Electrode and preparation method and application thereof
By forming a nickel transition layer on the electrode substrate and covering the porous active layer, the problem of low electrode activity during the electrolysis of water hydrogen production is solved, the stability and specific surface area of the electrode are improved, and efficient hydrogen and oxygen generation is achieved.
Patent Information
- Application Number
- CN202411514029.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the existing process of electrolytic hydrogen production, the hydrogen evolution electrode and oxygen evolution electrode have low activity, resulting in poor performance and hydrogen production efficiency of electrolytic cells. The active materials are prone to fall off under high current density, affecting long-term safe operation.
An electrode is used to form a nickel transition layer on the substrate and cover the porous active layer. The porous active layer material is a nickel-based alloy or a cobalt-based alloy, including zinc. The nanosheet stacking structure is formed by electroplating and zinc fading treatment to improve the specific surface area and binding force.
It significantly improves hydrogen and oxygen evolution activities, enhances the stability and binding force of the electrode, reduces the overpotential, and is suitable for high current density conditions, avoids the fall of active materials, and improves the long-term operating performance of the electrode.
Smart Images

Figure CN119020815A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials, and in particular to an electrode and a preparation method and application thereof. Background Art
[0002] Hydrogen energy has broad application prospects due to its advantages such as stable power generation, high combustion calorific value and no pollution. Hydrogen production by water electrolysis is considered to be the most promising method of hydrogen production due to its high yield and high product purity. Hydrogen production by water electrolysis includes two half reactions: hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). Among them, hydrogen evolution reaction is a two-electron reaction and oxygen evolution reaction is a four-electron reaction.
[0003] In the process of hydrogen production by electrolysis of water, electrode materials, as the core components of the electrolyzer, are key materials that affect the performance of the electrolyzer and the effect of hydrogen production by electrolysis of water. Alkaline electrolyzers are usually used in the process of hydrogen production by electrolysis of water. 3 / h) Nickel mesh is often used as hydrogen evolution electrode and oxygen evolution electrode in alkaline electrolytic cells, but the hydrogen evolution activity and oxygen evolution activity still need to be improved. Summary of the invention
[0004] The object of the present invention is to provide an electrode and a preparation method and application thereof. The electrode provided by the present invention has high activity for producing hydrogen by electrolysis of water, wherein the electrode (the material of the porous active layer is a nickel-based alloy) has high hydrogen evolution activity when used as a hydrogen evolution electrode, and the electrode (the material of the porous active layer is a cobalt-based alloy) has high oxygen evolution activity when used as an oxygen evolution electrode.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides an electrode, comprising a substrate, a nickel transition layer coated on the surface of the substrate, and a porous active layer coated on the surface of the nickel transition layer, wherein the material of the porous active layer is a nickel-based alloy or a cobalt-based alloy, and the alloy elements in the nickel-based alloy and the cobalt-based alloy include zinc.
[0006] Preferably, the electrode is a hydrogen evolution electrode or an oxygen evolution electrode; When the electrode is a hydrogen evolution electrode, the material of the porous active layer is a nickel-based alloy; When the electrode is an oxygen evolution electrode, the material of the porous active layer is a cobalt-based alloy.
[0007] Preferably, the thickness of the porous active layer is 1-50 μm, and the atomic percentage of zinc in the porous active layer is ≤20%; and the porous active layer is formed by stacking nanosheets.
[0008] Preferably, the thickness of the nickel transition layer is 0.2-2 μm.
[0009] Preferably, the substrate is a metal substrate.
[0010] The present invention provides a method for preparing the electrode described in the above technical solution, comprising the following steps: Placing the substrate in a first plating solution for pre-electroplating to form a nickel transition layer on the surface of the substrate to obtain a pre-plated substrate; the first plating solution contains a nickel salt; Placing the pre-plated substrate in a second plating solution for electroplating to form an active layer on the surface of the pre-plated substrate to obtain an electroplated substrate; the second plating solution contains a nickel salt and a zinc salt, or the second plating solution contains a cobalt salt and a zinc salt; The electroplated substrate is subjected to a zinc stripping treatment to remove a portion of zinc in the active layer and to form a porous structure in the active layer, thereby obtaining the electrode.
[0011] Preferably, the pre-plating treatment conditions include: the plating solution temperature is 25-60°C, the pH value is 1-6, and the current density is 0.1-10A / dm 2 , time is 1~30min; The electroplating treatment conditions include: the plating solution temperature is 25-55°C, the pH value is 1-10, and the current density is 0.1-10A / dm 2 , time is 1~300min.
[0012] Preferably, a heat treatment is further included between the electroplating treatment and the zinc stripping treatment; the temperature of the heat treatment is 100-400° C., and the holding time is 0.5-4 hours; and the heat treatment is carried out in an atmosphere containing oxygen.
[0013] The present invention provides the application of the electrode described in the above technical solution or the electrode prepared by the preparation method described in the above technical solution in hydrogen production by electrolysis of water.
[0014] Preferably, when the material of the porous active layer is a nickel-based alloy, the electrode is used as a hydrogen evolution electrode for electrolyzing water to produce hydrogen; when the material of the porous active layer is a cobalt-based alloy, the electrode is used as an oxygen evolution electrode for electrolyzing water to produce hydrogen.
[0015] Beneficial effects: The electrode provided by the present invention comprises a substrate, a nickel transition layer coated on the surface of the substrate, and a porous active layer coated on the surface of the nickel transition layer, wherein the material of the porous active layer is a nickel-based alloy or a cobalt-based alloy, and the alloying elements in the nickel-based alloy and the cobalt-based alloy include zinc. The electrode provided by the present invention has high activity for producing hydrogen by electrolysis of water, wherein the electrode (the material of the porous active layer is a nickel-based alloy) has high hydrogen evolution activity when used as a hydrogen evolution electrode, and the electrode (the material of the porous active layer is a cobalt-based alloy) has high oxygen evolution activity when used as an oxygen evolution electrode. Specifically, the porous active layer in the present invention has a large specific surface area, thereby providing a large number of active sites, which is conducive to improving the activity; at the same time, in the process of producing hydrogen and gas by electrolysis of water, the large specific surface area increases the gas escape velocity, which is also conducive to further improving the activity.
[0016] Furthermore, the electrode provided by the present invention has the characteristics of high stability and high binding force when used in hydrogen production by electrolysis of water, which is conducive to large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The SEM image of the hydrogen evolution electrode prepared in Example 2; Figure 2 The long-term stability test results of the hydrogen evolution electrodes prepared in Example 1 and Example 2 are shown; Figure 3 This is a graph showing the long-term stability test results of the hydrogen evolution electrode prepared in Example 2 and a commercial nickel mesh; Figure 4 This is a graph showing the test results of the binding strength of the hydrogen evolution electrode prepared in Example 3 and the binding strength of Raney nickel. DETAILED DESCRIPTION
[0018] The present invention provides an electrode, comprising a substrate, a nickel transition layer coated on the surface of the substrate, and a porous active layer coated on the surface of the nickel transition layer, wherein the material of the porous active layer is a nickel-based alloy or a cobalt-based alloy, and the alloy elements in the nickel-based alloy and the cobalt-based alloy include zinc.
[0019] The electrode of the present invention includes a substrate. In an embodiment of the present invention, the substrate may be a metal substrate; the material of the metal substrate may include nickel or nickel-chromium alloy, for example, the metal substrate may specifically be a nickel mesh, nickel foam, nickel plate, nickel-chromium alloy mesh or nickel-chromium alloy plate; wherein the specification of the nickel mesh may specifically be: the mesh number is 25 to 46 meshes, for example, it may be 25 meshes, 30 meshes, 40 meshes or 46 meshes; the wire diameter is 0.19 to 0.3 μm, for example, it may be 0.19 μm, 0.25 μm or 0.3 μm.
