Manufacturing method of watch crystal

Through chemical vapor deposition method and high-pressure and high-temperature treatment combined with microwave plasma assistance and other technologies, the problem of insufficient quality and durability of diamond watch crystals in the existing technology has been solved, and high-quality and beautiful diamond watch crystal manufacturing is achieved.

CN119020859APending Publication Date: 2024-11-26科里·阿尔伯特·莫罗
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410653470.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively manufacture durable and aesthetic diamond watch crystals, especially in terms of combining high quality and scratch resistance.

Method used

The diamond plate was grown in the initial step by chemical vapor deposition method and placed in a high-pressure and high-temperature environment for further processing, combining microwave plasma-assisted chemical vapor deposition, hot wire chemical vapor deposition and inductively coupled plasma enhanced chemical vapor deposition, etc. Steps to form high-quality diamond crystals.

Benefits of technology

Through this method, diamond watch crystals with excellent scratch resistance and beautiful appearance can be produced, ensuring the high quality and durability of the product and meeting the needs of luxury watches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020859A_ABST
    Figure CN119020859A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method of a diamond watch crystal, wherein a plurality of technologies are adopted to produce a final product. The method of the invention begins with a chemical vapor deposition process in which high purity graphite is used as the source substrate. The step further employs a gas, temperature, and an energy source to facilitate formation of the diamond layer on the substrate. The invention provides alternative energy sources during chemical vapor deposition, such as, but not limited to, microwave plasma, direct current plasma, inductively coupled plasma, and hot wire technology. According to the method, a high-pressure and high-temperature step is further adopted after the chemical vapor deposition step. The two steps are repeated, wherein the first subsequent step includes the diamond seed. Prior to cutting and polishing, impurities are removed using a final high-pressure, high-temperature step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates generally to diamond manufacturing and more particularly, but not exclusively, to a method of manufacturing watch crystals wherein the method utilizes a variety of techniques to provide for the manufacture of watch crystals. Background Art

[0002] The formation of lab grown diamonds can be done using two methods, chemical vapor deposition (CVD) and high pressure high temperature (HPHT). The chemical vapor deposition method starts with a small seed diamond, which is a small natural diamond fragment that can withstand extreme temperature and pressure conditions. Although many diamond fragments can be used as seed diamonds, the method usually starts with high-strength, high-grade diamond fragments as this is critical in the lab diamond manufacturing process. In the CVD method, the seed diamond is placed into a vacuum chamber, which is then filled with a carbon-rich gas. The vacuum chamber is made sure to fill with carbon-containing gas, and then heated to over 1,000 degrees Fahrenheit. The extreme temperature then turns the gas into a plasma. The plasma forms a diamond layer, resulting in a complete diamond at the end of the method, which can then be handled like a rough mined diamond.

[0003] Diamonds produced using the CVD method are generally of better quality than anything made from naturally mined diamonds. Another method of making synthetic diamonds is called HPHT. In this method, a pure carbon source is placed under high pressure and temperature. The extreme temperatures and enormous pressures cause the carbon to crystallize, forming a brand new diamond. It is well known that watch crystals (also known as dials) from luxury brands are often made from sapphire. Sapphire is an ideal material for watch crystals because the material is durable and has a pleasing aesthetic to the look of a luxury watch. While sapphire is durable, diamond is more scratch-resistant and can withstand greater pressure.

[0004] Therefore, there is a need for a method of manufacturing a watch crystal that employs a combination of diamond manufacturing techniques to facilitate the successful production of diamond watch crystals. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a watch crystal by a diamond growth process, wherein the method of the invention uses a chemical vapor deposition process in an initial step.

[0006] Another object of the present invention is to provide a method for growing diamond for use as a watch crystal, wherein the second step of the present invention places the diamond plate produced in the initial step in a high pressure and high temperature environment.

[0007] Another object of the present invention is to provide a method for manufacturing a watch crystal by a diamond growth process, wherein the additional step of the present invention comprises repeating the first two steps of the method of the present invention.

[0008] Another object of the present invention is to provide a method for growing diamond for use as a watch crystal, wherein another step of the method of the present invention uses microwave plasma assisted chemical vapor deposition.

