Superfine fiber porous material based on electrostatic air jet spinning and preparation method thereof

Through the wet-vapor-induced jet phase separation technology combining high-pressure static electricity and high-speed vortex airflow, the problems of low production efficiency and single morphology of microfiber materials are solved, and the preparation of microfiber porous materials with adjustable porosity and excellent mechanical properties is realized. Expand its application scope.

CN119020919AActive Publication Date: 2024-11-26DONGHUA UNIV

Patent Information

Application Number
CN202411182155.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The prior art has low production efficiency, single material form and poor mechanical properties when preparing microfiber materials, which limits its wide application in the fields of high temperature heat insulation, cold protection and warmth, filtration, sound absorption, etc.

Method used

Wet-var induced jet phase separation technology combining high-pressure static electricity and high-speed vortex airflow can accurately regulate the different curvature and entanglement levels of fibers by regulating the wet-var concentration and airflow velocity, and then combine or spray heat The rolling process reinforces the fiber connection and prepares porous microfiber materials with adjustable porosity.

Benefits of technology

It significantly improves the production speed and mechanical properties of microfiber porous materials, achieves precise control of porosity, and broadens its application potential in the fields of heat insulation, filtration, and warmth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020919A_ABST
    Figure CN119020919A_ABST
Patent Text Reader

Abstract

The invention relates to a superfine fiber porous material based on electrostatic gas jet spinning and a preparation method thereof, and belongs to the technical field of superfine fiber materials.The preparation method comprises the steps that firstly, a prepared spinning solution is conveyed to a variable-frequency temperature control device to be stored, then the spinning solution is poured into an electrostatic gas jet spinning device, and under the double-field action of an electric field and an airflow field, the electrostatic gas jet spinning device conducts electrostatic spinning; the preparation method comprises the following steps: carrying out jet flow drafting refining-whipping curling, carrying out rapid phase separation through wet steam induced jet flow, fixing the curling form of fibers to obtain a fiber aggregate material which is a fiber membrane or fiber flocculus, and finally carrying out fusion welding compounding / glue spraying hot rolling and drying shaping on the fiber aggregate material to obtain the superfine fiber porous material. Compared with the prior art, the method has the advantages that efficient preparation of the superfine fiber porous material is realized on the basis of electrostatic air jet spinning, and meanwhile, the porosity of the superfine fiber porous material can be accurately regulated and controlled by adopting the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultrafine fiber materials, and in particular to an ultrafine fiber porous material based on electrostatic air spinning and a preparation method thereof. Background Art

[0002] Ultrafine fibers have the advantages of small diameter and high specific surface area, which makes the materials made of them have many properties superior to conventional fiber materials, such as high porosity, light weight and softness, etc., and have great application potential in high-temperature insulation, cold protection, filtration and separation. The main methods for preparing ultrafine fibers are melt-blown spinning, centrifugal spinning, air-blowing and other methods. Among them, the diameter of fibers prepared by melt-blown spinning is mostly between 2 and 10 μm, and it is difficult to further refine, which limits the wide application of this method. The high-speed rotation of the centrifuge during the centrifugal spinning process will cause fiber breakage, so the product continuity is poor; the air-blowing method is difficult to control the airflow state during the preparation of fibers, which can easily make the fiber diameter and morphology vary greatly, affecting the quality of fiber products.

[0003] Electrostatic air-jet spinning technology is a technology that adds an air-jet device to electrostatic spinning, so that the jet is quickly stretched under the action of electrostatic force and air flow force at the same time to achieve efficient preparation of ultrafine fibers. Among them, high-voltage static electricity not only stretches and refines the jet, but also stabilizes the jet state. High-speed airflow further increases the fiber production rate. However, after adding the air-jet device, only fiber membranes can be prepared, and fluffy fiber flakes cannot be prepared in one step. Fiber flakes can only be formed by stacking and laying the net multiple times through post-processing technology, and the process is complicated.