[0020] The electrode of the present invention includes a nickel transition layer coated on the surface of the substrate. In an embodiment of the present invention, the thickness of the nickel transition layer can be 0.2-2 μm, specifically 0.2 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.2 μm, 1.5 μm or 2 μm. The nickel transition layer is arranged on the surface of the substrate, which can increase the specific surface area and is conducive to improving the bonding force between the porous active layer and the substrate.
[0021] The electrode of the present invention includes a porous active layer coated on the surface of the nickel transition layer, and the material of the porous active layer is a nickel-based alloy or a cobalt-based alloy, and the alloying elements in the nickel-based alloy and the cobalt-based alloy include zinc. In an embodiment of the present invention, the atomic percentage of zinc in the porous active layer can be ≤20%, further can be 3~18%, specifically can be 5%, 6%, 8%, 10%, 12%, 15%, 16% or 18%. In an embodiment of the present invention, the thickness of the porous active layer can be 1~50μm, further can be 3~25μm, specifically can be 2.5μm, 5μm, 5.5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm or 15μm. In an embodiment of the present invention, the porous active layer is specifically formed by stacking nanosheets (i.e., nickel-based alloy nanosheets or cobalt-based alloy nanosheets).
[0022] The present invention provides a method for preparing the electrode described in the above technical solution, comprising the following steps: Placing the substrate in a first plating solution for pre-electroplating to form a nickel transition layer on the surface of the substrate to obtain a pre-plated substrate; the first plating solution contains a nickel salt; Placing the pre-plated substrate in a second plating solution for electroplating to form an active layer on the surface of the pre-plated substrate to obtain an electroplated substrate; the second plating solution contains a nickel salt and a zinc salt, or the second plating solution contains a cobalt salt and a zinc salt; The electroplated substrate is subjected to a zinc stripping treatment to remove a portion of zinc in the active layer and to form a porous structure in the active layer, thereby obtaining the electrode.
[0023] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0024] The present invention places the substrate in a first plating solution for pre-plating treatment to form a nickel transition layer on the surface of the substrate to obtain a pre-plated substrate. In an embodiment of the present invention, before the pre-plating treatment, the substrate may be subjected to surface pre-treatment, degreasing treatment and acidification treatment in sequence.
[0025] In an embodiment of the present invention, the surface pretreatment method may be sandblasting, and the mesh size of the sand used for the sandblasting may be 100-200 meshes; the present invention has no special limitation on the specific operation method of the sandblasting, and a method familiar to those skilled in the art may be used; sandblasting can increase the specific surface area of the substrate, which is beneficial to improving the bonding strength between the nickel transition layer and the substrate.
[0026] In an embodiment of the present invention, the degreasing treatment may be performed by electrolytic degreasing. Specifically, the sandblasted substrate obtained after the sandblasting treatment may be immersed in a degreasing liquid, with the sandblasted substrate as the anode and the stainless steel plate as the cathode, and a direct current is connected for electrolytic degreasing. In an embodiment of the present invention, the degreasing liquid may be a mixed aqueous solution of sodium hydroxide, sodium carbonate, sodium silicate and trisodium phosphate; the concentration of sodium hydroxide in the degreasing liquid may be 50~100g / L, specifically 70~90g / L; the concentration of sodium carbonate may be 10~40g / L, specifically 20~30g / L; the concentration of sodium silicate may be 5~15g / L, specifically 8~12g / L; the concentration of trisodium phosphate may be 50~100g / L, specifically 70~90g / L. In an embodiment of the present invention, the current density of the direct current may be 1~5A / dm 2 , specifically 1A / dm 2 , 2A / dm 2 、3A / dm 2 , 4A / dm 2 or 5A / dm 2 The electrolytic degreasing time may be 5 to 30 minutes, specifically 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes; organic impurities on the surface of the substrate may be removed by degreasing treatment.
[0027] In an embodiment of the present invention, the acid reagent used for the acid treatment may be hydrochloric acid and / or sulfuric acid; the concentration of the acid reagent may be 10-40wt%, and further may be 20-30wt%; the acid treatment may be performed at room temperature, and the time of the acid treatment may be 10-20min, and specifically may be 15min. In an embodiment of the present invention, the deoiled substrate obtained after the deoiling treatment may be immersed in the acid reagent for the acid treatment; the metal oxide on the surface of the substrate may be removed by the acid treatment, and the substrate may be etched to a certain extent, and the corrosion defect sites are beneficial to improving the bonding strength between the nickel transition layer and the substrate, and improving the quality of the nickel transition layer.
[0028] In the embodiment of the present invention, after the acidification treatment is completed, the obtained acidified substrate is placed in a first plating solution for pre-electroplating treatment to form a nickel transition layer to obtain a pre-plated substrate. In the present invention, the first plating solution contains a nickel salt; in the embodiment of the present invention, the first plating solution also contains an activator and water. In the embodiment of the present invention, the nickel salt can be one or more of nickel chloride, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate and nickel ammonium sulfate, and can be specifically nickel sulfate, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate or nickel ammonium sulfate; the activator can be one or more of sodium chloride, potassium chloride, magnesium chloride and hydrochloric acid, and can be specifically sodium chloride, potassium chloride, magnesium chloride or hydrochloric acid, and can also be a combination of sodium chloride and hydrochloric acid. In an embodiment of the present invention, the concentration of the nickel salt in the first plating solution may be 50-500 g / L, further may be 60-300 g / L, specifically may be 60 g / L, 80 g / L, 100 g / L, 110 g / L, 120 g / L, 140 g / L, 160 g / L, 180 g / L, 200 g / L, 250 g / L, 280 g / L or 300 g / L; the concentration of the activator may be 10-300 g / L, further may be 15-100 g / L, specifically may be 15 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L. In an embodiment of the present invention, the acidified substrate is immersed in a first plating solution, the acidified substrate is used as a cathode, and a soluble anode or an insoluble anode is used to perform a pre-electroplating treatment. In an embodiment of the present invention, the soluble anode may include a nickel mesh or a nickel plate; the insoluble anode may include a titanium plate, a ruthenium-iridium-titanium mesh or a graphite plate. In an embodiment of the present invention, the conditions for the pre-electroplating treatment include: the plating solution temperature may be 25-60°C, specifically 25°C, 30°C, 33°C, 35°C, 40°C, 50°C or 60°C; the pH value may be 1-6, specifically 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6; the current density may be 0.1-10A / dm 2 , further can be 0.3~5A / dm 2 , specifically 0.3A / dm 2 , 0.5A / dm 2 , 1A / dm 2 , 2A / dm 2 , 2.5A / dm 2 、3A / dm 2 , 4A / dm 2 or 5A / dm 2The time may be 1 to 30 minutes, further may be 3 to 25 minutes, specifically may be 3 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes or 25 minutes.
[0029] After obtaining the pre-plated substrate, the present invention places the pre-plated substrate in a second plating solution for electroplating to form an active layer on the surface of the pre-plated substrate to obtain an electroplated substrate. In the present invention, the second plating solution contains a nickel salt and a zinc salt, or the second plating solution contains a cobalt salt and a zinc salt. In an embodiment of the present invention, the second plating solution can be an alkaline plating solution or an acidic plating solution, and the composition of the second plating solution is determined according to the type of metal element in the porous active layer, which is described in detail below.