[0009] Another object of the present invention is to provide a method of manufacturing a watch crystal by a diamond growth process which may alternatively employ a step involving hot-wire chemical vapor deposition.

[0010] Another object of the present invention is to provide a method for growing diamond for use as a watch crystal, wherein the method of the present invention can further use a step of using inductively coupled plasma enhanced chemical vapor deposition.

[0011] Another object of the present invention is to provide a method for manufacturing a watch crystal by a diamond growth process, wherein the method of the present invention also includes an alternative step of using direct current plasma enhanced chemical vapor deposition.

[0012] In order to achieve the above and related purposes, the present invention can be implemented in the form shown in the accompanying drawings. It should be noted that the drawings are only illustrative. Changes are considered part of the present invention and are limited only by the scope of the claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The present invention may be more fully understood with reference to the following detailed description and appended claims in conjunction with the accompanying drawings, in which:

[0014] Figure 1 Flow chart of the method of the present invention. DETAILED DESCRIPTION

[0015] Referring now to the accompanying drawings, wherein the various elements described are not necessarily drawn to scale and like elements are indicated by like reference numerals in the views and drawings, there is shown a method of manufacturing a watch crystal 100 constructed in accordance with the principles of the present invention.

[0016] One embodiment of the present invention is discussed herein with reference to the accompanying drawings. It will be appreciated by those skilled in the art that the detailed description of these drawings herein is for the purpose of explanation, and it is contemplated that alternative embodiments are feasible within the scope of the present invention. By way of example and not limitation, according to the teachings of the present invention, it will be appreciated by those skilled in the art that, in addition to the specific implementation selections in the embodiments described herein, a variety of alternatives and suitable methods of the functions of any given detail described herein can also be implemented according to the needs of a specific application. Various modifications and embodiments are within the scope of the present invention.

[0017] It should be further understood that the present invention is not limited to the specific methods, materials, uses and applications described herein, because they can change. In addition, it should also be understood that the terms used herein are only used for the purpose of describing specific embodiments, and are not intended to limit the scope of the present invention. It should be noted that, as used herein and in the claims, the singular forms "one / kind (a)", "one / kind (an)" and "the / said (the)" include plural references, unless the context clearly stipulates otherwise. Therefore, for example, a reference to "an element" is a reference to one or more elements, and includes equivalents known to those skilled in the art. All conjunctions used should be understood in the broadest sense as much as possible. Therefore, the word "or" should be understood as having a definition of logical "or", rather than a definition of logical "exclusive or (exclusive or)", unless the context clearly requires other definitions. The structure described herein should also be understood as referring to the functional equivalent of such a structure. Unless the context clearly stipulates otherwise, it can be interpreted as expressing an approximate language that should be understood in this way.

[0018] Reference to "one embodiment," "an embodiment," "exemplary embodiment," etc. may mean that embodiments of the invention may include particular features, structures, or characteristics, but not every embodiment must include the particular features, structures, or characteristics.

[0019] With particular reference to the accompanying drawings, Figure 1 The flow chart of FIG. 1 shows a method for manufacturing a watch crystal 100. It should be understood that within the scope of the present invention, the diamond crystal obtained by the method of the present invention can be produced in optional sizes, shapes and thicknesses. In step 101, the selection of starting materials is performed. It should be understood that within the scope of the present invention, ultra-high purity gases and high purity graphite are used as carbon sources. The gases used in the preferred embodiment of the present invention are hydrogen and methane. It should be understood that within the scope of the present invention, alternative gases can be used in the present invention and the desired results are obtained. In addition, within the scope of the present invention, alternative materials other than graphite or in combination with graphite are expected to be used as carbon sources. Step 103, start a chemical vapor deposition process. The chemical vapor deposition process is used to grow a thin diamond plate with a thickness of preferably 2-4 mm. It should be understood that within the scope of the present invention, the diamond plate can be manufactured to different thicknesses. In step 105, the graphite is placed in a vacuum chamber and the vacuum chamber is filled with a mixture of the above gases. Step 107, the vacuum chamber is heated to a temperature between 800 degrees Celsius and 1000 degrees Celsius.

