Method and device for synchronously depositing single-crystal diamond and polycrystalline diamond
By combining different growth mechanisms of single crystal and polycrystalline substrates and oxygen and argon auxiliary gases in the substrate table structure, the problem of low plasma utilization during single crystal diamond growth is solved, and high-efficiency and high-quality diamonds are achieved Co-deposition reduces costs and is suitable for semiconductor and thermal applications.
Patent Information
- Application Number
- CN202411042771.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-31
AI Technical Summary
When the prior art grows single crystal diamond, the plasma utilization rate is not high, resulting in high cost and inconsistent grain orientation, which cannot meet the application requirements of electronic devices.
Using a new substrate table structure, combining oxygen-assisted gas and bias power supply, through different growth mechanisms between single crystal and polycrystalline substrates, the single crystal surface step flow growth and polycrystalline surface competition growth are used to improve plasma Utilization, and through periodic oxygen etching and argon auxiliary gas, the substrate temperature and plasma distribution are regulated to achieve efficient and high-quality diamond co-deposition.
It improves plasma utilization, reduces single crystal growth cost, and realizes high-quality diamond co-deposition, suitable for semiconductor and heat dissipation applications.
Smart Images

Figure CN119020860A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of diamond single crystal and polycrystalline materials and their preparation, and relates to a method and device for growing diamond single crystals at a high rate by microwave plasma chemical vapor deposition. This method controls the substrate temperature of growing polycrystalline and single crystal by combining a deposition table in an external power supply heating mode with a bias power supply, so as to achieve the purpose of co-deposition of single crystal and polycrystalline; the present invention also provides a special substrate support structure for co-deposition of polycrystalline and single crystal, which can simultaneously control the temperature of single crystal substrate and polycrystalline substrate by setting different bottom heat dissipation structures for single crystal substrate and polycrystalline substrate, and combining the method of external power supply heating; in addition, the bias power supply connected to the substrate table will continuously provide bias to the substrate surface, guide ion bombardment, thereby improving the growth quality of single crystal and polycrystalline, and achieving the purpose of growing high-quality single crystal and polycrystalline. Background Art
[0002] The use of chemical vapor deposition (CVD) to grow polycrystalline diamond films on heterogeneous substrates was proposed in the early 1980s. Due to the low deposition cost of this method and the ability to deposit polycrystalline diamond films on a large area, the technology for heterogeneously growing polycrystalline diamond films has developed rapidly in recent years and has matured technically. However, due to factors such as inconsistent grain orientation caused by the competitive growth mechanism between grains, uneven temperature caused by heat dissipation on the substrate surface, different states of various locations under large-area distribution of plasma balls and differences in coupling with temperature, there are a large number of grain boundaries and defects in polycrystalline diamond films, which cannot meet the requirements of widespread application in electronic devices. After the invention of MPCVD equipment with higher energy density and purer chamber structure, the homoepitaxial single-crystalline diamond deposited by it is much higher in quality than polycrystalline diamond films. Most diamonds grown homoepitaxially using single-crystalline diamond as seed crystals are widely used in electronic application scenarios. However, due to the slow homoepitaxial growth rate of single crystal diamond, which is generally less than 5-10 microns / hour, single crystal diamond with a thickness of millimeters needs to grow continuously for more than 100-200 hours, which requires high stability of the growth system. In addition, due to the limitation of homoepitaxial growth mode, the seed size of single crystal diamond is small, and the plasma ball excited in the cavity of general MPCVD equipment cannot be fully utilized, which greatly increases the cost. In view of the problems existing in the development of homoepitaxial single crystal diamond, the traditional approach is to increase the growth rate of single crystal diamond by increasing process parameters such as methane concentration and temperature, but excessive methane concentration and temperature will cause excessive stress on the surface of single crystal diamond and produce defects. Another method is to increase the chamber pressure of microwave CVD equipment, compress the plasma ball area, and achieve high energy density in a small area to grow single crystal diamond at high speed. However, increasing the chamber pressure will cause the microwave plasma ball to become unstable, and the microwave CVD equipment maintained at the same temperature will reduce the power due to excessive chamber pressure, which is not conducive to the high-speed growth of single crystal diamond. In response to the above problems, Professor Wang Hongxing's team at Xi'an Jiaotong University (CN 112813497 B) used an auxiliary ring prepared from a polycrystalline sample to improve the temperature distribution on the surface of the single crystal sample during the deposition process, thereby achieving a method of high-speed growth. Li Hongdong et al. from Jilin University (CN100500951C) used a sample holder prepared from polycrystalline diamond and diamond powder to improve the stability of single crystal diamond during growth. Both methods reduce the cost of growing single crystals by increasing the growth rate of single crystals. Although effective, they do not fully utilize plasma by simply improving the efficiency of single crystal deposition. Another way is to achieve stable growth by changing the composition of the plasma ball or the discharge conditions. Element 6 increases the growth rate of single crystal diamond by adding nitrogen. Although the addition of nitrogen can accelerate the migration of atoms on the surface of the single crystal to the root of the step to form step growth, the doping of nitrogen changes the composition of diamond, making it difficult to grow high-purity semiconductor single crystal diamond.
