Laser cladding machine, cylinder sleeve manufacturing method and cylinder sleeve

The laser cladding machine forms a cladding layer of Ni60% WC alloy powder on the inner hole surface of the cylinder liner, which solves the problem of poor hardness and wear resistance of the inner hole of the bimetallic cylinder liner, extends the service life and prevents high-temperature deformation, and achieves the improvement High bonding strength and wear resistance.

CN119020774APending Publication Date: 2024-11-26JIANGSU YUANFANG POWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113754.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing bimetal cylinder liner has short service life due to poor surface hardness and poor wear resistance in drilling mud pumps, and deformation failure caused by high temperature friction.

Method used

A laser cladding machine is used to form a cladding layer of Ni60% WC alloy powder on the inner hole surface of the cylinder liner. The laser cladding process is carried out through induction heating and a synchronously moving cladding gun to improve the surface hardness and wear resistance of the inner hole of the cylinder liner. , and optimize the coating bond strength by adjusting the powder spray focal length and airflow parameters.

Benefits of technology

It significantly improves the surface hardness and wear resistance of the inner holes of the cylinder liner, extends the service life, and prevents deformation at high temperatures, and shows higher bonding strength and better wear resistance than bimetallic cylinder liner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020774A_ABST
    Figure CN119020774A_ABST
Patent Text Reader

Abstract

The invention relates to a laser cladding machine which comprises a machine tool body, and a chuck and a sliding seat assembly are arranged on the machine tool body. The chuck is used for clamping one end of the cylinder sleeve, and a cladding gun is mounted on the sliding seat assembly; and the transmission screw rod drives the cladding gun and the induction heating coil to synchronously and longitudinally move. A cylinder sleeve manufacturing method adopts the laser cladding machine and comprises the following steps that a cylinder sleeve blank is preheated and installed on the chuck; ni60% WC alloy powder is adopted, an inner hole of the cylinder sleeve is machined through a gun needle of a cladding gun, a cladding layer is formed on the inner wall of the cylinder sleeve, and manufacturing of the novel slurry pump cylinder sleeve is completed. The cylinder sleeve comprises a cylinder sleeve base body, and a cladding layer is arranged in an inner hole of the cylinder sleeve base body. The surface hardness of the inner hole of the cylinder sleeve is improved, so that the wear resistance is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mechanical parts processing and manufacturing, and in particular to a laser cladding machine, a method for manufacturing a drilling mud pump cylinder sleeve, and a mud pump cylinder sleeve. Background Art

[0002] At present, bimetallic cylinder liners are widely used in water injection pumps. The cylinder liners are made of bimetal, and the outer layer is made of 45 steel. After quenching and tempering, the tempered troostite structure is obtained, which has good comprehensive performance. Its inner layer is high-chromium white alloy cast iron. The failure characteristics of high-chromium cast iron cylinder liners are: wear of the martensite matrix and breakage and shedding of the protruding carbides, which occur alternately until failure. The breakage and shedding of carbides are the main mechanisms of cylinder liner wear failure. In order to improve the life of the cylinder liner, the breakage and shedding rate of carbides must be controlled. The selection of appropriate cylinder liner surface hardness can effectively improve the life of the high-chromium cast iron liner. Centrifugal casting can be used, and after quenching + tempering treatment, martensite + alloy carbide + residual austenite structure can be obtained, with a hardness of HRC55~60. When processing the inner hole of the liner, the inner wall machining allowance should be controlled to be less than 5mm as much as possible to retain the fine grain area after casting. The advantages of bimetallic cylinder liners are corrosion resistance, abrasion resistance, good running-in and high smoothness of the working surface; the disadvantages are short life and performance needs to be improved.

[0003] When the drilling mud pump is working normally, the piston reciprocates in the cylinder sleeve. On the one hand, the sand and gravel (mainly SiO 2 On the other hand, the bimetallic cylinder liner is a combination of an inner liner (high chromium cast iron) and an outer liner (45 steel). The high temperature generated by the friction between the piston and the cylinder liner causes the air in the joint gap to expand faster than the metal, causing the bimetallic cylinder liner to deform and fail. Due to these two reasons, the actual service life of the bimetallic cylinder liner is only about one week, and its performance needs to be improved. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide a laser cladding machine, a method for manufacturing a drilling mud pump cylinder sleeve and a mud pump cylinder sleeve, and solve the technical problems of poor hardness and poor wear resistance of the inner hole surface of the previous bimetallic cylinder sleeve.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] First aspect:

[0007] A laser cladding machine is provided, comprising:

[0008] The machine tool body has a chuck and a slide assembly disposed on the machine tool plate; the slide assembly is driven by a transmission screw on the machine tool to translate;

[0009] The chuck clamps one end of the cylinder sleeve, a cladding gun is installed on the slide assembly, and a gun needle of the cladding gun extends into the cylinder sleeve;

[0010] A coil seat is provided with an induction heating coil, the cylinder sleeve is located in the induction heating coil, and the coil seat is connected to a transmission screw; the transmission screw drives the cladding gun and the induction heating coil to move longitudinally synchronously.

