Method for extracting CuTi2 phase

Through multiple soaking and washing steps, the Cu-Ti alloy was corroded with a specific acid solution, and the problem of difficulty in extracting CuTi2 phase in Cu-Ti alloy was successfully overcome, and the accurate three-dimensional morphology analysis and growth behavior research of CuTi2 phase was realized. The error problem of the two-dimensional observation method in the prior art was solved.

CN119020788AActive Publication Date: 2024-11-26NORTHEASTERN UNIV CHINA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411438887.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-26
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The prior art is difficult to extract CuTi2 phases separately in Cu-Ti alloys, and there are uncontrollable errors in the two-dimensional tissue observation method, so it is impossible to accurately analyze its growth behavior and three-dimensional dimensions.

Method used

Using multiple soaking and washing steps, the Cu-Ti alloy is corroded with an acid solution composed of hydrofluoric acid, nitric acid and hydrochloric acid. The CuTi2 phase is obtained by ultrasonic washing and filter paper filtration, overcoming the limitations of two-dimensional observation and achieving three-dimensional morphology. analyze.

Benefits of technology

The CuTi2 phase was successfully extracted and its growth behavior and three-dimensional dimensions were accurately analyzed, which solved the problem of the similar corrosion properties of CuTi phase and CuTi2 phase in most corrosion fluids, and simplified the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020788A_ABST
    Figure CN119020788A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgy, in particular to a method for extracting a CuTi2 phase. The extraction method of the CuTi2 phase comprises the following steps: (a) immersing a Cu-Ti alloy comprising a CuTi phase and a CuTi2 phase in an acid solution, reacting for 2-4 hours, and washing; (b) immersing the washed Cu-Ti alloy into the acid liquor, reacting for 2-4 hours, and then washing; (c) repeating the step (b) for at least four times; the acid liquor is prepared by mixing the following components in parts by mass: 0.5-2 parts of hydrofluoric acid with the mass fraction of 40%, 2-5 parts of nitric acid with the mass fraction of 68%, 1-3 parts of hydrochloric acid with the mass fraction of 37% and 90-98 parts of water. The method can be used for extracting the CuTi2 phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metallurgy, and in particular to a CuTi 2 Phase extraction method. Background Art

[0002] Cu-Ti alloys exhibit good wear resistance, excellent antibacterial and corrosion resistance, and have broad application potential in the biomedical field. 2 Phase and eutectic structure (CuTi+CuTi 2 ) composition. Among them, CuTi 2 The CuTi phase exhibits high hard-brittle behavior and usually acts as a fine second phase to improve the strength and wear resistance of the alloy. 2 The phase appears in the material in the form of coarse grains, which will produce cracks and expand under continuous stress, leading to material fracture. 2 The microstructure of CuTi has a direct impact on its performance, including grain size, growth behavior, growth mechanism, etc. 2 This information is crucial for further optimizing the properties of Cu-Ti alloys. The commonly used method to characterize the grain size is to count and average the grain size on a two-dimensional plane. 2 The spatial morphology of a cell is not completely symmetrical in every spatial direction, so this two-dimensional statistical method will have uncontrollable errors. In addition, the growth behavior and growth mechanism will also be limited by the surrounding tissues and cannot be fully revealed.

[0003] In view of this, CuTi 2 The three-dimensional morphology of CuTi can be obtained more accurately 2 The spatial size, growth behavior, and growth mechanism of CuTi can be directly controlled by the preparation parameters. 2 It is of great significance to obtain a Cu-Ti alloy that meets specific functional and performance requirements and save subsequent processing costs.