[0030] In an embodiment of the present invention, when the material of the porous active layer is a nickel-based alloy (i.e., corresponding to the hydrogen evolution electrode), the composition of the alkaline plating solution includes a nickel salt, a zinc salt, an additive and water; the nickel salt may be one or more of nickel chloride, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate and nickel ammonium sulfate, specifically nickel chloride, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate or nickel ammonium sulfate; the zinc salt may be one or more of zinc sulfate, zinc chloride, zinc nitrate and zinc oxide, specifically zinc sulfate, zinc chloride, zinc nitrate or zinc oxide; the additive may be potassium pyrophosphate, pyrophosphate, or potassium pyrophosphate. The invention can be one or more of sodium pyrophosphate, sodium tripolyphosphate, potassium sodium tartrate, ammonium chloride, sodium chloride, magnesium chloride, sodium sulfate, ascorbic acid, sodium dodecyl sulfate, glutamic acid, methionine, proline, tryptophan, serine, tyrosine and glycine, and specifically can be one or more of potassium pyrophosphate, sodium pyrophosphate, potassium sodium tartrate, ammonium chloride, sodium chloride, ascorbic acid, glutamic acid and glycine. For example, potassium pyrophosphate, potassium sodium tartrate, glycine and sodium chloride can be used in combination, potassium pyrophosphate, glutamic acid, sodium chloride and ascorbic acid can be used in combination, and sodium pyrophosphate, glycine and ammonium chloride can be used in combination. In an embodiment of the present invention, the concentration of the nickel salt in the alkaline plating solution may be 20-100 g / L, specifically 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L; the concentration of the zinc salt may be 10-60 g / L, specifically 10 g / L, 20 g / L, 22 g / L, 25 g / L, 30 g / L, 40 g / L, 50 g / L or 60 g / L; the concentration of the additive may be 0.1-500 g / L, further 1-350 g / L, further 50-300 g / L, further 150-250 g / L, for example 177 g / L, 180 g / L or 248 g / L. In an embodiment of the present invention, the pre-plated substrate is immersed in an alkaline plating solution, the pre-plated substrate is used as the cathode, and a soluble anode or an insoluble anode is used for electroplating. The optional types of the soluble anode and the insoluble anode are consistent with the above technical solution and are not repeated here. In an embodiment of the present invention, the conditions for the electroplating treatment include: the plating solution temperature can be 25~55℃, specifically 25℃, 30℃, 35℃, 40℃, 45℃, 50℃ or 55℃; the pH value can be 8~10, specifically 8, 8.5, 9, 9.5 or 10 (in the embodiment of the present invention, ammonia water with a concentration of 30wt% can be used to adjust the pH value); the current density can be 0.1~10A / dm 2 , further can be 1~5A / dm 2 , specifically 1A / dm 2 , 1.5A / dm 2, 2A / dm 2 , 2.5A / dm 2 、3A / dm 2 、3.5A / dm 2 , 4A / dm 2 , 4.5A / dm 2 or 5A / dm 2 The time may be 1 to 300 min, further may be 15 to 120 min, specifically may be 15 min, 30 min, 50 min, 70 min, 90 min or 120 min.
[0031] In an embodiment of the present invention, when the material of the porous active layer is a nickel-based alloy (i.e., corresponding to the hydrogen evolution electrode), the composition of the acidic plating solution includes a nickel salt, a zinc salt and an additive; the nickel salt may be one or more of nickel chloride, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate and nickel ammonium sulfate, specifically nickel chloride, nickel sulfate, nickel fluoroborate, nickel sulfamate, nickel pyrophosphate or nickel ammonium sulfate, or a combination of nickel chloride and nickel sulfate; the zinc salt may be one or more of zinc sulfate, zinc chloride, zinc nitrate and zinc oxide, specifically zinc sulfate, zinc chloride, zinc nitrate or zinc oxide, or a combination of zinc sulfate and zinc chloride. The additive may be one or more of sodium citrate, citric acid, ammonium chloride, sodium chloride, magnesium chloride, potassium sodium tartrate, malic acid, boric acid, ascorbic acid, sodium dodecyl sulfate, tyrosine and glycine, and specifically may be one or more of sodium citrate, potassium sodium tartrate, boric acid, sodium chloride, sodium sulfate, sodium dodecyl sulfate and ascorbic acid, for example, sodium citrate, boric acid, ascorbic acid, sodium chloride, sodium sulfate and sodium dodecyl sulfate may be used in combination, sodium citrate, boric acid, ascorbic acid and sodium dodecyl sulfate may be used in combination, and potassium sodium tartrate, boric acid, ascorbic acid and sodium dodecyl sulfate may be used in combination. In an embodiment of the present invention, the concentration of the nickel salt in the acidic plating solution may be 30-200 g / L, further may be 50-180 g / L, specifically 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L or 180 g / L; the concentration of the zinc salt may be 5-40 g / L, specifically 5 g / L, 10 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L or 180 g / L. / L, 15g / L, 20g / L, 25g / L, 30g / L, 35g / L or 40g / L; the concentration of the additive can be 0.1~200g / L, and further can be 5~100g / L, specifically can be 5g / L, 10g / L, 20g / L, 30g / L, 40g / L, 50g / L, 60g / L, 70g / L, 80g / L, 90g / L or 100g / L, for example, in the embodiment can be 70.2g / L, 87.2g / L or 88.1g / L. In an embodiment of the present invention, the method of electroplating the pre-plated substrate using an acidic plating solution is consistent with the above-mentioned technical solution and will not be described in detail herein; the conditions of the electroplating treatment include: the plating solution temperature is 25-55°C, specifically 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or 55°C; the pH value can be 2-5, specifically 2, 2.5, 3, 3.5, 4, 4.5 or 5 (in the embodiment of the present invention, hydrochloric acid with a concentration of 30wt% can be used to adjust the pH value); the current density can be 0.1-10A / dm 2 , further can be 1~5A / dm2 , specifically 1A / dm 2 , 1.5A / dm 2 , 2A / dm 2 , 2.5A / dm 2 、3A / dm 2 、3.5A / dm 2 , 4A / dm 2 , 4.5A / dm 2 or 5A / dm 2 The time may be 1 to 300 min, further may be 10 to 90 min, specifically may be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min or 90 min.