[0004] In response to the above problems, researchers have conducted relevant research in this field. Patent ZL201811009580.5 sets an airflow nozzle in the center of the nozzle and multiple spinning nozzles at the edge of the nozzle, and uses the central airflow to simultaneously stretch the jets ejected from multiple spinning nozzles, which can easily lead to the phenomenon of clustering between fibers and thus affect the product quality; Patent ZL201210037687.7 sets the spinneret hole coaxially inside the pore, and prepares a polysulfoneamide nanofiber web by enhancing the jet stretching effect through airflow. This method can only enhance the stretching effect of the jet through airflow, and can only form a dense fiber web material, but cannot regulate the fiber molding structure and the morphology of the fiber assembly material; Patent ZL202210470343.9 uses electrospinning to prepare nanofibers while using flash spinning to prepare micron fibers, and uses the counter-reverse airflow to make the fibers entangled, curled and interpenetrated. In this method, two spinnerets produce filaments at the same time, the devices are easy to interfere with each other, and the curling shape of the fiber is difficult to fix, and the shape of the final material cannot be adjusted; Patent ZL201410667969.4 discloses a method and device for producing polymer nanofibers by high-speed airflow and high-voltage electrostatics, which utilizes double-layer high-speed airflow and high-voltage electrostatics to quickly transport and high-speed stretch the polymer solution, thereby increasing the electrospinning rate and realizing the rapid preparation of polymer nanofibers. However, this device transports the polymer spinning solution by the siphon effect generated by the pressure difference between the double-layer high-speed airflows. The interference between the double-layer high-speed airflows in different spinning nozzles is difficult to eliminate, and the prepared fiber material has poor morphology and a single style, which is difficult to meet product needs. Summary of the invention

[0005] The purpose of the present invention is to provide a superfine fiber porous material based on electrostatic air spinning and a preparation method thereof in order to overcome at least one of the defects of the above-mentioned prior art. The present invention realizes efficient preparation of superfine fiber porous materials based on electrostatic air spinning. At the same time, the method of the present invention can realize precise control of the porosity of superfine fiber porous materials, which is specifically embodied in:

[0006] Although the existing technology can produce ultrafine fibers, it is difficult to improve its production efficiency, which greatly limits the actual production needs. The present invention uses high-voltage static electricity to stretch the spinning solution, and adds a high-speed vortex airflow to quickly drive the spinning solution to spray, greatly improving the production speed.

[0007] Although the existing technology can prepare ultrafine fiber porous materials, the material form is single and usually only exists in the form of a film. The present invention proposes moisture-induced jet phase separation, which controls the phase separation solidification speed of the charged jet and cooperates with the high-speed blowing vortex airflow to achieve precise control of ultrafine fiber curling rates and entanglement degrees, and obtain dense fiber membranes or fluffy fiber flakes, which can effectively broaden the application of ultrafine fiber porous materials in the fields of heat insulation, filtration, warmth retention, sound absorption, etc.

[0008] Existing ultrafine fiber porous materials are easy to peel off between layers and have poor mechanical properties, which limits their practical applications. The present invention designs a welding composite / spraying hot rolling and drying and shaping process to enhance the physical connection between fibers, making the ultrafine fiber porous material not easy to delaminate and having good compression resilience and tensile fracture strength.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] One of the purposes of the present invention is to provide a method for preparing ultrafine fiber porous material based on electrostatic air spinning, comprising the following steps:

[0011] S1. Prepare spinning solution; adjust the stirring speed according to the solution viscosity before adding raw materials each time to ensure rapid dissolution and reaction of raw materials; at the same time, set a variable frequency temperature control device to adjust the solution viscosity and dispersion state by real-time control of the temperature of the reaction system to ensure long-term stable storage of the spinning solution;

[0012] S2. A choke rod is arranged at the coaxial nozzle to cross the air outlet, and a receiving plate is arranged opposite to the outlet of the coaxial nozzle; the spinning solution is extruded through the coaxial nozzle, and a jet is formed under the action of high-voltage static electricity. At the same time, the airflow passes through the choke rod to form a vortex airflow, which drives the charged jet to perform high-speed drafting and whip curling. The size of the vortex can be changed by adjusting the airflow speed, thereby adjusting the curling amplitude and shape of the jet;

[0013] S3, setting a constant temperature and humidity control device, by adjusting the moisture concentration in the spinning area, controlling the phase separation and solidification speed of the jet, fixing the different forms of the jet, thereby changing the form and entanglement degree of the fiber; when the jet slowly separates, straight fibers are obtained to form a fiber membrane; when the jet quickly separates, curly fibers are obtained, and the curly fibers are entangled with each other to form a three-dimensional interlocking structure to form a fiber flake;

[0014] S4. When the product obtained in S3 is a fiber membrane, the fiber membrane is placed under high temperature to allow the fibers to be fused and composited, and then dried and shaped to obtain an ultrafine fiber porous membrane, which is an ultrafine fiber porous material; or, when the product obtained in S3 is a fiber flake, the surface of the fiber flake is sprayed with glue and hot rolled, and then dried and shaped to obtain an ultrafine fiber flake material, which is an ultrafine fiber porous material.

