is not reached, which is not conducive to the subsequent chemical plating process. Figure 2 As shown in b, after air plasma treatment, the contact angle of the ink surface is 0°, indicating complete wetting, which undoubtedly helps improve the catalytic efficiency. In addition, before the ink surface is modified by air plasma, most of the modified silver surfaces will be coated with a thin layer of resin, and the catalyst particles at this time cannot effectively contact the chemical plating solution. When the cured ink surface is modified by air plasma, more catalytic sites will be exposed under the bombardment of high-energy particles, which undoubtedly helps improve the catalytic efficiency, such as Figure 3 shown.

[0128] Example 1 compares the surface resistance of the copper layer deposited before and after the air plasma treatment of the ink surface. Figure 4As shown in the figure, when the deposition time is extended to 120 min, the surface resistance of the copper layer on the ink surface that has not been modified by air plasma is 1160.2 mΩ / □, while the surface resistance of the copper layer on the ink surface that has been modified has been reduced to 8.1 mΩ / □, and the copper layer has shown high conductivity. In summary, the ink surface cured by air plasma treatment can improve the hydrophilicity of the ink surface and expose more catalytic sites, thus greatly improving the catalytic efficiency of subsequent chemical plating.

[0129] The catalyst ink prepared according to Example 1 was used to print interdigital electrodes with a line width of 500 μm on the surface of PET using screen printing technology. Figure 5 The pattern shown in a in the figure shows that the ink has good precision. After further chemical copper plating, Figure 5 As shown in d in the figure, the line width basically maintains the original accuracy and no obvious diffusion occurs. Figure 5 b and Figure 5 Figure c is a partial enlarged image of the catalyst ink printed on the PET surface. It can be seen that the ink surface is relatively rough. Figure 5 e and Figure 5 As shown in Figure 5(f), a dense copper layer is formed on the ink surface, indicating that the metal is deposited on the substrate surface.

[0130] In order to verify the chemical composition of the metal pattern prepared in Example 1, X-ray diffraction analysis was performed on PET, PET printed with catalyst ink, and PET after chemical copper plating. Figure 6 As shown, the peak at 25.96° is the characteristic peak of the PET substrate. In the XRD spectrum of the catalyst ink, the diffraction peaks at 38.2°, 44.4°, 64.6° and 77.5° fully match the (111), (200), (220) and (311) crystal planes of AgNPs, respectively. The XRD spectrum after the chemical plating of the copper layer shows that the diffraction peaks at 43.45°, 50.60° and 74.2° fully match the (111), (200) and (220) crystal planes of the copper layer, successfully proving the existence of copper. It is worth noting that only the diffraction peaks of elemental copper were found after chemical plating, but no diffraction peaks of copper oxide and other impurities were found. It can be inferred that the prepared flexible copper conductor has high conductivity.

[0131] In order to verify the application prospect of the copper interdigital electrode prepared in Example 1 in flexible electronic devices, the copper interdigital electrode prepared on PET was used as the bottom electrode. PEDOT:PSS was spin-coated on the microstructured polydimethylsiloxane film as the top electrode, and the side with PEDOT:PSS was opposite to the copper interdigital electrode surface, and finally packaged with 3M tape to construct a flexible pressure sensor, which has high sensitivity, wide detection range, fast response and recovery time, and can be used to monitor physiological signals such as human vocal cord sounding and finger bending.

[0132] Table 1 shows the Cu layer obtained by changing the chemical plating time according to the preparation method of Examples 2 to 6. Different chemical copper plating times correspond to different copper layer thicknesses and surface resistances. Specifically, when the chemical copper plating time is extended from 30 min to 60 min, 90 min, 120 min, and 150 min, copper layers with thicknesses of 0.7 μm, 1.3 μm, 2.2 μm, 2.7 μm, and 2.9 μm can be obtained. As the thickness increases, the surface resistance gradually decreases, which are 251.1 mΩ / □, 26.8 mΩ / □, 11.9 mΩ / □, 9.1 mΩ / □, and 7.5 mΩ / □, respectively. The copper layer with a deposition time of 150 min has a very low resistivity, which is close to 77.3% of the resistivity of bulk copper, and the resistivity is 2.2×10 -8 Ω·m, indicating that the copper layer prepared by this method has a very high electrical conductivity.