[0004] In the prior art, sulfuric acid, hydrogen peroxide solution, and ferric chloride solution are used to corrode the Cu solid solution in the Cu-Ti alloy, retaining the Cu-Ti intermetallic compound. Alternatively, a mixed solution of nitric acid and hydrofluoric acid is used to corrode the Ti solid solution in the Cu-Ti alloy, retaining the Cu-Ti intermetallic compound. The key to the success of the above corrosion is that there is a significant difference in the corrosion properties of the Cu solid solution (or Ti solid solution) and the Cu-Ti intermetallic compound. The corrosive liquid can corrode very quickly in the Cu solid solution (or Ti solid solution), but reacts very slowly or almost not at all with the Cu-Ti intermetallic compound. However, the corrosion properties of the Cu-Ti intermetallic compounds are not much different. Therefore, it is difficult to extract a single Cu-Ti intermetallic compound from a Cu-Ti alloy composed of multiple compounds. The prior art has not reported a method for extracting a compound from an alloy composed of multiple Cu-Ti intermetallic compounds.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a CuTi 2 phase extraction method, which can extract CuTi 2 phase, overcoming the limitations of two-dimensional organization observation and realizing the analysis of CuTi 2 Growth behavior, growth mechanism and quantitative three-dimensional size.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] The present invention provides a CuTi 2 The extraction method of the phase comprises the following steps:

[0009] (a) The phase composition includes CuTi phase and CuTi 2 The Cu-Ti alloy of the phase is immersed in an acid solution, reacted for 2 to 4 hours, and then washed;

[0010] (b), immersing the washed Cu-Ti alloy in the acid solution and reacting for 2 to 4 hours,

[0011] washing;

[0012] (c) Repeat step (b) at least 4 times;

[0013] The acid solution is prepared by mixing the following components by mass: 0.5 to 2 parts of hydrofluoric acid with a mass fraction of 40%, 2 to 5 parts of nitric acid with a mass fraction of 68%, 1 to 3 parts of hydrochloric acid with a mass fraction of 37%, and 90 to 98 parts of water.

[0014] Furthermore, the acid solution is prepared by mixing the following components by mass: 0.6-1.7 parts of hydrofluoric acid with a mass fraction of 40%, 2.8-4.2 parts of nitric acid with a mass fraction of 68%, 1.2-2.4 parts of hydrochloric acid with a mass fraction of 37%, and 91.7-95.4 parts of water.

[0015] Furthermore, a drying step is included after each washing.

[0016] Furthermore, the washing method includes ultrasonic water washing.

[0017] Furthermore, each washing time is 10 to 60 minutes.

[0018] Furthermore, after the last washing, the water washing liquid is filtered using filter paper with a pore size of 10 to 15 μm to obtain a filtrate.

[0019] Furthermore, after the filtration, the method further includes a step of drying the filtrate.

[0020] Furthermore, the Cu-Ti alloy consists of 39.85% to 55.06% Cu and 44.94% to 60.15% Ti in terms of mass percentage.

[0021] Furthermore, in step (a), before being immersed in the acid solution, the Cu-Ti alloy is ground and polished.

[0022] Furthermore, the grinding method includes: grinding the Cu-Ti alloy using 400-mesh sandpaper, 800-mesh sandpaper, 1200-mesh sandpaper, 1500-mesh sandpaper and 2000-mesh sandpaper in sequence; the polishing method includes: polishing using diamond polishing paste.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The extraction method provided by the present invention can extract CuTi 2 phase, or CuTi 2 Intermetallic compounds overcome the limitations of two-dimensional structure observation and realize the observation and analysis of CuTi 2 Growth behavior, growth mechanism and quantitative three-dimensional size.

[0025] (2) CuTi provided by the present invention 2 The extraction method of CuTi phase is simple to operate and solves the problem of CuTi phase and CuTi 2 The problem is that the phases in most corrosive solutions have similar corrosive properties and cannot be extracted separately. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The CuTi obtained in Example 1 provided by the present invention 2 SEM images of the phase;

[0028] Figure 2 The CuTi obtained in Example 2 provided by the present invention 2 SEM images of the phase;

[0029] Figure 3 The CuTi obtained in Example 3 provided by the present invention 2 SEM images of the phase;

[0030] Figure 4 This is a scanning electron microscope image of the alloy obtained in Comparative Example 1 provided by the present invention;

[0031] Figure 5 This is a scanning electron microscope image of the alloy obtained in Comparative Example 2 provided by the present invention;

[0032] Figure 6 This is a scanning electron microscope image of the alloy obtained in Comparative Example 3 provided by the present invention;

[0033] Figure 7 This is a scanning electron microscope image of the alloy obtained in Comparative Example 4 provided by the present invention;