[0011] Furthermore, the slide assembly includes

[0012] A longitudinal slide seat, a transverse slide seat and an adjusting screw rod, wherein the longitudinal slide seat is longitudinally slidably arranged on the machine tool body, the transmission screw rod is connected to the longitudinal slide seat, the transverse slide seat is transversely slidably arranged on the longitudinal slide seat, and the cladding gun is installed on the transverse slide seat;

[0013] The adjusting screw rod is arranged on the longitudinal sliding seat and connected with the transverse sliding seat. The adjusting screw rod is suitable for adjusting the transverse position of the cladding gun on the machine tool.

[0014] Furthermore, the powder spraying focal length of the cladding gun is 1.2-1.8 mm.

[0015] Second aspect:

[0016] A method for manufacturing a drilling mud pump cylinder sleeve is provided, using the above-mentioned laser cladding machine, comprising the following steps:

[0017] Step S01, selecting a steel pipe and rough turning it into a cylinder liner blank according to size;

[0018] Step S02, preheating the cylinder liner blank to 340-360° C., and then mounting the cylinder liner blank on a chuck;

[0019] Step S03, using Ni60WC alloy powder, the inner hole of the cylinder liner is processed by the gun needle of the cladding gun, and the processing parameters are:

[0020] The powder spray focal length is 1.2-1.8mm, the heating temperature of the induction heating coil is 350℃, the laser power of the cladding gun is 1700W, the cladding speed is 0.9-1.1m / min; single-channel traverse: 1.4-1.6mm; powder feeding speed: 1.5-2.0r / min; protective airflow: 13-15L / min; powder-carrying airflow: 4-6L / min.

[0021] During the laser cladding process, the transmission screw drives the induction heating coil and the cladding gun to move synchronously;

[0022] Step S04, after the laser cladding process is completed, a cladding layer is formed on the inner wall of the cylinder liner, the inner hole surface roughness is reduced to below Ra0.4μm by internal grinding, the chamfer is ground, and the outer surface is painted to complete the production of the new mud pump cylinder liner.

[0023] Furthermore, in step S02, the cylinder liner blank is preheated to 500°C and then kept warm to 340-360°C.

[0024] The third aspect:

[0025] A cylinder sleeve is provided, comprising

[0026] A cylinder liner substrate, wherein the inner hole of the cylinder liner substrate is provided with a cladding layer;

[0027] The cladding layer is manufactured by adopting the above-mentioned method for manufacturing the cylinder sleeve of a drilling mud pump.

[0028] The beneficial effects of the present invention are:

[0029] A cladding layer made of Ni60% WC alloy powder is formed inside the cylinder liner by laser cladding to increase the surface hardness of the inner hole of the cylinder liner and thus enhance its wear resistance. At the same time, the laser cladding coating and the substrate are metallurgically bonded and do not deform at high temperatures, thereby extending the service life of the cylinder liner. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described below in conjunction with the accompanying drawings.

[0031] Figure 1 It is a schematic diagram of the laser cladding machine of the present invention;

[0032] Figure 2 is a schematic diagram of a cladding gun head of the present invention;

[0033] Figure 3 It is a schematic diagram of the mud pump cylinder sleeve;

[0034] Among them, 1. machine tool body, 11. transmission screw;

[0035] 21. Longitudinal sliding seat, 22. Horizontal sliding seat, 23. Adjusting screw rod;

[0036] 3. Cladding gun;

[0037] 41. coil holder, 42. induction heating coil;

[0038] 51. Molten pool, 52. Laser, 53. Alloy powder;

[0039] 61. Cylinder liner substrate, 61. Cladding layer. DETAILED DESCRIPTION

[0040] The present invention will now be further described in conjunction with specific embodiments. These drawings are simplified schematic diagrams that only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.

[0041] This embodiment provides a laser cladding machine, such as Figure 1 Figure 2 As shown, the laser cladding machine includes

[0042] A machine tool body 1, on which a chuck and a slide assembly are arranged; the slide assembly is driven by a transmission screw 11 on the machine tool to translate;

[0043] The chuck clamps one end of the cylinder sleeve, and a cladding gun 3 is installed on the slide assembly, and a gun needle of the cladding gun 3 extends into the cylinder sleeve;

[0044] The coil seat 41 is provided with an induction heating coil 42 , the cylinder sleeve is located in the induction heating coil 42 , and the coil seat 41 is connected to the transmission screw 11 ; the transmission screw 11 drives the cladding gun 3 and the induction heating coil 42 to move synchronously longitudinally.