[0032] In an embodiment of the present invention, when the material of the porous active layer is a cobalt-based alloy (i.e., corresponding to the oxygen evolution electrode), the composition of the alkaline plating solution includes cobalt salt, zinc salt, additive and water; the cobalt salt can be one or more of cobalt chloride, cobalt sulfate, cobalt fluoroborate, cobalt aminosulfonate, cobalt pyrophosphate and ammonium cobalt sulfate, specifically cobalt chloride, cobalt sulfate, cobalt fluoroborate, cobalt aminosulfonate, cobalt pyrophosphate or ammonium cobalt sulfate; the zinc salt can be one or more of zinc sulfate, zinc chloride, zinc nitrate and zinc oxide, specifically zinc sulfate, zinc chloride, zinc nitrate or zinc oxide; the additive can be potassium pyrophosphate, sodium pyrophosphate, ammonium chloride, sodium chloride, The invention can be one or more of potassium, sodium benzoate, triethanolamine, potassium sodium tartrate, sodium sulfate, sodium dodecyl sulfate, ascorbic acid, proline, tryptophan, serine, tyrosine and glycine, and can further be one or more of potassium pyrophosphate, sodium pyrophosphate, ammonium chloride, sodium chloride, potassium chloride, ascorbic acid, sodium benzoate, triethanolamine, glutamic acid, glycine and tryptophan, and can specifically be one or more of potassium pyrophosphate, sodium pyrophosphate, sodium benzoate, sodium sulfate, sodium chloride, glycine and ammonium chloride, for example, potassium pyrophosphate, glycine and sodium benzoate can be used in combination, and can also be sodium sulfate, sodium pyrophosphate, sodium chloride and ammonium chloride can be used in combination. In an embodiment of the present invention, the concentration of the cobalt salt in the alkaline plating solution may be 20-100 g / L, specifically 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L; the concentration of the zinc salt may be 10-60 g / L, specifically 10 g / L, 20 g / L, 25 g / L, 30 g / L, 40 g / L, 45 g / L, 50 g / L or 60 g / L; the concentration of the additive may be 0.1-500 g / L, further 1-300 g / L, further 50-250 g / L, and further 150-230 g / L, for example, 170 g / L or 229 g / L in the embodiment. In an embodiment of the present invention, the method of electroplating the pre-plated substrate using an alkaline plating solution is consistent with the above-mentioned technical solution and will not be described in detail herein; the conditions of the electroplating treatment include: the plating solution temperature is 25-55°C, specifically 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or 55°C; the pH value can be 8-10, specifically 8, 8.5, 9, 9.5 or 10 (in the embodiment of the present invention, the pH value can be adjusted using 30wt% ammonia water); the current density can be 0.1-10A / dm 2 , further can be 1~5A / dm 2 , specifically 1A / dm 2 , 1.5A / dm 2 , 2A / dm 2 , 2.5A / dm 2 、3A / dm2 、3.5A / dm 2 , 4A / dm 2 , 4.5A / dm 2 or 5A / dm 2 The time may be 1 to 300 min, further may be 10 to 120 min, specifically may be 10 min, 15 min, 30 min, 50 min, 60 min, 70 min, 90 min or 120 min.
[0033] In an embodiment of the present invention, when the material of the porous active layer is a cobalt-based alloy (i.e., corresponding to the oxygen evolution electrode), the composition of the acidic plating solution includes a cobalt salt, a zinc salt and an additive; the cobalt salt may be one or more of cobalt chloride, cobalt sulfate, cobalt fluoroborate, cobalt aminosulfonate, cobalt pyrophosphate and ammonium cobalt sulfate, specifically cobalt chloride, cobalt sulfate, cobalt fluoroborate, cobalt aminosulfonate, cobalt pyrophosphate or ammonium cobalt sulfate, or a combination of cobalt sulfate and cobalt chloride; the zinc salt may be one or more of zinc sulfate, zinc chloride, zinc nitrate and zinc oxide, specifically zinc sulfate, zinc chloride, zinc nitrate or zinc oxide; the additive may be ammonium chloride, sodium citrate, citric acid or sodium succinate. , sodium chloride, potassium chloride, malic acid, boric acid, ascorbic acid, potassium sodium tartrate, sodium sulfate, sodium dodecyl sulfate, alanine, glutamic acid and glycine, and can further be one or more of sodium citrate, citric acid, sodium chloride, potassium chloride, malic acid, boric acid, ascorbic acid, potassium sodium tartrate, sodium sulfate, sodium dodecyl sulfate, glycine and glutamic acid, and specifically can be one or more of sodium citrate, citric acid, glutamic acid, sodium chloride, boric acid and potassium sodium tartrate, for example, it can be a combination of sodium citrate, glutamic acid, sodium chloride, boric acid and potassium sodium tartrate, or it can be a combination of potassium sodium tartrate, citric acid, sodium chloride and boric acid. In an embodiment of the present invention, the concentration of the cobalt salt in the acidic plating solution may be 10-100 g / L, specifically 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L; the concentration of the zinc salt may be 5-50 g / L, specifically 5 g / L, 10 g / L, 15 g / L, 20 g / L, 30 g / L, 40 g / L or 50 g / L; the concentration of the additive may be 0.1-500 g / L, further 0.5-400 g / L, further 50-380 g / L, further 150-360 g / L, for example, 155 g / L or 358 g / L in the embodiment. In an embodiment of the present invention, the method of electroplating the pre-plated substrate using an acidic plating solution is consistent with the above-mentioned technical solution and is not described in detail herein; the conditions of the electroplating treatment include: the plating solution temperature is 25-55°C, specifically 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or 55°C; the pH value can be 1-6, specifically 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6 (in the embodiment of the present invention, hydrochloric acid with a concentration of 30wt% can be used to adjust the pH value); the current density can be 0.1-10A / dm 2 , further can be 0.3~5A / dm 2 , specifically 0.3A / dm 2 , 0.5A / dm 2 , 1A / dm 2, 2A / dm 2 、3A / dm 2 , 4A / dm 2 or 5A / dm 2 The time may be 1 to 300 min, further may be 10 to 90 min, specifically may be 10 min, 15 min, 30 min, 50 min, 70 min or 90 min.
[0034] After obtaining the electroplated substrate, the present invention performs a zinc stripping treatment on the electroplated substrate to remove part of the zinc in the active layer and form a porous structure in the active layer to obtain the electrode. In an embodiment of the present invention, the zinc stripping reagent used in the zinc stripping treatment can be an acid reagent or an alkaline reagent; the pH value of the acid reagent can be 3 to 6, specifically 3, 3.5, 4, 4.5, 5, 5.5 or 6; the acid reagent can be one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, citric acid, malic acid, oxalic acid and oxalic acid, specifically hydrochloric acid or sulfuric acid; the alkaline reagent can be a KOH solution, and the concentration of the KOH solution can be 1 to 6 mol / L, specifically 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L or 6 mol / L. In an embodiment of the present invention, the electroplated substrate is immersed in the zinc stripping reagent for zinc stripping treatment; the temperature of the zinc stripping treatment can be 25-40°C, specifically 25°C, 30°C, 35°C or 40°C; the time can be 1-72h, further 1-48h, specifically 1h, 5h, 12h, 20h, 24h, 36h or 48h. In the embodiment of the present invention, zinc stripping treatment can remove part of the zinc in the active layer, that is, reduce the zinc content in the active layer, and form a porous active layer. Specifically, the present invention forms an active layer on the surface of the pre-plated substrate by electroplating treatment, and the active layer is specifically a cobalt-zinc alloy layer or a nickel-zinc alloy layer. The atomic percentage of zinc in the active layer is 5-40%. Since the electrode needs to be immersed in alkaline solution when used for electrolysis of water to produce hydrogen, if the zinc content itself is too high, it may cause the collapse of the active layer structure. The present invention removes part of zinc through zinc removal treatment and retains the nickel skeleton, and has a large number of porous structures to form a structure similar to that of Raney nickel material, but has higher bonding strength than that of Raney nickel material.
[0035] In an embodiment of the present invention, a heat treatment may be further included between the electroplating treatment and the zinc stripping treatment; the temperature of the heat treatment may be 100-400°C, specifically 100°C, 150°C, 200°C, 250°C, 300°C, 350°C or 400°C; the heating rate to the temperature of the heat treatment may be 1-20°C / min, specifically 1°C / min, 5°C / min, 10°C / min, 15°C / min or 20°C / min; the holding time may be 0.5-4h, specifically 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h. In the embodiment of the present invention, the heat treatment is beneficial to accelerate the speed of the zinc stripping treatment and improve the stability of the long-term operation of the electrode.
[0036] In the embodiment of the present invention, the heat treatment can be carried out in an atmosphere containing oxygen; the atmosphere containing oxygen can be air, or a mixed gas of at least one of nitrogen, argon and hydrogen and oxygen; the volume fraction of oxygen in the mixed gas can be 1-50%, specifically 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%. In the embodiment of the present invention, the heat treatment is carried out in an atmosphere containing oxygen, and the material of the porous active layer finally obtained is an alloy oxide, such as NiZnO alloy oxide (NiZn a O b ) or CoZnO alloy oxide (CoZn y O x ).