[0034] Figure 8 This is a scanning electron microscope image of the alloy obtained in Comparative Example 5 provided by the present invention. DETAILED DESCRIPTION

[0035] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0037] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0038] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0039] The present invention provides a CuTi 2 Phase extraction method, namely a CuTi 2 Three-dimensional morphology extraction method, in which CuTi 2 Phase is primary CuTi in Cu-Ti alloy 2 Phase, the extraction method comprises the following steps:

[0040] (a) The phase composition includes CuTi phase and CuTi 2 The Cu-Ti alloy of the phase is immersed in an acid solution, reacted for 2 to 4 hours, and then washed. The reaction time in step (a) includes but is not limited to any one of 2 hours, 2.5 hours, 3 hours, 3.5 hours, and 4 hours or any range between two of them. Immersing means soaking in an acid solution.

[0041] (b), immersing the washed Cu-Ti alloy in an acid solution, reacting for 2 to 4 hours, and then washing. The time for each reaction in step (b) includes but is not limited to any point value of 2 hours, 2.5 hours, 3 hours, 3.5 hours, and 4 hours or a range value between any two of them. It is understood that during the second and subsequent immersion processes, there is no need to replace the acid solution, and the acid solution used for the first immersion can continue to be used.

[0042] (c), repeating step (b) at least 4 times. Wherein, step (b) is repeated at least 4 times, for example, 5 times, 6 times, 7 times, 8 times.

[0043] The acid solution is prepared by mixing the following components by mass: 0.5 to 2 parts of hydrofluoric acid with a mass fraction of 40%, 2 to 5 parts of nitric acid with a mass fraction of 68%, 1 to 3 parts of hydrochloric acid with a mass fraction of 37%, and 90 to 98 parts of water. Wherein, the mass fraction of hydrofluoric acid includes but is not limited to any one of 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.3 parts, 1.5 parts, 1.8 parts, 2 parts or any range between two of them; the mass fraction of nitric acid includes but is not limited to any one of 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or any range between two of them; the mass fraction of hydrochloric acid includes but is not limited to any one of 1 part, 1.2 parts, 1.3 parts, 1.5 parts, 1.8 parts, 2 parts, 2.3 parts, 2.5 parts, 2.8 parts, 3 parts or any range between two of them; the mass fraction of water includes any one of 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts, 98 parts or any range between two of them.

[0044] In the above acid solution, CuTi in Cu-Ti alloy 2 The CuTi phase has strong corrosion resistance and hardly reacts with the acid solution within 2 to 4 hours, while the CuTi phase has poor corrosion resistance in the acid solution and will be corroded in large quantities after being immersed in the corrosive solution for 2 hours. 2 It will be completely exposed due to the corrosion of the surrounding CuTi.

[0045] The purpose of washing after each acid immersion is to remove the corrosion products on the surface of the Cu-Ti alloy. Because the corrosion products produced after a period of reaction will cover the entire surface of the Cu-Ti alloy, it can no longer directly contact the acid solution, resulting in the interruption of the reaction, so the washing, reaction, and washing process needs to be repeated many times.

[0046] The material obtained after multiple corrosion reactions was observed under a scanning electron microscope and was a single CuTi 2 phase, or CuTi 2 Compound.

[0047] Extraction of CuTi provided by the present invention 2 The method of phase analysis overcomes the limitation of two-dimensional organization observation and realizes the analysis of CuTi 2 Growth behavior, growth mechanism and quantitative three-dimensional size.

[0048] The CuTi provided by the present invention 2 The extraction method of CuTi phase is simple to operate and solves the problem of CuTi phase and CuTi 2 The problem is that the phases in most corrosive solutions have similar corrosive properties and cannot be extracted separately.

[0049] In some specific embodiments, in order to further improve the extraction efficiency, the acid solution is prepared by mixing the following components in parts by mass: 0.6 to 1.7 parts of hydrofluoric acid with a mass fraction of 40%, 2.8 to 4.2 parts of nitric acid with a mass fraction of 68%, 1.2 to 2.4 parts of hydrochloric acid with a mass fraction of 37%, and 91.7 to 95.4 parts of water.