[0133] Table 1 Cu layer thickness and surface resistance obtained at different chemical copper plating times

[0134] Example 2 Example 3 Example 4 Example 5 Example 6 Deposition time (min) 30 60 90 120 150 Cu layer thickness (μm) 0.7 1.3 2.2 2.7 2.9 C-plane resistance (mΩ / □) 251.1 26.8 11.9 9.1 7.5

[0135] Based on Example 5, the copper layer prepared on PET has strong bonding strength. The bonding strength of the copper layer prepared on PET was tested using a grid knife and 3M tape. The copper layer was cut into 100 squares with a side length of 1 mm using a grid knife. The 3M tape was pasted on the surface of the copper layer, the bubbles were squeezed out, and the tape was peeled off from the surface of the copper layer with a uniform force. No large amount of copper layer was found to peel off, which proves that the prepared flexible metal has good bonding strength.

[0136] Based on the flexible metal prepared on PET in Example 5, it was cut into metal strips with a length of 50 mm and a width of 5 mm, and clamped on a stretching table. The bending test of the flexible conductor was carried out by contraction and stretching of the stretching table. The flexible copper conductor prepared on the PET substrate had two bending states on the stretching machine, where the bending radius r was 5.58 mm and 2.50 mm respectively. Figure 7 a in the figure is the relationship curve between the normalized resistance and the bending times in two bending states. The chemical plating time is 120 min. Figure 7From the enlarged curve of the 4990th to 5000th bending cycles in b, it can be found that when the bending radius is 5.58 mm, after 5000 bending cycles, the normalized resistance is still maintained at 1, indicating that the resistance has basically not changed, and when the bending radius is 2.50 mm, after 5000 bending cycles, the normalized resistance only increases to 1.1. In summary, the flexible copper conductor prepared in this embodiment has good bending performance.

[0137] Based on the patterned flexible metal conductor prepared in Example 7, the gold interdigital electrodes prepared on PET are used as current collectors, Zn is electrodeposited as the negative electrode material on one side of the gold interdigital electrode current collector by electrodeposition technology, and Ti is printed on the other side of the interdigital electrodes by screen printing technology. 3 C 2 T x The ink is used as the positive electrode material, and then a layer of gel electrolyte is coated on the positive and negative electrode materials, and finally a PET film is used to encapsulate the planar energy storage device. The planar energy storage device has an excellent area capacity of 153.3mF·cm -2 , and it has good mechanical flexibility and can maintain similar electrochemical properties at different bending angles.

[0138] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0139] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention are within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A catalyst ink, characterized in that: The catalyst ink is composed of the following components in percentage by mass: 25% to 33% water-based polyurethane, 50% to 65% metal nanopowder, 1% to 5% water-based cross-linking agent, 0% to 3% water-based thickener, 0% to 3% water-based defoaming agent, and the rest is water, totaling 100%.

2. A catalyst ink according to claim 1, characterized in that: The metal nano powder is modified silver obtained by silanization treatment of silver nanoparticles with a particle size of 60nm to 120nm.

3. A catalyst ink according to claim 1, characterized in that: The water-based crosslinking agent is an aziridine crosslinking agent or a polycarbodiimide crosslinking agent.

4. The catalyst ink according to claim 1, characterized in that: The aqueous thickener is one or more of bentonite, attapulgite, aluminum silicate, cellulose thickener and acrylic thickener.

5. The catalyst ink according to claim 1, characterized in that: The aqueous defoamer is polyethylene glycol dimethyl ether or polyether-siloxane copolymer.

6. A method for preparing the catalyst ink according to any one of claims 1 to 5, characterized in that: The following steps are involved: Weigh the components according to the following mass percentages: 25% to 33% water-based polyurethane, 50% to 65% metal nanopowder, 1% to 5% water-based crosslinking agent, 0% to 3% water-based thickener, 0% to 3% water-based defoaming agent, and the rest is water, totaling 100%; The catalyst ink is obtained by uniformly mixing water-based polyurethane, metal nanopowder, water-based crosslinking agent, water-based thickener, water-based defoaming agent and water.

7. Use of the catalyst ink according to any one of claims 1 to 5 in preparing a patterned flexible metal conductor, characterized in that: The preparation of the patterned flexible metal conductor includes the following steps: Printing the catalyst ink on a flexible substrate and curing it at room temperature to obtain a cured ink; performing air plasma treatment on the cured ink to obtain treated ink; The treated ink is moved to a metal salt solution containing a reducing agent for chemical plating to obtain a patterned flexible metal conductor.

8. The use of the catalyst ink according to claim 7 in preparing a patterned flexible metal conductor, characterized in that: The curing time is 10min to 30min.

9. The use of the catalyst ink according to claim 7 in preparing a patterned flexible metal conductor, characterized in that: Air plasma treatment, the treatment time is 1min to 10min, and the power is 20W to 90W.

10. The use of the catalyst ink according to claim 7 in preparing a patterned flexible metal conductor, characterized in that: The chemical plating is chemical copper plating or chemical gold plating.

Citation Information

Patent Citations

  • Method for preparing flexible metal conductor based on resin binder

    CN115910481A