[0003] Advanced single crystal diamond cost reduction technology requires not only efficient single crystal growth rate, but also high plasma utilization. Summary of the invention
[0004] The purpose of the present invention is to provide a method for co-deposition of single crystal and polycrystalline diamond, which utilizes a novel substrate table structure and oxygen as an auxiliary gas to achieve efficient and high-quality diamond co-deposition.
[0005] The present invention adopts the following technical scheme: a method for co-deposition of single crystal diamond and polycrystalline diamond, characterized in that a single crystal growth substrate is placed in the central area of an MPCVD substrate table, and a ring-shaped polycrystalline substrate is placed in the outer edge area; the different growth mechanisms of single crystal and polycrystalline are used in the growth process, single crystal diamond grows in a step flow formed by the movement of surface carbon atoms, and polycrystalline diamond grows in a competitive columnar crystal formed by multiple single crystals on the surface; the concentrations of carbon-containing groups in the microwave plasma required by the two are different, so the single crystal diamond in the central area of the plasma can be deposited together with the polycrystalline diamond in the edge area.
[0006] Furthermore, the substrate stage uses two structures for regulating the temperature of the edge polycrystalline substrate; the central area of the substrate stage structure is used to place the single crystal diamond seed crystal, and the outer area is used to place the silicon ring to deposit polycrystalline diamond, and the temperature of the silicon ring is ensured to be a suitable temperature for polycrystalline diamond deposition by regulating the channel area for heat dissipation below the polycrystalline deposition area. Oxygen is added during the deposition process to improve the quality of the deposited crystal, and the generation of graphite phase in polycrystalline deposition and edge polycrystalline in single crystal deposition is reduced by periodically applying bias oxygen etching to the substrate; the surface temperature of the polycrystalline substrate is set to a suitable growth temperature for diamond by adjusting the width of the heat dissipation groove below the polycrystalline substrate and adjusting the heating power of the resistance wire below the polycrystalline, so as to achieve the purpose of single crystal and polycrystalline co-deposition.
[0007] Furthermore, the bottom of the substrate table is connected to a bias power supply, which continuously outputs a negative bias voltage to the substrate surface during the co-deposition process of polycrystals and single crystals, guiding the positive ions in the plasma to continuously bombard the growth surfaces of the single crystals and polycrystals, providing energy for the step flow growth on the surface of the single crystal and the columnar crystal growth of the polycrystals, and removing the secondary nucleation grains on the surface of the single crystal and the graphite phase on the surface of the polycrystal.