[0050] In some specific embodiments, the water comprises deionized water.

[0051] In some specific embodiments, a drying step is further included after each washing step. Drying can prevent residual water or other detergents on the surface of the Cu-Ti alloy from entering the acid solution and causing changes in the acid solution concentration.

[0052] In some specific embodiments, after each washing, filtering and drying are performed in sequence.

[0053] In some specific embodiments, each washing method includes ultrasonic washing, that is, ultrasonic cleaning using deionized water.

[0054] In some specific embodiments, the washing time each time is 10 to 60 minutes, including but not limited to any one of 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, and 60 minutes, or a range between any two of them.

[0055] In some specific embodiments, after the last washing, the water washing liquid obtained after the last washing is filtered using filter paper with a pore size of 10 to 15 μm to obtain a filtrate. The filtrate contains CuTi 2 Mutually.

[0056] It can be understood that the above-mentioned filter paper with a pore size of 10 to 15 μm refers to a filter paper with a pore size specification of 10 to 15 μm.

[0057] In some specific embodiments, the filtration further comprises a step of drying the filtrate to obtain CuTi 2 The drying temperature may be any commonly used drying temperature, for example, 80 to 100° C., but is not limited thereto.

[0058] In some specific embodiments, the Cu-Ti alloy is composed of 39.85% to 55.06% of Cu element and 44.94% to 60.15% of Ti element in terms of mass percentage. The mass percentage of the Cu element includes but is not limited to any point value of 39.85%, 40%, 43%, 45%, 48%, 50%, 53%, 55.06% or any range value between the two; the mass percentage of the Ti element includes but is not limited to any point value of 44.94%, 45%, 48%, 50%, 53%, 55%, 58%, 60%, 60.15% or any range value between the two. It is understood that the sum of the mass percentages of the Cu element and the Ti element is 100%.

[0059] In some specific embodiments, in step (a), before immersing in the acid solution, the Cu-Ti alloy is ground and polished. The grinding and polishing can remove the oxide scale produced by processing, ensure that the sample used is a Cu-Ti alloy, and ensure that the CuTi 2 Smooth extraction of phase and improved extraction efficiency.

[0060] In some specific implementations, the grinding method includes: grinding the Cu-Ti alloy using 400-mesh sandpaper, 800-mesh sandpaper, 1200-mesh sandpaper, 1500-mesh sandpaper and 2000-mesh sandpaper in sequence.

[0061] In some specific implementations, the polishing method includes: polishing with diamond polishing paste.

[0062] In some specific embodiments, in step (a), the Cu-Ti alloy comprises a block Cu-Ti alloy having a length, a width, and a height of 4 to 6 mm, 4 to 6 mm, and 2 to 4 mm, respectively, and CuTi 2 The extraction of the phase is preferably a cubic Cu-Ti alloy. That is, the shape of the Cu-Ti alloy includes a cubic shape, such as a cuboid. However, it is not limited thereto, and other shapes of Cu-Ti alloys may also be used.

[0063] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0064] Example 1

[0065] The CuTi provided in this embodiment 2 The extraction method of the phase comprises the following steps:

[0066] (1) A cubic Cu-Ti alloy with a length × width × height of 5 mm × 5 mm × 3 mm is prepared. The Cu-Ti alloy is composed of 54% Cu and 46% Ti by mass. The Cu-Ti alloy includes a CuTi phase and a CuTi phase. 2 Each surface of the Cu-Ti alloy was polished with 400-grit sandpaper, 800-grit sandpaper, 1200-grit sandpaper, 1500-grit sandpaper and 2000-grit sandpaper in sequence, polished with 0.25 μm diamond polishing paste, and then ultrasonically cleaned with deionized water and dried.

[0067] (2) The polished Cu-Ti alloy obtained in step (1) is immersed in an acid solution, wherein the acid solution is prepared by mixing the following components by mass: 1.2 parts of hydrofluoric acid with a mass fraction of 40%, 3.5 parts of nitric acid with a mass fraction of 68%, 1.8 parts of hydrochloric acid with a mass fraction of 37%, and 93.5 parts of deionized water. After immersion and reaction for 2 hours, the Cu-Ti alloy is removed and ultrasonically cleaned with deionized water for 10 minutes to remove corrosion products on the surface of the metal block, and then dried.