[0037] The present invention provides the application of the electrode described in the above technical solution or the electrode prepared by the preparation method described in the above technical solution in hydrogen production by electrolysis of water.
[0038] In an embodiment of the present invention, when the porous active layer is a nickel-based alloy, the electrode can be used as a hydrogen evolution electrode for electrolysis of water to produce hydrogen. At this time, the hydrogen evolution electrode is specifically used as a cathode in the process of electrolysis of water to produce hydrogen, and the anode used in conjunction with it can be a nickel mesh, nickel foam or other oxygen evolution active electrodes (such as the oxygen evolution electrode described in the present invention).
[0039] In an embodiment of the present invention, when the porous active layer is a cobalt-based alloy, the electrode can be used as an oxygen evolution electrode for electrolysis of water to produce hydrogen. At this time, the oxygen evolution electrode is specifically used as an anode in the process of electrolysis of water to produce hydrogen, and the cathode used in conjunction with it can be a nickel mesh, nickel foam or other hydrogen evolution active electrode (such as the hydrogen evolution electrode described in the present invention).
[0040] In the current related technologies, 1000Nm 3 / h alkaline electrolyzers mostly use Raney nickel materials as cathodes and / or anodes, and Raney nickel materials generally use plasma spraying technology, specifically, nickel-aluminum mixed metal powders are sprayed on the substrate surface by high temperature and high pressure, and then soaked in alkaline solution to remove aluminum, retain nickel on the substrate surface and form a porous nickel structure, increase the specific surface area of the electrode, and improve electrode activity. Although Raney nickel materials have high activity and high specific surface area, they have poor binding force, and active materials are easy to fall off, resulting in greater safety hazards. In particular, with the further increase in the current density demand of alkaline electrolyzers, the shedding phenomenon of active materials will become more and more serious, which is not conducive to the long-term safe operation of alkaline electrolyzers. Compared with the existing Raney nickel materials on the market, in the electrode prepared by the method of the present invention, the physical binding force between the active material (porous active layer) and the substrate and the active material is greatly improved, which effectively avoids the physical shedding of the active material under working conditions, and the catalytic activity is better.
[0041] The electrode whose porous active layer is a nickel-based alloy in the present invention can be used as a hydrogen evolution electrode. Under working conditions, the hydrogen evolution overpotential is reduced by 190-250 mV compared with the hydrogen evolution overpotential of a commercial nickel mesh, which is better than most commercially available Raney nickel active electrodes; and it has the advantages of high activity, high stability and high structural strength, and can provide a rich pore structure, thereby increasing the material specific surface area and improving the hydrophilic and hydrophobic properties, which is beneficial to its application as an electrode material.
[0042] In addition, regarding the anode for hydrogen production by electrolysis of water, in the current related technologies, high-nickel materials such as pure nickel mesh, nickel foam or Raney nickel material are often used as anodes in large commercial alkaline electrolyzers. However, the intrinsic catalytic activity of OER of such materials is poor, which seriously restricts the development of alkaline electrolyzers in the mode of reducing costs and increasing efficiency. Compared with hydrogen evolution electrodes, the conditions for realizing high-activity and high-stability oxygen evolution electrodes are more stringent due to the slow OER reaction and harsh environment. The electrode prepared by the method of the present invention, when its porous active layer is a cobalt-based alloy, can be used as an oxygen evolution electrode, and a CoZn alloy is formed by electroplating. On this basis, in combination with a heat treatment process (carried out in an atmosphere containing oxygen) and a zinc stripping process, the chemical coordination of metal atoms can be regulated, thereby improving the active material (CoZnO alloy oxide, CoZn y O x )'s oxygen evolution activity. At the same time, the zinc removal process can form a porous structure that is more suitable for high current density. Under operating test conditions, the oxygen evolution overpotential is reduced by 89~200mV compared with that of commercial nickel mesh.
[0043] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The degreasing liquid used in the following examples is a mixed aqueous solution of sodium hydroxide, sodium carbonate, sodium silicate and trisodium phosphate, wherein the concentration of sodium hydroxide is 80 g / L, the concentration of sodium carbonate is 25 g / L, the concentration of sodium silicate is 10 g / L, and the concentration of trisodium phosphate is 80 g / L.
[0045] The solvent of the pre-plating solution and the plating solution used in the following examples is water.
[0046] Example 1 Hydrogen Evolution Electrode The nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 150 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, and a stainless steel plate was used as a cathode, and a direct current was connected at a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh is immersed in the pre-plating solution, the acidified nickel mesh is used as the cathode, the nickel plate is used as the anode, and the current density is 2A / dm 2 The pre-plating was performed for 5 minutes under the conditions to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 110 g / L nickel chloride, 50 g / L hydrochloric acid, the pH value of the pre-plating solution is 4.5, and the temperature is 40°C; The pre-nickel-plated mesh was immersed in the plating solution, with the pre-nickel-plated mesh as the cathode and the nickel plate as the anode. 2 Electroplating was performed for 15 minutes under the conditions to form a nickel-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 50 g / L nickel sulfate, 190 g / L potassium pyrophosphate, 19 g / L potassium sodium tartrate, 19 g / L glycine, 20 g / L sodium chloride, and 25 g / L zinc sulfate, the pH value of the plating solution is 8 (the pH value is adjusted by using 30 wt% ammonia water), and the temperature is 35°C; The electroplated nickel mesh was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc stripping treatment at 40° C. for 24 hours to obtain a hydrogen evolution electrode.
[0047] Example 2 Hydrogen Evolution Electrode The nickel plate was sandblasted with sand having a particle size of 100 mesh to obtain a sandblasted nickel plate; the sandblasted nickel plate was immersed in a degreasing liquid, the sandblasted nickel plate was used as an anode, the stainless steel plate was used as a cathode, a direct current was connected, and a current density of 2A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel plate to obtain a degreasing nickel plate; the degreasing nickel plate was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain an acidified nickel plate; The acidified nickel plate is immersed in the pre-plating solution, the acidified nickel plate is used as the cathode, the graphite plate is used as the anode, and the current density is 1.5A / dm 2 The pre-plating was performed under the conditions of 50°C for 5 minutes to form a nickel transition layer on the surface of the acidified nickel plate, thereby obtaining a pre-plated nickel plate; wherein the composition of the pre-plating solution is: 200 g / L nickel sulfate, 40 g / L hydrochloric acid, and 10 g / L sodium chloride, the pH value of the pre-plating solution is 3, and the temperature is 30°C; The pre-nickel plate was immersed in the plating solution, the pre-nickel plate was used as the cathode, the graphite plate was used as the anode, and the current density was 2.5 A / dm 2 Electroplating is performed under the following conditions for 30 minutes to form a nickel-zinc active layer on the surface of the pre-nickel-plated plate, thereby obtaining an electroplated nickel plate; wherein the composition of the plating solution is: 100 g / L nickel sulfate, 80 g / L nickel chloride, 20 g / L sodium citrate, 40 g / L boric acid, 5 g / L ascorbic acid, 20 g / L sodium chloride, 20 g / L sodium sulfate, 0.2 g / L sodium dodecyl sulfate, 10 g / L zinc sulfate, 20 g / L zinc chloride, the pH value of the plating solution is 4.5 (the pH value is adjusted by using hydrochloric acid with a concentration of 30 wt%), and the temperature is 45°C; The electroplated nickel plate is placed in a muffle furnace, heated from room temperature to 300° C. at a rate of 10° C. / min in an air atmosphere, and heat-treated at 300° C. for 2 h to obtain a heat-treated nickel plate; The heat-treated nickel plate was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc removal treatment at 40° C. for 24 hours to obtain a hydrogen evolution electrode.