[0008] Furthermore, the method for co-deposition of single crystal and polycrystalline diamond is characterized in that the co-deposition is a molybdenum support structure for co-deposition of polycrystalline and single crystal, the central single crystal substrate and the edge polycrystalline annular substrate are arranged together, and a growth method of cyclic etching by oxygen and bias power supply is combined through a resistance wire and a molybdenum support heat dissipation structure; argon is used as an auxiliary gas, oxygen etching is periodically introduced, and a negative bias is applied to the substrate to assist, and the specific steps are as follows:
[0009] Step 1: Use a mixed solution of sulfuric acid and nitric acid in a ratio of 1:3 and acetone to clean the single crystal diamond substrate in turn; use diamond particles with a particle size of 4-6 microns to grind the surface of the silicon ring substrate for 8-12 minutes until the surface is covered with tiny scratches;
[0010] Step 2: Place the single crystal diamond and silicon ring substrate in step 1 into the MPCVD device and introduce H2 / O2 plasma to etch surface defects;
[0011] Step 3: After step 2, adjust the chamber pressure and power of the MPCVD equipment until the growth temperature of the single crystal diamond substrate surface reaches 820-1000°C;
[0012] Step 4: After step 3 is completed, the temperature of the silicon substrate at the edge is heated to the growth temperature of polycrystalline diamond 850-1100°C by adjusting the power of the molybdenum support outer ring resistance wire, and methane and argon are introduced to start growth;
[0013] Step 5: After step 4 is completed, turn on the bias power supply connected to the substrate stage, set the output voltage of the bias power supply, and continuously apply a negative bias voltage to the substrate surface;
[0014] Step 6: During the growth of single crystal and polycrystalline after step 5, a certain amount of 1% oxygen is introduced into the chamber for etching at a cycle of 43-47 hours.
[0015] Furthermore, a novel substrate stage structure used in the present invention is a substrate stage structure connected to a bias power supply for co-deposition of polycrystalline diamond and single crystal diamond, such as Figure 1 As shown, the bias power supply is used to continuously apply bias to the substrate surface, which is used to guide positive ions in the plasma to bombard the substrate surface, wherein the central area of the substrate table is a single crystal grown substrate, and the edge area is a polycrystalline grown substrate.
[0016] Furthermore, the polycrystalline diamond substrate is in the shape of a processed ring, and the top view of the substrate table is as follows: Figure 2 As shown, the inner and outer diameters of the polycrystalline ring can be freely adjusted to deposit and grow polycrystalline diamond sheets that meet various size requirements. The substrate of the single crystal growth area in the center is a single crystal substrate, and the outer polycrystalline deposition substrate is a single crystal silicon ring.
[0017] Furthermore, a groove suspended from the molybdenum support is provided below the polycrystalline diamond substrate. The part of the silicon wafer in contact with the molybdenum support dissipates heat quickly, while the suspended part dissipates heat poorly, causing the overall temperature of the silicon wafer to increase. The heat dissipation of the polycrystalline substrate is changed by setting the groove width, so that the silicon substrate at the edge of the plasma ball reaches a suitable temperature.
[0018] Furthermore, the outer ring at the bottom of the molybdenum tray has a circle of resistance wire for heating. The function of this resistance wire is to assist the surface temperature of the polycrystalline substrate at the edge of the molybdenum tray to reach a suitable growth temperature through heating, improve the temperature uniformity of the center edge of the molybdenum tray, and ensure that the edge polycrystalline substrate reaches a suitable diamond growth temperature during the single crystal growth process.
[0019] Furthermore, the lower end of the substrate stage is connected to a bias power supply, which will output a negative bias voltage to the single crystal and polycrystalline substrates, attracting positive ions in the plasma ball to continuously bombard the substrate surface, thereby eliminating small polycrystalline particles generated during the growth process of the single crystal substrate surface and non-diamond phases generated during the growth process of the polycrystalline substrate surface.
[0020] The present invention provides a highly efficient method for co-deposition of polycrystalline and single crystal diamond and a special deposition table structure, so that different areas inside a chamber meet the deposition conditions of single crystal diamond and polycrystalline diamond at the same time, thereby improving the utilization rate of plasma in the chamber, reducing the cost of single crystal growth, and improving the efficiency of MPCVD synthetic diamond; wherein, high-quality single crystals are used for diamond semiconductor applications, while synchronously grown polycrystalline diamonds can be used for diamond heat dissipation applications, thereby providing an effective solution for preparing high-quality semiconductor diamonds and mass-producing heat dissipation-grade diamonds.
[0021] Advantages and functions of the present invention
[0022] 1. Innovation analysis
[0023] The innovations of the present invention are: 1. The plasma ball is not fully utilized during the growth of CVD single crystal diamond. By arranging a silicon ring for the growth of polycrystalline diamond on the edge of the molybdenum support, the concentration of carbon groups in the plasma required for the growth of polycrystalline diamond is less than that of single crystal diamond, thereby increasing the utilization efficiency of the plasma ball and saving costs.