[0068] (3) The dried Cu-Ti alloy obtained in step (2) is further immersed in an acid solution, reacted for 2 hours, taken out, ultrasonically cleaned with deionized water for 10 minutes and dried; the soaking-ultrasonic water washing-drying steps are repeated 4 times, and after the last water washing, the water washing liquid is filtered using a filter paper with a pore size of 10 to 15 μm to obtain a filtrate, and then the filtrate is dried to obtain CuTi 2 Phase. 2 Phase was observed under scanning electron microscope, such as Figure 1 As shown, it can be seen that the CuTi 2 phase, and its three-dimensional morphology can be observed.

[0069] Example 2

[0070] The CuTi provided in this embodiment 2 The extraction method of the phase comprises the following steps:

[0071] (1) A cubic Cu-Ti alloy with a length × width × height of 5 mm × 5 mm × 3 mm is prepared. The Cu-Ti alloy is composed of 54% Cu and 46% Ti by mass. The Cu-Ti alloy includes a CuTi phase and a CuTi phase. 2 Each surface of the Cu-Ti alloy was polished with 400-grit sandpaper, 800-grit sandpaper, 1200-grit sandpaper, 1500-grit sandpaper and 2000-grit sandpaper in sequence, polished with 0.25 μm diamond polishing paste, and then ultrasonically cleaned with deionized water and dried.

[0072] (2) The polished Cu-Ti alloy obtained in step (1) is immersed in an acid solution, wherein the acid solution is prepared by mixing the following components by mass: 1.7 parts of hydrofluoric acid with a mass fraction of 40%, 4.2 parts of nitric acid with a mass fraction of 68%, 2.4 parts of hydrochloric acid with a mass fraction of 37%, and 91.7 parts of deionized water. After immersion and reaction for 2 hours, the Cu-Ti alloy is removed and ultrasonically cleaned with deionized water for 10 minutes to remove corrosion products on the surface of the metal block, and then dried.

[0073] (3) The dried Cu-Ti alloy obtained in step (2) is further immersed in an acid solution, reacted for 2 hours, taken out, ultrasonically cleaned with deionized water for 10 minutes and dried; the soaking-ultrasonic water washing-drying steps are repeated 4 times, and after the last water washing, the water washing liquid is filtered using a filter paper with a pore size of 10 to 15 μm to obtain a filtrate, and then the filtrate is dried to obtain CuTi 2 Phase. 2 Phase was observed under scanning electron microscope, such as Figure 2 As shown, it can be seen that the CuTi 2 phase, and its three-dimensional morphology can be observed.

[0074] Example 3

[0075] The CuTi provided in this embodiment 2 The extraction method of the phase comprises the following steps:

[0076] (1) A cubic Cu-Ti alloy with a length × width × height of 5 mm × 5 mm × 3 mm is prepared. The Cu-Ti alloy is composed of 52.5% Cu and 47.5% Ti by mass. The Cu-Ti alloy includes a CuTi phase and a CuTi 2 Each surface of the Cu-Ti alloy was polished with 400-grit sandpaper, 800-grit sandpaper, 1200-grit sandpaper, 1500-grit sandpaper and 2000-grit sandpaper in sequence, polished with 0.25 μm diamond polishing paste, and then ultrasonically cleaned with deionized water and dried.

[0077] (2) The polished Cu-Ti alloy obtained in step (1) is immersed in an acid solution, wherein the acid solution is prepared by mixing the following components by mass: 0.6 parts of hydrofluoric acid with a mass fraction of 40%, 2.8 parts of nitric acid with a mass fraction of 68%, 1.2 parts of hydrochloric acid with a mass fraction of 37%, and 95.4 parts of deionized water. After immersion and reaction for 2 hours, the Cu-Ti alloy is removed and ultrasonically cleaned with deionized water for 10 minutes to remove corrosion products on the surface of the metal block, and then dried.