[0015] More specifically, the phase separation state of the jet can be confirmed by turbidity titration of the spinning solution at different humidity. Under high humidity concentration (>80%), obvious phase separation occurs within 30 seconds, and the phase separation speed is fast; under low humidity concentration (<50%), phase separation will not occur until more than 130 seconds, and the phase separation speed is slow. Since the fiber formation speed is very fast during the electrospinning process and the jet specific surface area is large, the solution with fast phase separation will phase separate within a few milliseconds after being ejected during the spinning process.

[0016] More specifically, the present invention is provided with a constant temperature and humidity control device, which includes a wet steam conveying pipeline, a wet steam outlet, a temperature and humidity sensor, an air pump, and a temperature and humidity control / feedback adjustment system; the temperature and humidity control / feedback adjustment system sets the required spinning temperature and humidity, and the wet steam is pressurized by the air pump, conveyed to the wet steam outlet through the wet steam conveying pipeline and evenly dispersed to the spinning area; during the spinning process, the temperature and humidity sensor monitors the temperature and humidity changes in the area in real time, and feeds back to the temperature and humidity control / feedback adjustment system to maintain the regional temperature and humidity constant; by adjusting the wet steam concentration in the spinning area, the phase separation and solidification speed of the jet is controlled, and the different forms of the jet are fixed, thereby changing the morphology and entanglement degree of the fiber.

[0017] Furthermore, the spinning solution of the ultrafine fiber porous material includes a raw material and a solvent for dissolving the raw material, and the concentration of the raw material is 10 to 60 wt%;

[0018] The raw material is selected from one or more of polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, polymethyl methacrylate, polytrimethylene terephthalate, polystyrene, polyurethane, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polyethylene, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyamide, polyamideimide, polyvinyl alcohol, polyvinyl butyral, polysulfone, polyethyleneimine, polyimide, aramid 1313, titanium tetramethoxide, titanium tetraethoxide, titanium n-propoxide, titanium isopropoxide, titanium n-butoxide, titanium isobutoxide, tetraethyl orthosilicate, titanium tert-butoxide, titanium tetrapentoxide, titanium isooctoxide, zirconium tetramethoxide, zirconium tetraethoxide, zirconium n-propoxide, zirconium isopropoxide, zirconium n-butoxide, zirconium isobutoxide, zirconium tert-butoxide, zirconium tetrapentoxide, trimethoxyaluminum, triethoxide, tri-n-propoxyaluminum, aluminum isopropoxide, aluminum n-butoxide, aluminum sec-butoxide or aluminum tert-butoxide;

[0019] The solvent is selected from one or more of water, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, formic acid, acetic acid, dimethyl sulfoxide, toluene, acetone, cyclohexane, isobutanol, dichloromethane, butyl acetate, ethyl acetate, chloroform, methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol, glycerol, carbon tetrachloride, benzene, toluene, dichloroethane, dichloromethane, chloroform, ether, diphenyl ether, ethyl acetate, acetone, tetrahydrofuran, N-methylpyrrolidone or N,N-dimethylformamide.

[0020] Further, the raw material is selected from one or more of polyurethane, titanium n-butoxide, polysulfone or tetraethyl orthosilicate; the solvent is selected from one or more of N,N-dimethylformamide, water or ethanol. Further, in S2, the spinning solution forms a jet under 0-150kV electrostatic action; the speed of the air flow is 0-25m / s; the receiving distance between the coaxial nozzle and the receiving plate is 10-70cm; the injection speed of the coaxial nozzle outlet is 5-80ml / h.

[0021] Furthermore, in S3, the spinning temperature of the spinning area is 10-50° C., the relative humidity of the environment is 10-99%, and the fiber curling rate is 5-60%.

[0022] Furthermore, in S4, the welding method of the welding composite is one or more of heat welding, ultrasonic welding, microwave irradiation welding, infrared irradiation welding, ultraviolet irradiation welding, electron beam irradiation welding, and plasma irradiation welding, the heating roller temperature is 20 to 800°C, and the microwave generator frequency is 3000 to 300000 MHz.

[0023] Furthermore, in S4, during the glue spraying hot rolling process, the glue spraying atomizing nozzle used has a glue spraying amount ranging from 0 to 50 mL / min, and a diameter of the atomized glue is 1 to 10 μm.