[0048] Example 3 Hydrogen Evolution Electrode A nickel mesh (30 mesh, 0.3 μm wire diameter) was sandblasted with sand having a particle size of 100 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, a stainless steel plate was used as a cathode, a direct current was connected, and a current density of 2 A / dm 2The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh was immersed in the pre-plating solution, with the acidified nickel mesh as the cathode and the nickel plate as the anode, at a current density of 2.5 A / dm 2 The pre-plating was performed under the conditions of 30°C for 3 minutes to form a nickel transition layer on the surface of the acidified nickel mesh, thereby obtaining a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 200 g / L nickel sulfate, 40 g / L hydrochloric acid, and 10 g / L sodium chloride, the pH value of the pre-plating solution is 3, and the temperature is 30°C; The pre-nickel-plated mesh was immersed in the plating solution, with the pre-nickel-plated mesh as the cathode and the nickel plate as the anode. 2 Electroplating was performed for 30 minutes under the conditions to form a nickel-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 30 g / L nickel sulfate, 150 g / L potassium pyrophosphate, 15 g / L glutamic acid, 10 g / L sodium chloride, 2 g / L ascorbic acid, and 16 g / L zinc sulfate, the pH value of the plating solution is 8 (the pH value is adjusted by using 30 wt% ammonia water), and the temperature is 35°C; The electroplated nickel mesh was immersed in hydrochloric acid with a pH value of 5, and subjected to zinc removal treatment at 40° C. for 24 hours to obtain a hydrogen evolution electrode.
[0049] Example 4 Hydrogen Evolution Electrode A nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 200 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, a stainless steel plate was used as a cathode, a direct current was connected, and a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh was immersed in the pre-plating solution, with the acidified nickel mesh as the cathode and the nickel plate as the anode, at a current density of 2.5 A / dm 2 The pre-plating was performed under the conditions of 10 minutes to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 200 g / L nickel sulfate, 40 g / L hydrochloric acid, the pH value of the pre-plating solution is 3, and the temperature is 30°C; The pre-nickel-plated mesh is immersed in the plating solution, the pre-nickel-plated mesh is used as the cathode, the nickel plate is used as the anode, and the current density is 2A / dm 2Electroplating is performed for 30 minutes under the conditions to form a nickel-zinc active layer on the surface of the pre-nickel-plated mesh to obtain an electroplated nickel mesh; wherein the composition of the plating solution is: 100 g / L nickel sulfate, 70 g / L nickel chloride, 30 g / L sodium citrate, 50 g / L boric acid, 8 g / L ascorbic acid, 0.1 g / L sodium dodecyl sulfate, 10 g / L zinc chloride, and 10 g / L zinc sulfate, the pH value of the plating solution is 4 (the pH value is adjusted by using hydrochloric acid with a concentration of 30 wt%), and the temperature is 40°C; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 350° C. at a rate of 10° C. / min in an air atmosphere, and heat-treated at 350° C. for 2.5 hours to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc removal treatment at 40° C. for 20 h to obtain a hydrogen evolution electrode.
[0050] Example 5 Hydrogen Evolution Electrode The nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 150 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, and a stainless steel plate was used as a cathode, and a direct current was connected at a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh is immersed in the pre-plating solution, the acidified nickel mesh is used as the cathode, the graphite plate is used as the anode, and the current density is 2A / dm 2 The pre-plating was performed under the conditions of 50°C for 5 minutes to form a nickel transition layer on the surface of the acidified nickel mesh, thereby obtaining a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 200 g / L nickel sulfate, 40 g / L hydrochloric acid, and 10 g / L sodium chloride, the pH value of the pre-plating solution is 3, and the temperature is 30°C; The pre-nickel-plated mesh was immersed in the plating solution, the pre-nickel-plated mesh was used as the cathode, the graphite plate was used as the anode, and the current density was 2A / dm 2 Electroplating was performed for 30 minutes under the conditions to form a nickel-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 40 g / L nickel sulfate, 150 g / L sodium pyrophosphate, 20 g / L glycine, 10 g / L ammonium chloride, and 22 g / L zinc chloride, the pH value of the plating solution is 9 (the pH value is adjusted by using 30 wt% ammonia water), and the temperature is 43°C; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 300° C. at a rate of 10° C. / min in an atmosphere of an oxygen-nitrogen mixed gas with an oxygen volume fraction of 20%, and heat-treated at 300° C. for 4 hours to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in sulfuric acid with a pH value of 5 and subjected to a zinc removal treatment at 40° C. for 24 hours to obtain a hydrogen evolution electrode.
[0051] Example 6 Hydrogen Evolution Electrode The nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 150 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, and a stainless steel plate was used as a cathode, and a direct current was connected at a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh is immersed in the pre-plating solution, the acidified nickel mesh is used as the cathode, the nickel plate is used as the anode, and the current density is 2A / dm 2 The pre-plating was performed for 15 minutes under the conditions to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 200 g / L nickel sulfate, 40 g / L hydrochloric acid, the pH value of the pre-plating solution is 3, and the temperature is 30°C; The pre-nickel-plated mesh was immersed in the plating solution, with the pre-nickel-plated mesh as the cathode and the nickel plate as the anode. 2 Electroplating is performed under the following conditions for 30 minutes to form a nickel-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 120 g / L nickel sulfate, 60 g / L nickel chloride, 25 g / L potassium sodium tartrate, 40 g / L boric acid, 5 g / L ascorbic acid, 0.2 g / L sodium dodecyl sulfate, 20 g / L zinc chloride, and 15 g / L zinc sulfate; the pH value of the plating solution is 4.5 (the pH value is adjusted by using hydrochloric acid with a concentration of 30 wt%), and the temperature is 45°C; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 250° C. at a rate of 10° C. / min in an air atmosphere, and heat-treated at 250° C. for 4 hours to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc removal treatment at 40° C. for 20 h to obtain a hydrogen evolution electrode.
[0052] Table 1 shows the index parameters of the hydrogen evolution electrodes prepared in Examples 1 to 6.
[0053] Table 1 Index parameters of hydrogen evolution electrodes prepared in Examples 1 to 6
[0054] Test Example 1 Figure 1 This is a SEM image of the hydrogen evolution electrode prepared in Example 2. The results show that the nickel-zinc active layer of the hydrogen evolution electrode is formed by the accumulation of nanosheets and has a porous structure, which can provide a large number of active sites; and the nanosheets are interconnected, which is beneficial to ensure that the hydrogen evolution electrode does not fall off during operation, thereby improving its long-term operation stability; at the same time, the nanosheets have a large specific surface area and can be used as an intermediate layer structure, which is beneficial to the later loading of other materials and improving the bonding force with other materials.
[0055] The SEM images of the hydrogen evolution electrodes prepared in the other embodiments of the present invention are similar to those of Figure 1 Similar, all have the above-mentioned morphological structure.
[0056] Test Example 2 The performance of the hydrogen evolution electrodes prepared in Examples 1 to 6 was tested using a three-electrode system and compared with a commercial nickel mesh (40 mesh, 0.25 μm wire diameter; the same as the nickel mesh used in Example 1), and the specific conditions were as follows: In the three-electrode system, the counter electrode is a platinum mesh, the reference electrode is a Hg / HgO electrode, and the working electrode is a target material (the hydrogen evolution electrode prepared in Examples 1 to 6 or a commercial nickel mesh, with a size of 1 cm×1 cm); the electrolyte is a KOH solution with a concentration of 1 mol / L; the test temperature is 80°C, and the test current density is 3000~5000 A / m 2 ;The reference electrode is in contact with the electrolyte through a salt bridge.