[0078] (3) The dried Cu-Ti alloy obtained in step (2) is further immersed in an acid solution, reacted for 2 hours, taken out, ultrasonically cleaned with deionized water for 20 minutes and dried; the soaking-ultrasonic water washing-drying steps are repeated 4 times, and after the last water washing, the water washing liquid is filtered using a filter paper with a pore size of 10 to 15 μm to obtain a filtrate, and then the filtrate is dried to obtain CuTi 2 Phase. 2 Phase was observed under scanning electron microscope, such as Figure 3 As shown, it can be seen that the CuTi 2 phase, and its three-dimensional morphology can be observed.

[0079] Example 4

[0080] The CuTi provided in this embodiment 2 The extraction method of the phase is basically the same as that of Example 1, except that the chemical composition of the Cu-Ti alloy used in step (1) is different. The Cu-Ti alloy used in this example consists of 52% Cu and 48% Ti by mass.

[0081] Example 5

[0082] The CuTi provided in this embodiment 2 The extraction method of the phase is basically the same as that of Example 1, except that in step (3), the steps of immersion-ultrasonic water washing-drying are repeated 5 times.

[0083] Example 6

[0084] The CuTi provided in this embodiment 2 The extraction method of the phase is basically the same as that of Example 1, except that the soaking time is 4 h each time, that is, the reaction time is 4 h each time.

[0085] Comparative Example 1

[0086] The CuTi provided in this comparative example 2 The extraction method of the phase is basically the same as that of Example 1, except that the hydrofluoric acid in the acid solution is replaced by an equal mass of nitric acid, that is, the acid solution is prepared by mixing the following components by mass: 4.7 parts of nitric acid with a mass fraction of 68%, 1.8 parts of hydrochloric acid with a mass fraction of 37%, and 93.5 parts of deionized water.

[0087] The scanning electron microscope image of the alloy finally obtained in this comparative example is as follows Figure 4 As shown in the figure, it can be seen that the corrosion resistance of the Cu-Ti alloy in the acid solution of this comparative example is good. Only a small amount of corrosion pits appear on the surface of the Cu-Ti alloy, and no large amount of CuTi phase is corroded. Therefore, it is impossible to extract CuTi 2 Mutually.

[0088] Comparative Example 2

[0089] The CuTi provided in this comparative example 2 The extraction method of the phase is basically the same as that of Example 1, except that the nitric acid in the acid solution is replaced by an equal mass of hydrochloric acid, that is, the acid solution is prepared by mixing the following components by mass: 1.2 parts of hydrofluoric acid with a mass fraction of 40%, 5.3 parts of hydrochloric acid with a mass fraction of 37%, and 93.5 parts of deionized water.

[0090] The scanning electron microscope image of the alloy finally obtained in this comparative example is as follows Figure 5 As shown in the figure, it can be seen that the corrosiveness of the etching solution is not enough to completely remove the CuTi phase. 2 The CuTi phase is still surrounded by a mixture of unreacted CuTi phase and corrosion products, so it is impossible to extract the single CuTi phase. 2 Mutually.

[0091] Comparative Example 3

[0092] The CuTi provided in this comparative example 2 The extraction method of the phase is basically the same as that of Example 1, except that the hydrochloric acid in the acid solution is replaced by an equal mass of hydrofluoric acid, that is, the acid solution is prepared by mixing the following components by mass: 3 parts of hydrofluoric acid with a mass fraction of 40%, 3.5 parts of nitric acid with a mass fraction of 68%, and 93.5 parts of deionized water.

[0093] The scanning electron microscope image of the alloy finally obtained in this comparative example is as follows Figure 6 As shown in the figure, it can be seen that the corrosion resistance of the Cu-Ti alloy in the acid solution of this comparative example is good, and only a small amount of corrosion pits appear on the surface of the Cu-Ti alloy, and the CuTi phase and CuTi 2 Differential corrosion of phases, unable to obtain separate CuTi 2 Mutually.