[0024] Furthermore, in S4, during the drying and shaping process, the ultrafine fiber porous material is post-treated with dry hot air and cold air, the temperature range of the hot air is 40-150° C., the temperature range of the cold air is 5-20° C., and the suction pressure is 0.1-10 MPa.

[0025] The second object of the present invention is to provide an ultrafine fiber porous material based on electrostatic air spinning, which is prepared by the preparation method as described above.

[0026] Furthermore, the ultrafine fiber porous material is an ultrafine fiber porous membrane or an ultrafine fiber flake material;

[0027] When the ultrafine fiber porous material is an ultrafine fiber porous membrane:

[0028] In the present invention, the thickness of the ultrafine fiber porous membrane is 0.1 to 2 mm;

[0029] In the present invention, the porosity of the ultrafine fiber porous membrane is 20 to 90%;

[0030] In the present invention, the tensile strength of the ultrafine fiber porous membrane is higher than 5MPa;

[0031] In the present invention, the diameter of the ultrafine fiber porous membrane is 50 to 10000 nm;

[0032] When the ultrafine fiber porous material is an ultrafine fiber flake material:

[0033] In the present invention, the thickness of the ultrafine fiber flake material is 5 to 60 mm;

[0034] In the present invention, the volume density of the ultrafine fiber flake material is 2 to 100 mg / cm 3 ;

[0035] In the present invention, the porosity of the ultrafine fiber flake material is higher than 95%;

[0036] In the present invention, the compression resilience of the ultrafine fiber flake material is above 90%;

[0037] In the present invention, the elongation at break of the ultrafine fiber flake material is higher than 10%;

[0038] In the present invention, the diameter of the ultrafine fiber flake material is 50 to 10000 nm.

[0039] The technical principles of the present invention are as follows:

[0040] The ultrafine fiber porous material with adjustable porosity is prepared by the method of spinning raw materials through spinning solution configuration, electrostatic air jet spinning, jet phase separation solidification fiberization and welding composite / spray glue hot rolling-drying and shaping.

[0041] Long-term stable storage of spinning solution: First, the dissolved spinning solution is transported to a closed tank, and the temperature of the system is controlled in real time to adjust the viscosity and dispersion state of the spinning solution, so that the gelation behavior of the spinning solution is inhibited, thereby obtaining a spinning solution that can be stored stably for a long time.

[0042] Phase separation molding of ultrafine fibers: The spinning solution is extruded through the nozzle, and a jet is formed under the dual effects of high-voltage static electricity and high-speed airflow. At the same time, the vortex formed by the airflow passing through the baffle rod can drive the jet to perform high-speed drawing and whip curling, thereby forming jets with different morphological structures (straight or curled); at the same time, a constant temperature and humidity control device is set up to control the phase separation and curing speed of the jet by adjusting the moisture concentration, and at the same time, the size of the vortex is adjusted. When the jet is rapidly phase-separated and solidified, the curling shape of the jet can be quickly fixed to obtain curled fibers and form ultrafine fiber flake materials with high porosity; when the jet is slowly phase-separated, the curing speed of the jet slows down to obtain straight fibers and form ultrafine fiber membrane materials with low porosity. Therefore, the moisture-induced phase separation molding technology can change the curling and entanglement structure of the fiber and obtain fiber aggregate materials (fiber flakes or fiber membranes) with different porosities.

[0043] Strengthening and shaping of ultrafine fiber porous materials: The ultrafine fiber membrane material is welded and composited, the ultrafine fiber flake material is sprayed with glue and hot rolled, and then dried and shaped, finally obtaining an ultrafine fiber porous material with adjustable porosity and high strength.

[0044] Compared with the prior art, the present invention has the following advantages:

[0045] (1) The coaxial nozzle of the present invention is designed with a flow blocking rod that crosses the air outlet, and the prepared spinning solution is placed in the spinning module to quickly form fibers. At the same time, high-speed airflow and phase separation molding technology are used to control the curling degree and entanglement morphology of the fibers. According to the porosity of the ultrafine fiber material and application requirements, it is welded, composited or sprayed with glue and hot rolled, and finally dried and shaped. This method can obtain ultrafine fiber porous materials with adjustable porosity and good mechanical properties, which broadens the application scenarios of ultrafine fiber materials.