[0024] 2. The edge of the molybdenum support is heated by the heat dissipation groove and the resistance wire to increase the temperature of the polycrystalline growth substrate in the edge area, solving the problem of excessive temperature difference between the center and the edge, so that single crystal diamond and polycrystalline diamond can be deposited at the same time.
[0025] 3. By using a bias power supply to apply a negative bias to the substrate surface, the positive ions in the plasma are guided to continuously bombard the substrate surface, and the non-diamond phase on the sample surface is continuously etched during the single crystal and polycrystalline co-deposition process, so as to achieve the purpose of growing high-quality single crystals and polycrystalline diamonds.
[0026] 4. During the co-deposition of single crystal and polycrystalline diamond, argon is introduced into the chamber as an auxiliary gas. Argon as an auxiliary gas can stabilize plasma groups, increase additional ionization in plasma reactions, provide high-quality argon ions to bombard the substrate surface, transfer energy to carbon-containing groups, provide higher energy for atomic migration of surface step growth, and improve the growth quality of single crystal diamond; in addition, the introduction of argon will expand the area of the plasma ball, expand the MPCVD deposition area, and improve the edge polycrystalline diamond deposition efficiency.
[0027] 5. During the co-deposition process of single crystals and polycrystalline, oxygen is periodically introduced into the chamber as an auxiliary gas. Oxygen as an auxiliary gas can etch defects in diamond and graphite, thereby ensuring high deposition efficiency while improving the quality of diamond crystals.
[0028] The beneficial effects of the present invention and the prior art are:
[0029] (1) The present invention designs a substrate support structure and growth method for depositing single crystal diamond and polycrystalline diamond together. Compared with the original single crystal diamond deposition method, the present invention has higher plasma utilization, lower cost and higher diamond output, and effectively provides a solution for the mass production of single crystal and polycrystalline diamond.
[0030] (2) The present invention improves the plasma deposition capability by introducing argon and oxygen cyclic etching auxiliary bias applied to the MPCVD system for single crystal and polycrystal co-deposition. The periodic etching auxiliary bias promotes the step flow growth on the single crystal surface and the columnar crystal growth on the polycrystal surface, thereby improving the quality of the deposited diamond crystal.
[0031] The present invention designs a substrate holder structure for single crystal and polycrystal co-deposition, combines negative bias, assists argon and oxygen, and performs cyclic etching on the substrate to improve diamond deposition efficiency and crystal quality, thereby providing an efficient solution for mass production of semiconductor single crystal diamond and polycrystalline diamond. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the structure of a single crystal and polycrystal co-deposition platform;
[0033] Figure 2 It is a schematic diagram of the top view of the single crystal and polycrystal co-deposition platform;
[0034] Figure 3 Schematic diagram of the single crystal and polycrystal co-deposition process;
[0035] Figure 4 Schematic diagram of atomic migration on the growth step surface of single crystal diamond;
[0036] Figure 5 Schematic diagram of competitive growth of columnar crystals on the surface of polycrystalline diamond;
[0037] Figure 6 Schematic diagram of the surface morphology of single crystal diamond growth;
[0038] Among them: 1. Polycrystalline diamond substrate holder; 2. Polycrystalline diamond heat sink; 3. Resistance wire heater; 4. Single crystal diamond substrate holder; 5. Bias power supply; 6. Resistance heating wire power supply; 7. Plasma ball under bias state; 8. Polycrystalline substrate; 9. Single crystal substrate; 10. Single crystal step surface atoms; 11. Polycrystalline surface columnar crystals; 12. Polycrystalline internal columnar crystals; 13. Polycrystalline surface graphite phase defects; 14. Single crystal diamond secondary nucleation grains. (There is no reference number 14 in the attached figure)
[0039] Among them: the size of the deposition table is 3 inches in diameter, and the inner diameter of the polycrystalline diamond ring can be adjusted from 2 inches to 70 mm. This distance depends on the ratio of the deposited single crystal diamond and polycrystalline diamond areas. DETAILED DESCRIPTION
[0040] Implementation steps
[0041] A method of co-deposition of single crystal and polycrystalline diamond of the present invention is as follows:
[0042] Step 1: Use a mixed solution of sulfuric acid and nitric acid (1:3) and acetone to clean the single crystal diamond substrate and the polycrystalline diamond substrate in turn.