[0094] Comparative Example 4

[0095] The CuTi provided in this comparative example 2 The extraction method of the phase is basically the same as that of Example 1, except that the acid solution is prepared by mixing the following components by mass: 5 parts of hydrofluoric acid with a mass fraction of 40%, 8 parts of nitric acid with a mass fraction of 68%, 5 parts of hydrochloric acid with a mass fraction of 37%, and 82 parts of deionized water. The scanning electron microscope image of the alloy finally obtained in this comparative example is as follows Figure 7 As shown in the figure, it can be seen that due to the excessive acid concentration, the CuTi that was originally able to resist corrosion 2 The phase also begins to be corroded, losing the effect of selective corrosion.

[0096] Comparative Example 5

[0097] The CuTi provided in this comparative example 2 The extraction method of the phase is basically the same as that of Example 1, except that the soaking time is 8 h each time, that is, the reaction time is 8 h each time.

[0098] The scanning electron microscope image of the alloy finally obtained in this comparative example is as follows Figure 8 As shown in the figure, it can be seen that due to the long corrosion time, more corrosion products are produced, and these products accumulate on the surface of the alloy and affect the subsequent corrosion. The large amount of corrosion products formed may be due to the secondary corrosion, which produces more water-insoluble corrosion products that cannot be washed away, so it is impossible to obtain a separate CuTi 2 Mutually.

[0099] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A CuTi 2 Phase extraction method, It is characterized in that The steps include: (a) The phase composition includes CuTi phase and CuTi 2 The Cu-Ti alloy of the phase is immersed in an acid solution, reacted for 2 to 4 hours, and then washed; (b), immersing the washed Cu-Ti alloy in the acid solution, reacting for 2 to 4 hours, and then washing; (c) Repeat step (b) at least 4 times; The acid solution is prepared by mixing the following components by mass: 0.5 to 2 parts of hydrofluoric acid with a mass fraction of 40%, 2 to 5 parts of nitric acid with a mass fraction of 68%, 1 to 3 parts of hydrochloric acid with a mass fraction of 37%, and 90 to 98 parts of water.

2. CuTi according to claim 1 2 Phase extraction method, It is characterized in that The acid solution is prepared by mixing the following components by mass: 0.6-1.7 parts of hydrofluoric acid with a mass fraction of 40%, 2.8-4.2 parts of nitric acid with a mass fraction of 68%, 1.2-2.4 parts of hydrochloric acid with a mass fraction of 37%, and 91.7-95.4 parts of water.

3. CuTi according to claim 1 2 Phase extraction method, It is characterized in that Each washing step is followed by a drying step.

4. CuTi according to claim 1 2 Phase extraction method, It is characterized in that The washing method includes ultrasonic water washing.

5. CuTi according to claim 1 2 Phase extraction method, It is characterized in that The washing time each time is 10 to 60 minutes.

6. CuTi according to claim 1 2 Phase extraction method, It is characterized in that After the last washing, the water washing liquid is filtered using filter paper with a pore size of 10 to 15 μm to obtain a filtrate.

7. CuTi according to claim 6 2 Phase extraction method, It is characterized in that After the filtration, the method further comprises the step of drying the filtrate.

8. CuTi according to claim 1 2 Phase extraction method, It is characterized in that The Cu-Ti alloy consists of 39.85% to 55.06% of Cu and 44.94% to 60.15% of Ti in terms of mass percentage.

9. CuTi according to claim 1 2 Phase extraction method, It is characterized in that In step (a), before being immersed in the acid solution, the Cu-Ti alloy is ground and polished.

10. CuTi according to claim 9 2 Phase extraction method, It is characterized in that The grinding method comprises: grinding the Cu-Ti alloy with 400-mesh sandpaper, 800-mesh sandpaper, 1200-mesh sandpaper, 1500-mesh sandpaper and 2000-mesh sandpaper in sequence; The polishing method comprises: performing polishing using diamond polishing paste.

Citation Information

Patent Citations

  • Titanium-copper for electronic component

    CN102686755A

  • Copper-titanium corrosive liquid for integrated circuit and production process of copper-titanium corrosive liquid

    CN113564598A

  • Metallographic etching reagent

    CN1167839A

  • Near-atomic-ratio nickel-titanium alloy pipe metallographic etchant and corrosion method

    CN118547289A

  • Method of etching a ti-nb-x based titanium alloy

    KR1020130026159A