[0046] (2) The present invention can use different types of polymers or inorganic spinning solutions for efficient spinning, covering both organic and inorganic spinning solution systems. The method has strong versatility and a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 It is an overall schematic diagram of the constant temperature and humidity control device of the present invention;

[0048] As shown in the figure: 1-wet steam conveying pipeline, 2-wet steam outlet, 3-spinneret, 4-temperature and humidity sensor, 6-air pump, 7-temperature and humidity control / feedback adjustment system. DETAILED DESCRIPTION

[0049] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0050] Figure 1 It is an overall schematic diagram of the constant temperature and humidity control device used in the following embodiments, which includes a moisture conveying pipeline 1, a moisture outlet 2, a temperature and humidity sensor 4, an air pump 6, and a temperature and humidity control / feedback adjustment system 7; the temperature and humidity control / feedback adjustment system 7 sets the required spinning temperature and humidity, and the moisture is pressurized by the air pump 6, and is conveyed to the moisture outlet 2 through the moisture conveying pipeline 1 and evenly dispersed to the spinning area; during the spinning process, the temperature and humidity sensor 4 monitors the temperature and humidity changes in the area in real time, and feeds back to the temperature and humidity control / feedback adjustment system 7 to maintain the temperature and humidity of the area constant; by adjusting the moisture concentration in the spinning area, the phase separation and solidification speed of the jet is controlled, and the different forms of the jet are fixed, thereby changing the form and degree of entanglement of the fiber.

[0051] The spinning solution of the ultrafine fiber porous material of the present invention comprises raw materials and a solvent for dissolving the raw materials, wherein the concentration of the raw materials is 10 to 60 wt %;

[0052] The raw material is selected from one or more of polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, polymethyl methacrylate, polytrimethylene terephthalate, polystyrene, polyurethane, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polyethylene, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyamide, polyamideimide, polyvinyl alcohol, polyvinyl butyral, polysulfone, polyethyleneimine, polyimide, aramid 1313, titanium tetramethoxide, titanium tetraethoxide, titanium n-propoxide, titanium isopropoxide, titanium n-butoxide, titanium isobutoxide, tetraethyl orthosilicate, titanium tert-butoxide, titanium tetrapentoxide, titanium isooctoxide, zirconium tetramethoxide, zirconium tetraethoxide, zirconium n-propoxide, zirconium isopropoxide, zirconium n-butoxide, zirconium isobutoxide, zirconium tert-butoxide, zirconium tetrapentoxide, trimethoxyaluminum, triethoxide, tri-n-propoxyaluminum, aluminum isopropoxide, aluminum n-butoxide, aluminum sec-butoxide or aluminum tert-butoxide;

[0053] The solvent is selected from one or more of water, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, formic acid, acetic acid, dimethyl sulfoxide, toluene, acetone, cyclohexane, isobutanol, dichloromethane, butyl acetate, ethyl acetate, chloroform, methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol, glycerol, carbon tetrachloride, benzene, toluene, dichloroethane, dichloromethane, chloroform, ether, diphenyl ether, ethyl acetate, acetone, tetrahydrofuran, N-methylpyrrolidone or N,N-dimethylformamide.

[0054] Example 1

[0055] This embodiment provides a method for preparing an ultrafine fiber porous material based on electrostatic air spinning, and the specific steps are as follows:

[0056] The first step: the spinning solution raw materials include 20wt% polyurethane and 80wt% N,N-dimethylformamide. The polyurethane and N,N-dimethylformamide are put into a reactor, and the stirring speed is adjusted according to the viscosity of the solution before each addition of the raw materials. The polyurethane spinning solution is obtained after stirring and dissolving in the reactor; at the same time, a frequency conversion temperature control device is set to adjust the temperature of the spinning solution system to 60°C to ensure the long-term stable storage of the spinning solution.

[0057] The second step: the polyurethane spinning solution is extruded from the coaxial nozzle at a speed of 15mL / h, and a jet is formed under the action of 60kV high-voltage static electricity. At the same time, an airflow of 15m / s is blown out from each jet hole. The distance between the spinneret and the receiving plate is set to 60cm. The airflow passes through the baffle rod to form a vortex airflow, which drives the jet to perform high-speed drawing and whip curling.

[0058] Step 3: Set the temperature in the spinning area to 30°C and the relative humidity to 50%. Under this humidity, perform turbidity point titration on the spinning solution. Phase separation occurs after more than 130 seconds, and the phase separation speed is slow. The fiber curling rate is 5%, forming an ultrafine fiber membrane.