[0045] The induction heating coil 42 is connected to an induction heating power source nearby.

[0046] Specifically, as an optional implementation in this embodiment, Figure 1 As shown, the slide assembly includes

[0047] A longitudinal slide seat 21, a transverse slide seat 22 and an adjusting screw 23, wherein the longitudinal slide seat 21 is longitudinally slidably arranged on the machine tool body 1, the transmission screw 11 is connected to the longitudinal slide seat 21, the transverse slide seat 22 is transversely slidably arranged on the longitudinal slide seat 21, and the cladding gun 3 is installed on the transverse slide seat 22;

[0048] The adjusting screw rod 23 is arranged on the longitudinal sliding seat 21 and connected to the transverse sliding seat 22 . The adjusting screw rod 23 is suitable for adjusting the transverse position of the cladding gun 3 on the machine tool.

[0049] Specifically, as an optional implementation in this embodiment, Figure 2 As shown, the powder spraying focal length of the cladding gun 3 is 1.2-1.8 mm.

[0050] Working principle of laser cladding machine:

[0051] The machine tool controller controls the operation of the transmission screw 11. Since the coil seat 41 and the longitudinal slide seat 21 are connected to the transmission screw 11 at the same time, the transmission screw 11 can drive the coil seat 41 and the longitudinal slide seat 21 to move synchronously, that is, the induction heating coil 42 and the cladding gun 3 can move synchronously.

[0052] The adjusting screw rod 23 drives the horizontal sliding seat 22 to move horizontally, that is, drives the cladding gun 3 to move radially in the cylinder sleeve, and adjusts the distance between the gun head of the cladding gun 3 and the inner wall of the cylinder sleeve.

[0053] This embodiment provides a method for manufacturing a drilling mud pump cylinder sleeve, such as Figure 1 Figure 2 As shown, the above-mentioned laser cladding machine is used, including the following steps:

[0054] Step S01, selecting a steel pipe and rough turning it into a cylinder liner blank according to size;

[0055] Step S02, preheating the cylinder liner blank to 340-360° C., and then mounting the cylinder liner blank on a chuck;

[0056] Step S03, using Ni60WC alloy powder 53, the inner hole of the cylinder sleeve is processed by the gun needle of the cladding gun 3, and the processing parameters are:

[0057] The powder spraying focal length is 1.2-1.8 mm, the heating temperature of the induction heating coil 42 is 350°C, the laser power of the cladding gun 3 is 1700 W, the cladding speed is 0.9-1.1 m / min; single-channel traverse: 1.4-1.6 mm; powder feeding speed: 1.5-2.0 r / min; protective airflow: 13-15 L / min; powder-carrying airflow: 4-6 L / min.

[0058] During the laser cladding process, the transmission screw 11 drives the induction heating coil 42 to move synchronously with the cladding gun 3;

[0059] Step S04, after the laser cladding process is completed, a cladding layer is formed on the inner wall of the cylinder liner, the inner hole surface roughness is reduced to below Ra0.4μm by internal grinding, the chamfer is ground, and the outer surface is painted to complete the production of the new mud pump cylinder liner.

[0060] Specifically, as an optional implementation in this embodiment, in step S02, the cylinder liner blank is first preheated to 500°C and then kept warm to 340-360°C.

[0061] In this embodiment, the cylinder liner is finally kept warm at 350°C.

[0062] The purpose of ensuring the constant temperature of the cylinder liner and the synchronous movement of the induction heating coil 42 and the cladding gun 3 is to ensure that the cylinder liner of the mud pump is always kept at a constant temperature and solve the problem of mismatch between the linear expansion coefficients of Ni60% WC powder and the substrate.

[0063] like Figure 2 As shown, the powder spraying focal length L is the distance between the intersection of the alloy powder 53 and the underlying substrate. The laser 52 carries the alloy powder 53 to the substrate to form a molten pool 51 .

[0064] In the method for manufacturing the cylinder sleeve of a drilling mud pump, when the following processing parameters are constant, the cladding speed is 1.0 m / min; the single-pass traverse is 1.5 mm; the powder feeding speed is 1.7 r / min; the protective air flow is 13-15 L / min; the powder-carrying air flow is 5.0 L / min; the laser power is controlled at 1700 W. At this time, by controlling the powder spraying focal length L, the following test data are obtained, which are summarized in the following table:

[0065]

[0066] It can be seen from the table that when the powder spraying focal length L is 1.0mm, although the bonding strength is high, it is basically burned and the cylinder liner cannot be used; when the powder spraying focal length L is 2.0mm, the bonding strength of the coating on the substrate is low and it is easy to fall off. In this embodiment, the powder spraying focal length L is preferably 1.5mm, the bonding strength of the coating on the substrate is moderate, and the coating appearance is good.