[0057] Table 2 shows the hydrogen evolution overpotentials of the hydrogen evolution electrodes prepared in Examples 1 to 6 and the commercial nickel mesh. The results show that the hydrogen evolution overpotential of the hydrogen evolution electrode prepared in the present invention is reduced by 190 to 250 mV compared with the hydrogen evolution overpotential of the commercial nickel mesh.
[0058] Table 2 Hydrogen evolution overpotentials of the hydrogen evolution electrodes prepared in Examples 1 to 6 and the commercial nickel mesh
[0059] Test Example 3 The hydrogen evolution electrodes prepared in Example 1 and Example 2 were heated to 2 Nm 3 / h electrolyzer under simulated operating conditions to test its long-term stability. The test temperature was 80±5℃ and the electrolyzer pressure was 1.6MPa.
[0060] Figure 2 The long-term stability test results of the hydrogen evolution electrodes prepared in Example 1 and Example 2 are shown in FIG. Figure 2 It can be seen that the material performance of the hydrogen evolution electrode prepared in Example 1 begins to decay after running for about 50 hours, while the performance of the hydrogen evolution electrode prepared in Example 2 remains stable, indicating that zinc removal treatment after heat treatment can improve the stability of the hydrogen evolution electrode.
[0061] Test Example 4 The hydrogen evolution electrode prepared in Example 2 was heated to 2 Nm 3 / h electrolyzer under simulated operating conditions to test its long-term stability, with the test temperature being 80±5℃ and the electrolyzer pressure being 1.6MPa, and compared with commercial nickel mesh.
[0062] Figure 3 The long-term stability test results of the hydrogen evolution electrode prepared in Example 2 and the commercial nickel mesh are shown in FIG. Figure 3 It can be seen that, compared with the commercial nickel mesh, during the operation of the hydrogen evolution electrode prepared in Example 2, the cell voltage is stable between 1.75 and 1.78 V, and there is no obvious performance attenuation after running for 200 hours.
[0063] Test Example 5 The hydrogen evolution electrode prepared in Example 3 was placed in a sample bottle containing water and ultrasonicated for 2 min at an ultrasonic power of 380 W. The material shedding phenomenon after ultrasonication was observed and compared with a commercially available Raney nickel product.
[0064] Figure 4 The graph is a test result of the binding force of the hydrogen evolution electrode prepared in Example 3 and the binding force of Raney nickel. The left side is a photo of the Raney nickel after ultrasound, and the right side is a photo of the hydrogen evolution electrode prepared in Example 3 after ultrasound. Figure 4 It can be seen that the Raney nickel material has poor bonding strength and has a falling-off phenomenon after ultrasound, while the hydrogen evolution electrode prepared by the present invention has good bonding strength and has no powder falling phenomenon after ultrasound.
[0065] Example 7 Oxygen Evolution Electrode The nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 150 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, and a stainless steel plate was used as a cathode, and a direct current was connected at a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh was immersed in the pre-plating solution, with the acidified nickel mesh as the cathode and the nickel plate as the anode, at a current density of 2.5 A / dm 2The pre-plating was performed for 10 minutes under the conditions to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 120 g / L nickel chloride, 50 g / L hydrochloric acid, the pH value of the pre-plating solution is 4.5, and the temperature is 35° C.; The pre-nickel-plated mesh was immersed in the plating solution, with the pre-nickel-plated mesh as the cathode and the nickel plate as the anode. 2 Electroplating was performed for 60 minutes under the conditions to form a cobalt-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 50 g / L cobalt sulfate, 190 g / L potassium pyrophosphate, 19 g / L glycine, 20 g / L sodium benzoate, and 25 g / L zinc sulfate, the pH value of the plating solution is 8 (the pH value is adjusted by using 30 wt% ammonia water), and the temperature is 50°C; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 300° C. at a rate of 10° C. / min in an air atmosphere, and heat-treated at 300° C. for 2 h to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc stripping treatment at 40° C. for 24 hours to obtain an oxygen evolution electrode.
[0066] Example 8 Oxygen Evolution Electrode The nickel plate was sandblasted with sand having a particle size of 100 mesh to obtain a sandblasted nickel plate; the sandblasted nickel plate was immersed in a degreasing liquid, the sandblasted nickel plate was used as an anode, the stainless steel plate was used as a cathode, a direct current was connected, and a current density of 2A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel plate to obtain a degreasing nickel plate; the degreasing nickel plate was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain an acidified nickel plate; The acidified nickel plate is immersed in the pre-plating solution, the acidified nickel plate is used as the cathode, the nickel plate is used as the anode, and the current density is 2.5A / dm 2 The pre-plating was performed under the following conditions for 10 minutes to electroplate a nickel transition layer on the surface of the acidified nickel plate to obtain a pre-plated nickel plate; wherein the pre-plating solution comprises: 120 g / L nickel chloride and 50 g / L hydrochloric acid, the pH value of the pre-plating solution is 4.5, and the temperature is 35° C.; The pre-nickel plate was immersed in the plating solution, the pre-nickel plate was used as the cathode, the graphite plate was used as the anode, and the current density was 2.5 A / dm 2Electroplating is performed for 15 minutes under the conditions to form a cobalt-zinc active layer on the surface of the pre-nickel-plated plate to obtain an electroplated nickel plate; wherein the composition of the plating solution is: 30 g / L cobalt sulfate, 50 g / L cobalt chloride, 230 g / L sodium citrate, 23 g / L glutamic acid, 50 g / L sodium chloride, 45 g / L boric acid, 10 g / L potassium sodium tartrate, and 15 g / L zinc chloride, the pH value of the plating solution is 4.5 (the pH value is adjusted by using hydrochloric acid with a concentration of 30 wt%), and the temperature is 45°C; The electroplated nickel plate is placed in a muffle furnace, heated from room temperature to 200° C. at a rate of 10° C. / min in an oxygen-nitrogen mixed gas atmosphere with an oxygen volume fraction of 40%, and heat-treated at 200° C. for 3 hours to obtain a heat-treated nickel plate; The heat-treated nickel plate was immersed in a KOH solution with a concentration of 1 mol / L and subjected to zinc removal treatment at 40° C. for 24 hours to obtain an oxygen evolution electrode.
[0067] Example 9 Oxygen Evolution Electrode A nickel mesh (30 mesh, 0.3 μm wire diameter) was sandblasted with sand having a particle size of 100 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, a stainless steel plate was used as a cathode, a direct current was connected, and a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh was immersed in the pre-plating solution, with the acidified nickel mesh as the cathode and the nickel plate as the anode, at a current density of 2.5 A / dm 2 The pre-plating was performed under the following conditions for 10 minutes to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 280 g / L nickel sulfate, 40 g / L hydrochloric acid, and 20 g / L sodium chloride, the pH value of the pre-plating solution is 2, and the temperature is 33° C.; The pre-nickel-plated mesh is immersed in the plating solution, the pre-nickel-plated mesh is used as the cathode, the nickel plate is used as the anode, and the current density is 2A / dm 2 Electroplating was performed for 30 minutes under the conditions to form a cobalt-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution was: 30 g / L cobalt chloride, 15 g / L potassium sodium tartrate, 100 g / L citric acid, 15 g / L sodium chloride, 25 g / L boric acid, and 40 g / L zinc sulfate; the pH value of the plating solution was 4 (the pH value was adjusted by using hydrochloric acid with a concentration of 30 wt%), and the temperature was 55° C.; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 300° C. at a rate of 10° C. / min in an argon-nitrogen mixed gas atmosphere with an oxygen volume fraction of 20%, and heat-treated at 300° C. for 2 h to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in a KOH solution with a concentration of 1 mol / L and subjected to a zinc stripping treatment at 40° C. for 24 hours to obtain an oxygen evolution electrode.