[0059] Step 4: placing the prepared ultrafine fiber membrane under ultrasonic waves to generate high temperature to fuse the fibers, and then drying and cooling to shape them, thereby obtaining a dense ultrafine fiber porous membrane material;

[0060] The ultrafine fiber porous material finally obtained has a fiber diameter of 180 nm, a thickness of 0.2 mm, a porosity of 35%, and a tensile strength of 15 MPa.

[0061] Example 2

[0062] This embodiment provides an ultrafine fiber porous material based on electrostatic air spinning and a preparation method thereof, and the specific steps are as follows:

[0063] The first step: the spinning solution raw materials include 10wt% titanium n-butoxide, 70wt% water, and 10wt% ethanol. Titanium n-butoxide water and ethanol are put into a reactor, and the stirring speed is adjusted according to the viscosity of the solution before each addition of the raw materials. After stirring and dissolving in the reactor, the titanium n-butoxide spinning solution is obtained; at the same time, a frequency conversion temperature control device is set to adjust the temperature of the spinning solution system to 50°C to ensure the long-term stable storage of the spinning solution.

[0064] The second step: the titanium n-butoxide spinning solution is extruded from the coaxial nozzle at a speed of 5 mL / h, and a jet is formed under the action of 50 kV high-voltage static electricity. At the same time, an airflow of 10 m / s is blown out from each jet hole. The distance between the spinneret and the receiving plate is set to 45 cm. The airflow passes through the baffle rod to form a vortex airflow, which drives the jet to perform high-speed drawing and whip curling.

[0065] Step 3: Set the temperature in the spinning area to 25°C, the relative humidity to 45%, the jet phase separation speed to be slow, the fiber curling rate to be 12%, and form an ultrafine fiber membrane. This is because when it is an inorganic spinning solution, the water vapor in the spinning environment continuously enters the jet, the water and alcohol dissolve each other, and the solvent volatilization in the jet is reduced, which is not conducive to fiber formation, so the jet phase separation speed is slow.

[0066] Step 4: placing the prepared ultrafine fiber membrane under ultrasonic waves to generate high temperature to fuse the fibers, and then drying and cooling to shape them, thereby obtaining a dense ultrafine fiber porous membrane material;

[0067] The ultrafine fiber porous material finally obtained has a fiber diameter of 500 nm, a thickness of 0.5 mm, a porosity of 50%, and a tensile strength of 7 MPa.

[0068] Example 3

[0069] This embodiment provides an ultrafine fiber porous material based on electrostatic air spinning and a preparation method thereof, and the specific steps are as follows:

[0070] The first step: the spinning solution raw materials include 20wt% polysulfone, 10% polyurethane and 70wt% N,N-dimethylformamide. The polysulfone, polyurethane and N,N-dimethylformamide are put into a reactor, and the stirring speed is adjusted according to the viscosity of the solution before each addition of the raw materials. The polyurethane spinning solution is obtained after stirring and dissolving in the reactor; at the same time, a frequency conversion temperature control device is set to adjust the temperature of the spinning solution system to 80°C to ensure the long-term stable storage of the spinning solution.

[0071] The second step: the polyurethane spinning solution is extruded from the coaxial nozzle at a speed of 30mL / h, and a jet is formed under the action of 80kV high-voltage static electricity. At the same time, an airflow of 20m / s is blown out from each jet hole. The distance between the spinneret and the receiving plate is set to 70cm. The airflow passes through the baffle rod to form a vortex airflow, which drives the jet to perform high-speed drawing and whip curling.

[0072] Step 3: Set the temperature in the spinning area to 30°C and the relative humidity to 90%. Under this humidity, perform turbidity point titration on the spinning solution. Phase separation will occur within 20 seconds. The phase separation speed is fast, and the fiber curling rate is 39%, forming ultrafine fiber flakes.

[0073] Step 4: spray glue on the surface of the prepared ultrafine fiber and hot-roll it with a high-temperature roller, and then dry and cool it to shape it, and finally obtain a fluffy ultrafine fiber porous material;

[0074] The final ultrafine fiber porous material has a fiber diameter of 3500nm, a thickness of 40mm, a porosity of 98%, and a volume density of 3mg / cm 3 , the compression rebound rate is 98% and the elongation at break is 34%.