[0067] The drilling mud pump cylinder liner manufacturing method of the present invention involves working parameters only for a specific alloy powder 53, namely Ni60% WC alloy powder 53; and cladding is performed at a specific power (1700W), and the powder spraying focal length is limited to 1.2-1.8mm, preferably 1.5mm; combined with cladding speed: 1.0m / min; single-channel lateral displacement: 1.5mm; powder feeding speed: 1.7r / min; protective airflow: 13-15L / min; powder-carrying airflow: 5.0L / min, these parameters, the processed coating has high bonding strength and enhances its wear resistance; at the same time, the laser cladding coating and the substrate are metallurgically bonded and do not deform at high temperatures, thereby extending the service life of the cylinder liner.

[0068] This embodiment provides a cylinder sleeve, comprising

[0069] A cylinder liner substrate, wherein the inner hole of the cylinder liner substrate is provided with a cladding layer;

[0070] The cladding layer is manufactured by adopting the above-mentioned method for manufacturing the cylinder sleeve of a drilling mud pump.

[0071] The laser cladding coating and the substrate are metallurgically bonded, with extremely high bonding strength. Compared with thermal spraying and electroplating, there is no coating shedding.

[0072] Compared with the nested bonding of bimetallic cylinder liners, the metallurgical bonding has no pores on the bonding surface and no possibility of high-temperature deformation.

[0073] The inner hole surface hardness and wear resistance of the nickel-based tungsten carbide coating are greatly improved compared to the bimetallic cylinder liner, and the service life of the cylinder liner is extended.

[0074] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A laser cladding machine, characterized in that: include A machine tool body (1), wherein a chuck and a slide assembly are arranged on the machine tool plate; the slide assembly is driven by a transmission screw (11) on the machine tool to perform translation; The chuck clamps one end of the cylinder sleeve, a cladding gun (3) is installed on the slide assembly, and a gun needle of the cladding gun (3) extends into the cylinder sleeve; A coil seat (41), an induction heating coil (42) is arranged on the coil seat (41), the cylinder sleeve is located in the induction heating coil (42), and the coil seat (41) is connected to a transmission screw (11); the transmission screw (11) drives the cladding gun (3) and the induction heating coil (42) to move synchronously longitudinally.

2. The laser cladding machine according to claim 1 is characterized in that: The slide assembly includes A longitudinal sliding seat (21), a transverse sliding seat (22) and an adjusting screw (23), wherein the longitudinal sliding seat (21) is arranged to slide longitudinally on the machine tool body (1), the transmission screw (11) is connected to the longitudinal sliding seat (21), the transverse sliding seat (22) is arranged to slide transversely on the longitudinal sliding seat (21), and the cladding gun (3) is installed on the transverse sliding seat (22); The adjusting screw rod (23) is arranged on the longitudinal sliding seat (21) and connected to the transverse sliding seat (22). The adjusting screw rod (23) is suitable for adjusting the transverse position of the cladding gun (3) on the machine tool.

3. The laser cladding machine according to claim 1 or 2, characterized in that: The powder spraying focal length of the cladding gun (3) is 1.2-1.8 mm.

4. A method for manufacturing a cylinder liner, characterized in that: The laser cladding machine according to claim 3 comprises the following steps: Step S01, selecting a steel pipe and rough turning it into a cylinder liner blank according to size; Step S02, preheating the cylinder liner blank to 340-360° C., and then mounting the cylinder liner blank on a chuck; Step S03, using Ni60WC alloy powder, the inner hole of the cylinder sleeve is processed by the gun needle of the cladding gun (3), and the processing parameters are: The powder spraying focal length is 1.2-1.8 mm, the heating temperature of the induction heating coil (42) is 350° C., the laser power of the cladding gun (3) is 1700 W, the cladding speed is 0.9-1.1 m / min; the single-channel traverse speed is 1.4-1.6 mm; the powder feeding speed is 1.5-2.0 r / min; the protective air flow is 13-15 L / min; and the powder-carrying air flow is 4-6 L / min. During the laser cladding process, the transmission screw (11) drives the induction heating coil (42) and the cladding gun (3) to move synchronously; Step S04, forming a cladding layer (62) on the inner wall of the cylinder liner after the laser cladding process, reducing the inner hole surface roughness to less than Ra0.4μm by internal grinding, grinding and chamfering, and spraying paint on the outer surface to complete the production of the new mud pump cylinder liner.

5. The method for manufacturing a drilling mud pump cylinder sleeve according to claim 4, wherein: In step S02, the cylinder liner blank is preheated to 500°C and then kept warm to 340-360°C.

6. A cylinder liner, characterized in that: include A cylinder liner base (61), wherein an inner hole of the cylinder liner base (61) is provided with a cladding layer (62); The cladding layer (62) is manufactured by the method for manufacturing a drilling mud pump cylinder liner according to claim 4.