[0020] In step 109, the material in the vacuum chamber is exposed to an energy source, wherein the energy source dissociates the gas molecules and forms a diamond layer on the graphite substrate. Within the scope of this energy source, alternative energy sources or alternative substrate materials can be considered. For example, a preferred energy source is microwave plasma, wherein the material in the chamber is exposed thereto. With this technology, microwaves are used to generate plasma, thereby decomposing a gas mixture containing carbon and hydrogen. The plasma provides sufficient energy to promote the growth of diamond crystals on the substrate. Alternatively, within the scope of the present invention, it is considered to use inductively coupled plasma as an energy source, wherein this technology uses inductively coupled plasma to generate high-energy plasma to promote the growth of diamond crystals. Another energy source that can be used is a direct current plasma energy source. Direct current plasma technology is used to generate plasma, which decomposes a gas mixture containing carbon and hydrogen, thereby promoting the growth of diamond crystals on the substrate. Finally, within the scope of the present invention, it is considered to use hot wire technology as an energy source. With this technology, a tungsten filament is heated to a high temperature, which causes a plasma to be generated in the vacuum chamber, which decomposes the gas mixture therein, wherein the carbon atoms generated are deposited on the substrate, and diamond crystals are grown on the substrate. It is further contemplated within the scope of the present invention to employ chemical vapor deposition or alternative forms of plasma-assisted techniques thereof in the present invention. For example, but not limited to, these may include thermal chemical vapor deposition, plasma-enhanced chemical vapor deposition, hot-wire chemical vapor deposition, and ultra-high vacuum chemical vapor deposition.

[0021] In step 111, steps 107 and 109 are repeated until the desired diamond plate thickness is obtained. In step 113, high pressure and high temperature treatment is started. In step 115, the diamond plate produced by step 111 is placed in a high pressure chamber together with a small diamond seed. In step 117, the chamber is heated to a temperature range between 1500 degrees Celsius and 2000 degrees Celsius. In addition, in this step, a pressure of up to 70,000 atmospheres is applied to the diamond plate placed in the chamber. This step causes the carbon atoms in the diamond plate to rearrange and form diamond crystals of the desired size. In step 119, steps 103 to 117 are repeated to obtain diamond crystals of the desired thickness and quality. Although chemical vapor deposition and high pressure and high temperature methods are used in the preferred embodiment of the present invention, it should be understood that within the scope of the present invention, the use of high pressure and high temperature methods may not be necessary, depending on the purity of the starting carbon source material. In addition, it should be understood that within the scope of the present invention, high pressure and high temperature treatment can be used alone and independently of chemical vapor deposition treatment. It should be understood that these steps can be repeated in alternating amounts. In step 121, the diamond plate produced by the method of the present invention is subjected to a final high pressure and high temperature step as described in step 117. This final high pressure and high temperature treatment can be used to remove any defects and / or impurities, thereby improving the quality of the final diamond crystal. In step 123, the diamond crystal is subjected to cutting and polishing, wherein the diamond crystal is cut and polished to a desired size and shape.

[0022] In the foregoing detailed description, reference has been made to the accompanying drawings which form a part of this document, in which specific embodiments in which the present invention can be practiced are shown by way of illustration. These embodiments and some variations thereof have been described in sufficient detail to enable those skilled in the art to practice the present invention. It should be understood that other suitable embodiments may be utilized and logical changes may be made without departing from the spirit or scope of the present invention. This description may omit certain information known to those skilled in the art. Therefore, the foregoing detailed description is not intended to be limited to the specific forms described herein, but rather, it is intended to cover these substitutions, modifications, and equivalents, as they may reasonably be included within the spirit and scope of the appended claims.