[0043] Step 2: Place the single crystal diamond and polycrystalline diamond substrates prepared in step 1 into an MPCVD device and introduce H2 / O2 plasma to etch surface defects;
[0044] Step 3: After step 2 is completed, turn on the power supply of the resistance heating wire, adjust the heating power of the resistance wire, and measure the surface temperature of the polycrystalline ring substrate at the same time;
[0045] Step 4: After step 3, apply negative bias to the substrate and introduce argon / methane / hydrogen (1 / 5 / 100)
[0046] Step 5: After step 4 is completed, the power of the resistance heating wire is adjusted so that the polycrystalline substrate and the single crystal diamond substrate reach the diamond deposition temperature at the same time;
[0047] Step 6: Adjust the oxygen flow rate during the growth process, periodically introduce 1% oxygen every 45 hours, and turn off the oxygen after etching for 10 minutes.
[0048] 1. Device structure and function
[0049] The device and its functions of the present invention are described below with reference to the accompanying drawings and specific examples.
[0050] The embodiment of the present invention discloses a molybdenum support structure and growth method for co-deposition of single crystal diamond and polycrystalline diamond, including a single crystal diamond substrate support 4 arranged at the center of the molybdenum support and a polycrystalline diamond substrate support 1 around it. Figure 1 As shown, the heat sink 2 and the heating resistor 3 arranged below the polycrystalline substrate holder, as well as the resistor power supply 6 for regulating the temperature of the resistor, increase the temperature of the polycrystalline substrate by affecting heat dissipation and active heating.
[0051] The top view of the co-deposition support of the single crystal and polycrystalline diamond is shown in Figure 2 As shown, the single crystal substrate is square and the polycrystalline substrate is ring-shaped.
[0052] The bias power supply 5 for applying a negative bias voltage to the substrate surface applies a negative bias voltage to the surface of the single crystal substrate and the polycrystalline substrate during the deposition process. Figure 3 As shown, it includes: a single crystal diamond substrate 9, a polycrystalline diamond substrate 8, and a plasma 7 under applied bias.
[0053] Taking Ib-type single crystal diamond and (100) oriented single crystal silicon ring as single crystal and polycrystalline diamond substrate materials respectively, the surface roughness is ≤1nm. Before use, the surface is cleaned with a mixed solution of sulfuric acid and nitric acid in a volume ratio of 1:3. Then, they are cleaned and dried with acetone, alcohol, and deionized water respectively. The single crystal diamond substrate 9 and the polycrystalline diamond ring substrate 8 are placed in an MPCVD device with a bias power supply, and a 1% concentration of O2 / H2 plasma is first introduced to etch the surface and subsurface defects for 2h, and then placed on a CVD sample growth table for enhanced bias nucleation, with a negative voltage of -500V. The single crystal diamond substrate 9 and the polycrystalline diamond ring substrate 8 are placed in the MPCVD for growth, and the growth process is: gas pressure 100Torr, gas flow rate 500sccm, CH4 / H2=5%, 1% Ar is introduced, the substrate temperature is 900℃, and a negative bias is continuously applied to the substrate during the growth process, and the negative voltage is -50V.