[0075] Example 4

[0076] This embodiment provides an ultrafine fiber porous material based on electrostatic air spinning and a preparation method thereof, and the specific steps are as follows:

[0077] The first step: the spinning solution raw materials include 10wt% of tetraethyl orthosilicate, 70wt% of water, and 10wt% of ethanol. Tetraethyl orthosilicate, water, and ethanol are put into a reactor, and the stirring speed is adjusted according to the viscosity of the solution before each addition of the raw materials. After stirring and dissolving in the reactor, the tetraethyl orthosilicate spinning solution is obtained; at the same time, a frequency conversion temperature control device is set to adjust the temperature of the spinning solution system to 60°C to ensure the long-term stable storage of the spinning solution.

[0078] The second step: extrude the ethyl orthosilicate spinning solution from the coaxial nozzle at a speed of 35 mL / h, and form a jet under the action of 90 kV high-voltage static electricity. At the same time, a 25 m / s airflow is blown out from each jet hole. The distance between the spinneret and the receiving plate is set to 85 cm. The airflow passes through the baffle rod to form a vortex airflow, which drives the jet to perform high-speed drawing and whip curling.

[0079] Step 3: Set the temperature in the spinning area to 25°C and the relative humidity to 25%. At this time, the jet phase separation speed is faster, the fiber curling rate is 43%, and ultrafine fiber flakes are formed. This is because when it is an inorganic spinning solution, the less water vapor in the spinning environment, the faster the water and alcohol in the solvent will evaporate, which is conducive to fiber formation, so the jet phase separation speed is faster.

[0080] Step 4: spray glue on the surface of the prepared ultrafine fiber and hot-roll it with a high-temperature roller, and then dry and cool it to shape it, and finally obtain a fluffy ultrafine fiber porous material;

[0081] The final ultrafine fiber porous material has a fiber diameter of 375nm, a thickness of 60mm, a porosity of 99%, and a volume density of 4.5mg / cm 3 , the compression rebound rate is 95% and the elongation at break is 22%.

[0082] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing ultrafine fiber porous material based on electrostatic air spinning, characterized in that: The steps include: S1, preparing spinning solution; S2. A choke rod is arranged at the coaxial nozzle to cross the air outlet, and a receiving plate is arranged opposite to the outlet of the coaxial nozzle; the spinning solution is extruded through the coaxial nozzle, and a jet is formed under the action of high-voltage static electricity. At the same time, the airflow passes through the choke rod to form a vortex airflow, which drives the charged jet to perform high-speed drafting and whip curling. The size of the vortex can be changed by adjusting the airflow speed, thereby adjusting the curling amplitude and shape of the jet; S3, setting a constant temperature and humidity control device, by adjusting the moisture concentration in the spinning area, controlling the phase separation and solidification speed of the jet, fixing the different forms of the jet, thereby changing the form and entanglement degree of the fiber; when the jet slowly separates, straight fibers are obtained to form a fiber membrane; when the jet quickly separates, curly fibers are obtained, and the curly fibers are entangled with each other to form a three-dimensional interlocking structure to form a fiber flake; S4. When the product obtained in S3 is a fiber membrane, the fiber membrane is placed under high temperature to allow the fibers to be fused and composited, and then dried and shaped to obtain an ultrafine fiber porous membrane, which is an ultrafine fiber porous material; or, when the product obtained in S3 is a fiber flake, the surface of the fiber flake is sprayed with glue and hot rolled, and then dried and shaped to obtain an ultrafine fiber flake material, which is an ultrafine fiber porous material.

2. The method for preparing ultrafine fiber porous material based on electrostatic air spinning according to claim 1, characterized in that: The spinning solution of the ultrafine fiber porous material includes raw materials and a solvent for dissolving the raw materials, and the concentration of the raw materials is 10 to 60 wt%; The raw material is selected from one or more of polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, polymethyl methacrylate, polytrimethylene terephthalate, polystyrene, polyurethane, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polyethylene, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyamide, polyamideimide, polyvinyl alcohol, polyvinyl butyral, polysulfone, polyethyleneimine, polyimide, aramid 1313, titanium tetramethoxide, titanium tetraethoxide, titanium n-propoxide, titanium isopropoxide, titanium n-butoxide, titanium isobutoxide, tetraethyl orthosilicate, titanium tert-butoxide, titanium tetrapentoxide, titanium isooctoxide, zirconium tetramethoxide, zirconium tetraethoxide, zirconium n-propoxide, zirconium isopropoxide, zirconium n-butoxide, zirconium isobutoxide, zirconium tert-butoxide, zirconium tetrapentoxide, trimethoxyaluminum, triethoxide, tri-n-propoxyaluminum, aluminum isopropoxide, aluminum n-butoxide, aluminum sec-butoxide or aluminum tert-butoxide; The solvent is selected from one or more of water, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, formic acid, acetic acid, dimethyl sulfoxide, toluene, acetone, cyclohexane, isobutanol, dichloromethane, butyl acetate, ethyl acetate, chloroform, methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol, glycerol, carbon tetrachloride, benzene, toluene, dichloroethane, dichloromethane, chloroform, ether, diphenyl ether, ethyl acetate, acetone, tetrahydrofuran, N-methylpyrrolidone or N,N-dimethylformamide.