Claims

1. A method for manufacturing a diamond watch crystal, wherein the method comprises the following steps: selecting a starting material to produce a gas mixture and a high purity carbon source substrate, wherein the starting material consists of a high purity gas; initiating a chemical vapor deposition process, wherein the chemical vapor deposition process includes using a vacuum chamber; placing the substrate into the vacuum chamber; filling the vacuum chamber with the high purity gas; heating the vacuum chamber; exposing the starting material disposed in the vacuum chamber to an energy source; growing a diamond plate on the substrate to a target thickness; placing the diamond plate into a high pressure chamber, wherein the diamond plate is placed into the high pressure chamber together with a diamond seed crystal to perform a high pressure and high temperature treatment; heating the high pressure chamber, wherein the high pressure chamber is heated to about 1500 degrees Celsius to 2000 degrees Celsius; applying pressure to the high pressure chamber, wherein the high pressure chamber has applied thereto a pressure of up to 70,000 atmospheres; Repeating the chemical vapor deposition process and the high pressure and high temperature process to complete the production of diamond crystals; and Cutting and polishing the diamond crystal, wherein the diamond crystal is cut into a desired size and polished.

2. The method for manufacturing a diamond watch crystal according to claim 1, wherein the energy source consists of microwaves to generate plasma to decompose the gas mixture placed in the vacuum chamber.

3. The method for manufacturing a diamond watch crystal according to claim 1, wherein the energy source consists of direct current, wherein the direct current is used to generate a plasma that decomposes the gas mixture in the vacuum chamber.

4. The method for manufacturing a diamond watch crystal according to claim 1, wherein the energy source consists of an inductively coupled plasma, and the inductively coupled plasma is used to promote the growth of diamond crystals.

5. A method of manufacturing a diamond watch crystal according to claim 1, wherein the energy source is comprised of a tungsten filament, wherein the tungsten filament is heated to a temperature that produces a plasma operable to decompose the gas mixture in the vacuum chamber.

6. The method of manufacturing a diamond watch crystal according to claim 2, wherein the gas mixture consists of hydrogen and methane.

7. The method for manufacturing a diamond watch crystal according to claim 6, further comprising the step of repeating at least one complete cycle of chemical vapor deposition treatment and high temperature and high pressure treatment.

8. The method of manufacturing a diamond watch crystal according to claim 7, wherein the vacuum chamber is heated to a temperature between 800 degrees Celsius and 1000 degrees Celsius.

9. The method of manufacturing a diamond watch crystal according to claim 8, further comprising the step of performing a final high pressure and high temperature treatment, wherein the final high pressure and high temperature treatment is operable to remove impurities from the diamond watch crystal.

10. A method for manufacturing a diamond watch crystal, wherein the method comprises the following steps: selecting a starting material to produce a gas mixture and a high purity carbon source substrate, wherein the starting material consists of a high purity gas; initiating a chemical vapor deposition process, wherein the chemical vapor deposition process includes using a vacuum chamber; placing the substrate into the vacuum chamber; filling the vacuum chamber with the high purity gas; heating the vacuum chamber; exposing the starting material disposed in the vacuum chamber to an energy source; and A diamond plate is grown on the substrate to a target thickness.

11. The method of manufacturing a diamond watch crystal according to claim 10, wherein the energy source consists of direct current, wherein the direct current is used to generate a plasma that decomposes the gas mixture in the vacuum chamber.

12. The method of manufacturing a diamond watch crystal according to claim 10, wherein the energy source consists of an inductively coupled plasma, and the inductively coupled plasma is used to promote the growth of diamond crystals.

13. The method of manufacturing a diamond watch crystal according to claim 10, wherein the energy source is comprised of a tungsten filament, wherein the tungsten filament is heated to a temperature that produces a plasma operable to decompose the gas mixture in the vacuum chamber.

14. The method of manufacturing a diamond watch crystal according to claim 10, wherein the energy source consists of microwaves to generate plasma to decompose the gas mixture placed in the vacuum chamber.

15. A method for manufacturing a diamond watch crystal, wherein the method comprises the following steps: placing a diamond plate into a high pressure chamber, wherein the diamond plate is placed into the high pressure chamber together with a diamond seed crystal to perform a high pressure and high temperature treatment; heating the high pressure chamber, wherein the high pressure chamber is heated to about 1500 degrees Celsius to 2000 degrees Celsius; applying pressure to the high pressure chamber, wherein the high pressure chamber has applied thereto a pressure of up to 70,000 atmospheres; Repeating the high pressure and high temperature treatment to complete the production of diamond crystals; and Cutting and polishing the diamond crystal, wherein the diamond crystal is cut to a desired size and polished to complete the formation of the diamond watch crystal.