[0054] During the growth process, the surface of the single crystal diamond transfers energy to the carbon-containing groups due to electrons and positive ions. The energy provided by the electrons causes the atoms 10 on the step surface to continue to migrate to the bottom of the step, forming step flow growth. The growth mechanism of the polycrystalline diamond surface is a columnar growth mode formed by the competition of multiple single crystal diamonds 11. The difference between the two growth modes is that the step flow growth of the single crystal requires a dense arrangement at the atomic level to proceed, so the number of carbon-containing groups that need to be dissociated is large, and the carbon atoms provided are sufficient for dense arrangement at the atomic level. The polycrystalline is a columnar crystal growth mode formed by the competition of multiple single crystals 11. In this mode, the single diamond crystal does not need to grow completely. The growth of the polycrystalline diamond is composed of the fastest growing single crystal diamond 11, and the single crystal diamond 12 with a slower growth rate will be covered by other crystals. Therefore, the dense arrangement during the growth of the polycrystalline diamond is more macroscopic than that of the single crystal diamond. It is a dense arrangement at the crystal level, which can allow the appearance of holes. Therefore, the concentration of carbon-containing groups required for the growth of the polycrystalline diamond is less than that of the single crystal diamond. Therefore, this substrate configuration with a single crystal center and polycrystalline edges can ensure that the carbon-containing group concentration required for the growth of single crystal diamond and polycrystalline diamond is consistent with the plasma distribution, effectively improving the efficiency of diamond deposition. And the surface is continuously bombarded by positive and negative ions in the plasma, such as Figure 3 As shown in FIG. 1 , continuous positive ion bombardment removes fine grains 14 on the surface of the single crystal. Figure 6 The graphite phase and the black defect 13 on the surface of the polycrystalline have a certain etching effect, which improves the quality of crystal growth.
[0055] During the co-deposition process of single crystal and polycrystalline diamond, oxygen with a flow rate of 3 sccm is introduced into the chamber for 10 minutes every 40 hours. The introduction of oxygen has a strong etching effect on the surface of single crystals and polycrystalline crystals, and has a stronger etching effect on larger defects and graphite phases. In order not to affect the growth rate of diamond single crystals and polycrystalline crystals, oxygen is introduced once every 40 hours. By intermittently introducing oxygen etching, the methane concentration can be appropriately increased, thereby improving the quality of the grown single crystals and polycrystalline crystals while maintaining a higher growth rate.
Claims
1. A method for co-deposition of single crystal and polycrystalline diamond, characterized in that: A single crystal growth substrate is placed in the central area of the MPCVD substrate table, and a ring-shaped polycrystalline substrate is placed in the outer edge area. The different growth mechanisms of single crystal and polycrystalline are utilized during the growth process. Single crystal diamond grows as a step flow formed by the movement of surface carbon atoms, while polycrystalline diamond grows as a columnar crystal formed by multiple single crystals on the surface. The concentration of carbon groups in the microwave plasma required for the two is different, so the single crystal diamond in the central area of the plasma can be deposited together with the polycrystalline diamond in the edge area.
2. The method for co-deposition of single crystal and polycrystalline diamond according to claim 1, characterized in that: The substrate stage adopts two structural settings for regulating the temperature of the edge polycrystalline substrate; the central area of the substrate stage structure is used to place the single crystal diamond seed crystal, and the outer area is used to place the silicon ring to deposit polycrystalline diamond, and the temperature of the silicon ring is ensured to be a suitable temperature for polycrystalline diamond deposition by regulating the groove area used for heat dissipation below the polycrystalline deposition area; oxygen is added during the deposition process to improve the quality of the deposited crystal, and the generation of graphite phase in polycrystalline deposition and edge polycrystalline in single crystal deposition is reduced by periodically applying bias oxygen etching to the substrate; the surface temperature of the polycrystalline substrate is set to a suitable growth temperature for diamond by adjusting the width of the heat dissipation groove below the polycrystalline substrate and adjusting the heating power of the resistance wire below the polycrystalline, so as to achieve the purpose of single crystal and polycrystalline co-deposition.
3. The method for co-deposition of single crystal and polycrystalline diamond according to claim 2, characterized in that: The bottom of the substrate table is connected to a bias power supply, which continuously outputs a negative bias voltage to the substrate surface during the co-deposition process of polycrystals and single crystals, guiding the positive ions in the plasma to continuously bombard the growth surfaces of the single crystals and polycrystals, providing energy for the step flow growth on the surface of the single crystal and the columnar crystal growth of the polycrystals, and removing the secondary nucleation grains on the surface of the single crystal and the graphite phase on the surface of the polycrystal.