3. The method for preparing ultrafine fiber porous material based on electrostatic air spinning according to claim 2, characterized in that: The raw material is selected from one or more of polyurethane, titanium n-butoxide, polysulfone or tetraethyl orthosilicate; the solvent is selected from one or more of N,N-dimethylformamide, water or ethanol.

4. According to the method for preparing ultrafine fiber porous materials based on electrostatic air spinning in claim 1, in S2, the spinning solution forms a jet under the electrostatic action of 0 to 150 kV; the speed of the air flow is 0 to 25 m / s; the receiving distance between the coaxial nozzle and the receiving plate is 10 to 70 cm; the injection speed of the coaxial nozzle outlet is 5 to 80 ml / h.

5. According to the method for preparing ultrafine fiber porous materials based on electrostatic air spinning according to claim 1, in S3, the spinning temperature of the spinning area is 10-50°C, the relative humidity of the environment is 10-99%, and the fiber curling rate is 5-60%.

6. According to the method for preparing a superfine fiber porous material based on electrostatic air spinning according to claim 1, in S4, the welding method of the welding composite is one or more of thermal welding, ultrasonic welding, microwave irradiation welding, infrared irradiation welding, ultraviolet irradiation welding, electron beam irradiation welding, and plasma irradiation welding.

7. According to the method for preparing ultrafine fiber porous materials based on electrostatic air spinning according to claim 1, in S4, during the glue spraying hot rolling process, the glue spraying atomizing nozzle used has a glue spraying amount range of 0 to 50 mL / min, and the diameter of the atomized glue is 1 to 10 μm.

8. According to the method for preparing a superfine fiber porous material based on electrostatic air spinning according to claim 1, in S4, during the drying and shaping process, the superfine fiber porous material is post-treated with dry hot air and cold air, the temperature range of the hot air is 40 to 150°C, the temperature range of the cold air is 5 to 20°C, and the suction pressure is 0.1 to 10 MPa.

9. A porous ultrafine fiber material based on electrostatic air-spinning, characterized in that: The invention discloses a novel nanostructured carbon foam prepared by the preparation method according to any one of claims 1 to 8.

10. The ultra-fine fiber porous material based on electrostatic air-spinning according to claim 9, characterized in that: The ultrafine fiber porous material is an ultrafine fiber porous membrane or an ultrafine fiber flake material; When the ultrafine fiber porous material is an ultrafine fiber porous membrane, at least one of the following conditions is met: ① The thickness of the ultrafine fiber porous membrane is 0.1 to 2 mm; ② The porosity of the ultrafine fiber porous membrane is 20 to 90%; ③ The tensile strength of the ultrafine fiber porous membrane is higher than 5MPa; ④ The diameter of the ultrafine fiber porous membrane is 50 to 10000 nm; When the ultrafine fiber porous material is an ultrafine fiber flake material, at least one of the following conditions is met: ① The thickness of the ultrafine fiber flake material is 5 to 60 mm; ② The volume density of the ultrafine fiber flake material is 2 to 100 mg / cm 3 ; ③ The porosity of the ultrafine fiber flake material is higher than 95%; ④ The compression resilience of the ultrafine fiber flake material is above 90%; ⑤ The elongation at break of the ultrafine fiber flake material is higher than 10%; ⑥The diameter of the ultrafine fiber flake material is 50 to 10000 nm.

Citation Information

Patent Citations

  • Device and process for mass production of nanometer fiber by melt electro-spinning method

    CN102839431A

  • Electrostatic spinning device and preparation method of nanofibers

    CN115110160A

  • Spinning unit

    CN115110210A

  • Asymmetric transparent fiber-based thin film as well as preparation method and application thereof

    CN116575192A

  • Electrostatic spinning device is assisted to air current

    CN204939670U

Cited By

  • Precise control system and method for wool type fiber spinning process

    CN120509218A

  • A precise control system and method for wool fiber spinning process

    CN120509218B