[0068] Example 10 Oxygen evolution electrode The nickel mesh (40 mesh, 0.25 μm wire diameter) was sandblasted with sand having a particle size of 150 mesh to obtain a sandblasted nickel mesh; the sandblasted nickel mesh was immersed in a degreasing liquid, the sandblasted nickel mesh was used as an anode, and a stainless steel plate was used as a cathode, and a direct current was connected at a current density of 2 A / dm 2 The degreasing treatment was carried out for 10 minutes under the conditions to remove organic impurities attached to the surface of the sandblasted nickel mesh to obtain the degreasing nickel mesh; the degreasing nickel mesh was immersed in hydrochloric acid with a concentration of 20wt%, and acidification treatment was carried out at room temperature for 15 minutes to obtain the acidified nickel mesh; The acidified nickel mesh was immersed in the pre-plating solution, with the acidified nickel mesh as the cathode and the nickel plate as the anode, at a current density of 2.5 A / dm 2 The pre-plating was performed under the following conditions for 10 minutes to electroplate a nickel transition layer on the surface of the acidified nickel mesh to obtain a pre-plated nickel mesh; wherein the composition of the pre-plating solution is: 280 g / L nickel sulfate, 40 g / L hydrochloric acid, and 20 g / L sodium chloride, the pH value of the pre-plating solution is 2, and the temperature is 33° C.; The pre-nickel-plated mesh was immersed in the plating solution, the pre-nickel-plated mesh was used as the cathode, the graphite plate was used as the anode, and the current density was 2A / dm 2 Electroplating was performed for 30 minutes under the conditions to form a cobalt-zinc active layer on the surface of the pre-nickel-plated mesh, thereby obtaining an electroplated nickel mesh; wherein the composition of the plating solution is: 40 g / L cobalt sulfate, 50 g / L sodium sulfate, 100 g / L sodium pyrophosphate, 10 g / L sodium chloride, 10 g / L ammonium chloride, and 30 g / L zinc chloride, the pH value of the plating solution is 9 (the pH value is adjusted by using 30 wt% ammonia water), and the temperature is 50°C; The electroplated nickel mesh is placed in a muffle furnace, heated from room temperature to 400° C. at a rate of 10° C. / min in an air atmosphere, and heat-treated at 400° C. for 2 h to obtain a heat-treated nickel mesh; The heat-treated nickel mesh was immersed in hydrochloric acid with a pH value of 5, and subjected to zinc removal treatment at 40° C. for 24 hours to obtain an oxygen evolution electrode.
[0069] Table 3 shows the index parameters of the oxygen evolution electrodes prepared in Examples 7 to 10.
[0070] Table 3 Index parameters of oxygen evolution electrodes prepared in Examples 7 to 10
[0071] Test Example 6 The oxygen evolution electrodes prepared in Examples 7 to 10 were tested for performance using a three-electrode system and compared with a commercial nickel mesh (40 mesh, 0.25 μm wire diameter; the same as the nickel mesh used in Example 7), and the specific conditions were as follows: In the three-electrode system, the counter electrode is a platinum mesh, the reference electrode is a Hg / HgO electrode, and the working electrode is the target material (the oxygen evolution electrode prepared in Examples 7 to 10 or a commercial nickel mesh, with a size of 1 cm×1 cm); the electrolyte is a KOH solution with a concentration of 1 mol / L; the test temperature is 80°C, and the test current density is 3000~5000 A / m 2 ;The reference electrode is in contact with the electrolyte through a salt bridge.
[0072] Table 4 shows the hydrogen evolution overpotentials of the oxygen evolution electrodes prepared in Examples 7 to 10 and the commercial nickel mesh. The results show that the hydrogen evolution overpotential of the oxygen evolution electrode prepared in the present invention is reduced by 89 to 200 mV compared with the hydrogen evolution overpotential of the commercial nickel mesh.
[0073] Table 4 Oxygen evolution overpotential of oxygen evolution electrodes prepared in Examples 7 to 10 and commercial nickel mesh
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An electrode, characterized in that: It includes a substrate, a nickel transition layer coated on the surface of the substrate and a porous active layer coated on the surface of the nickel transition layer. The material of the porous active layer is a nickel-based alloy or a cobalt-based alloy. The alloy elements in the nickel-based alloy and the cobalt-based alloy include zinc.
2. The electrode according to claim 1, characterized in that The electrode is a hydrogen evolution electrode or an oxygen evolution electrode; When the electrode is a hydrogen evolution electrode, the material of the porous active layer is a nickel-based alloy; When the electrode is an oxygen evolution electrode, the material of the porous active layer is a cobalt-based alloy.
3. The electrode according to claim 1 or 2, characterized in that The thickness of the porous active layer is 1-50 μm, and the atomic percentage of zinc in the porous active layer is ≤20%; the porous active layer is formed by stacking nanosheets.
4. The electrode according to claim 1 or 2, characterized in that: The thickness of the nickel transition layer is 0.2-2 μm.
5. The electrode according to claim 1 or 2, characterized in that: The substrate is a metal substrate.
6. The method for preparing an electrode according to any one of claims 1 to 5, characterized in that: The following steps are involved: Placing the substrate in a first plating solution for pre-electroplating to form a nickel transition layer on the surface of the substrate to obtain a pre-plated substrate; The first plating solution contains nickel salt; Placing the pre-plated substrate in a second plating solution for electroplating to form an active layer on the surface of the pre-plated substrate to obtain an electroplated substrate; The second plating solution contains a nickel salt and a zinc salt, or the second plating solution contains a cobalt salt and a zinc salt; The electroplated substrate is subjected to a zinc stripping treatment to remove a portion of zinc in the active layer and to form a porous structure in the active layer, thereby obtaining the electrode.
7. The preparation method according to claim 6, characterized in that: The conditions of the pre-electroplating treatment include: the plating solution temperature is 25-60°C, the pH value is 1-6, and the current density is 0.1-10A / dm 2 , time is 1~30min; The electroplating treatment conditions include: the plating solution temperature is 25-55°C, the pH value is 1-10, and the current density is 0.1-10A / dm 2 , time is 1~300min.
8. The preparation method according to claim 6 or 7, characterized in that: A heat treatment is also included between the electroplating treatment and the zinc stripping treatment; the temperature of the heat treatment is 100-400° C., and the insulation time is 0.5-4 hours; and the heat treatment is carried out in an atmosphere containing oxygen.
9. Use of the electrode according to any one of claims 1 to 5 or the electrode prepared by the preparation method according to any one of claims 6 to 8 in hydrogen production by electrolysis of water.
10. The use according to claim 9, characterized in that: When the material of the porous active layer is a nickel-based alloy, the electrode is used as a hydrogen evolution electrode for electrolyzing water to produce hydrogen; when the material of the porous active layer is a cobalt-based alloy, the electrode is used as an oxygen evolution electrode for electrolyzing water to produce hydrogen.
Citation Information
Patent Citations
Preparation method of nanocrystalline nickel-molybdenum alloy porous composite electrode
CN111850599A
Method for treating metal substrate for producing electrode
CN115335556A
Negative electrode containing transition layer and used for hydrogen production by alkaline electrolysis of water
CN118704037A
Production of cathode for generating hydrogen
JP1987253791A
Method of preparing a cathode by high and low temperature electroplating of catalytic and sacrificial metals, and electrode prepared thereby
US4331517A
Cited By
Metal-based active material and preparation method and application thereof