4. The method for co-deposition of single crystal and polycrystalline diamond according to claim 1, characterized in that: Co-deposition is a molybdenum support structure in which polycrystalline and single crystal are co-deposited. The central single crystal substrate and the edge polycrystalline annular substrate are set together. The growth method of cyclic etching of oxygen and bias power supply is combined through the heat dissipation structure of the resistance wire and the molybdenum support; argon is used as the auxiliary gas, oxygen etching is periodically introduced, and the substrate assists in applying a negative bias. The specific steps are as follows: Step 1: Use a mixed solution of sulfuric acid and nitric acid and acetone to clean the single crystal diamond substrate in sequence; use diamond particles with a particle size of 4-6 microns to grind the surface of the silicon ring substrate for 8-12 minutes until the surface is covered with tiny scratches; Step 2: Place the single crystal diamond and silicon ring substrate in step 1 into the MPCVD device and introduce H2 / O2 plasma to etch surface defects; Step 3: After step 2, adjust the chamber pressure and power of the MPCVD equipment until the growth temperature of the single crystal diamond substrate surface reaches 820-1000°C; Step 4: After step 3 is completed, the temperature of the silicon substrate at the edge is heated to the growth temperature of polycrystalline diamond 850-1100°C by adjusting the power of the molybdenum support outer ring resistance wire, and methane and argon are introduced to start growth; Step 5: After step 4 is completed, turn on the bias power supply connected to the substrate stage, set the output voltage of the bias power supply, and continuously apply a negative bias voltage to the substrate surface; Step 6: During the growth of single crystal and polycrystalline after step 5, a certain amount of 1% oxygen is introduced into the chamber for etching at a cycle of 43-47 hours.
5. The method for co-deposition of single crystal and polycrystalline diamond according to claim 2, characterized in that: The substrate table structure is a substrate table structure connected to a bias power supply on which polycrystalline diamond and single crystal diamond are deposited together, wherein the bias power supply is used to continuously apply a bias voltage on the substrate surface, and this method is used to guide positive ions in the plasma to bombard the substrate surface. The central area of the substrate table is a single crystal grown substrate, and the edge area is a polycrystalline grown substrate.
6. The method for co-deposition of single crystal and polycrystalline diamond according to claim 5, characterized in that: The polycrystalline diamond substrate is in the shape of a processed ring, and the inner and outer diameters of the polycrystalline ring can be freely adjusted to deposit and grow polycrystalline diamond sheets that meet various size requirements. The substrate of the single crystal growth area in the center is a single crystal substrate, and the outer polycrystalline deposition substrate is a single crystal silicon ring.
7. The method for co-deposition of single crystal and polycrystalline diamond according to claim 5, characterized in that: A groove suspended from the molybdenum support is provided below the polycrystalline diamond substrate. The part of the silicon wafer in contact with the molybdenum support dissipates heat quickly, while the suspended part dissipates heat poorly, causing the overall temperature of the silicon wafer to rise. The heat dissipation of the polycrystalline substrate is changed by setting the groove width, so that the silicon substrate at the edge of the plasma ball reaches a suitable temperature.
8. The method for co-deposition of single crystal and polycrystalline diamond according to claim 7, characterized in that: The outer ring at the bottom of the molybdenum tray has a circle of resistance wire for heating. The function of this resistance wire is to assist the surface temperature of the polycrystalline substrate at the edge of the molybdenum tray to reach a suitable growth temperature through heating, improve the temperature uniformity of the center edge of the molybdenum tray, and ensure that the edge polycrystalline substrate reaches a suitable diamond growth temperature during the single crystal growth process.
9. The method for co-deposition of single crystal and polycrystalline diamond according to claim 5, characterized in that: The lower end of the substrate stage is connected to a bias power supply, which outputs a negative bias voltage to the single crystal and polycrystalline substrates, attracting positive ions in the plasma ball to continuously bombard the substrate surface, thereby eliminating small polycrystalline particles generated during the growth of the single crystal substrate surface and non-diamond phases generated during the growth of the polycrystalline substrate surface.
Citation Information
Patent Citations
Method for preparing diamond films by adopting microwave plasma chemical vapor deposition method
CN107164740A
Large-size single-crystal diamond heteroepitaxial growth method
CN111088523A
Method for batch production of diamond single crystals through MPCVD method and molybdenum substrate table
CN114561698A
Method for growing monocrystal diamond through periodic amplitude and pulse width modulation space-time energy
CN118007235A
Preparation method of diamond composite heat dissipation substrate
CN118256992A