Manufacturing method of flexible semiconductor refrigeration temperature-adjusting fabric
Through thermal spraying technology, conductive coatings and fabrics are combined to prepare flexible semiconductor cooling and temperature-regulating fabrics, which solves the problem that semiconductor ceramic refrigeration sheets cannot achieve insufficient flexibility and thermal conductivity of devices, and achieves efficient and controllable refrigeration effects and adapts to curved surface installation. Flexible fabric.
Patent Information
- Application Number
- CN202310659990.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing semiconductor ceramic refrigeration sheets cannot achieve device flexibility, which limits its application field. Moreover, the thermal conductivity of the ceramic sheets is insufficient, resulting in poor refrigeration effect.
The thermal spraying technology is used to combine conductive coatings with fabrics to prepare flexible semiconductor cooling and temperature-regulating fabrics. By preparing conductive fillers, N-type and P-type semiconductor composite layers, and using screen printing technology to form conductive paths and semiconductor modules on the flexible fabrics. Achieve flexible and efficient refrigeration.
The continuous, effective and controllable preparation of flexible semiconductor cooling and temperature-regulating fabrics is achieved, which improves the refrigeration effect and adapts to the needs of curved surface installation, and reduces production complexity and cost.
Smart Images

Figure CN119021012A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a flexible semiconductor refrigeration temperature regulating fabric, and belongs to the field of semiconductor materials. Background Art
[0002] Semiconductor refrigeration, also known as thermoelectric refrigeration, is the application of the Peltier effect in refrigeration. Currently, most of the semiconductor ceramic refrigeration sheets on the market are semiconductor refrigeration sheets. Traditional semiconductor refrigeration sheets are composed of ceramic substrates, copper conductors, grains, and solder. The refrigeration sheet uses a ceramic sheet as a substrate, and its appearance is hard, flat, and cannot be bent. As a result, the current semiconductor refrigeration sheet has a single structure type and cannot match the curved surface installation requirements of the terminal. Therefore, the application field is greatly limited, and the thermal conductivity of the ceramic sheet limits the cooling effect of the semiconductor.
[0003] Chinese invention patent [CN106579590A] discloses a temperature-regulating garment based on variable thermal resistance, including a garment fabric layer, a flexible semiconductor thermoelectric array, a garment lining layer, a converter, an adjustable load, a controller and an external power connector. The flexible semiconductor thermoelectric array is placed between the garment fabric layer and the garment lining layer, and the flexible semiconductor thermoelectric array is connected to the adjustable load or sequentially connected to the controller and the external power connector through the converter, and the converter realizes the switching of the connection relationship. By setting a garment temperature control circuit or a hat temperature circuit in a garment body or a hat body, the garment body or the hat body adopts a flexible semiconductor temperature control cloth, and the flexible semiconductor temperature control cloth is encapsulated with doped N-type and P-type semiconductor refrigeration (or heating) particles, and contains a temperature sensor in the garment body or the hat body, the garment temperature control circuit or the hat temperature circuit adjusts the temperature of the flexible semiconductor temperature control cloth according to the temperature collected by the temperature sensors installed on both sides of the flexible semiconductor temperature control cloth, thereby realizing the temperature control of the garment or the hat, and meeting the needs of the user's daily life.
[0004] In the above patent, the flexible semiconductor temperature control cloth is made of foam rubber or blended cloth, and the doped N-type and P-type semiconductor particles inside the lining are encapsulated with thermal conductive adhesive, and the particles are encapsulated with a plastic layer to form an N-type-P-type-N-type interval arrangement effect; and connected with an FPC flexible circuit, the doped N-type and P-type semiconductor particles are covered with a plastic layer; the upper and lower surfaces of the entire flexible semiconductor temperature control cloth are encapsulated with thermal conductive adhesive. After encapsulation, a metal film 140 is vacuum plated on the upper and lower surfaces to finally obtain a flexible semiconductor temperature control cloth.
[0005] The flexible semiconductor temperature control fabric in the above patent uses a plastic layer to encapsulate N-type semiconductor particles and P-type semiconductor particles, which reduces its operating efficiency and makes the cost too expensive. The N-type-P-type-N-type spacing arrangement effect of the composition, and the FPC flexible copper sheet and all the individual components are complexly composed, making the construction process too complicated. Therefore, the design leads to the use of the clothes, and the clothing material properties must be matched with it, and the temperature control and refrigeration must have corresponding conditions to be able to proceed. Under this limitation, the clothes made must be equipped with zippers and buttons to cool or heat, and the operation is extremely complicated.
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for manufacturing a semiconductor flexible refrigeration and temperature-regulating fabric, which uses thermal spraying technology to combine a new conductive coating with the fabric, thereby solving the technical limitation of existing semiconductor ceramic refrigeration sheets that cannot achieve device flexibility. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention provides a continuous, effective and controllable method for preparing a semiconductor temperature regulating fabric.
[0008] In order to achieve the above object, the technical solution adopted by the present invention mainly includes the following steps:
[0009] 1. Preparation of conductive coating: Add 4-5 parts of silane coupling agent to 30 grams of ethanol, mix thoroughly and stir at room temperature of 25 degrees Celsius for 15-20 minutes; then add 12-15 parts of nano-conductive carbon black, stir for 2-3 minutes, then add 2-4 parts of carbon nanotubes, stir for 3-5 minutes, and let stand for 1 hour; place the mixture in a water bath and stir mechanically for 70-85 minutes to allow the three to react fully; filter the mixture, take the filter residue, use ethanol to wash the filter residue, and remove the unreacted silane coupling agent; finally, place the modified filler in a vacuum drying oven to dry to obtain a preliminary product. Add 5-8 parts of silane coupling agent to 50-60 parts of solvent and stir mechanically, add 60-70 parts of conductive metal powder to the above solvent and stir evenly to obtain metal powder slurry. Dissolve 15-25 parts of film-forming resin in the solvent to obtain a resin solution with a content of 25% to 40%. The above-mentioned silane coupling agent-modified nano-conductive carbon black, carbon nanotubes and metal powder are added into a film-forming resin solution with a solid content of 25% to 40%, and ground and dispersed to obtain a conductive coating paint.
[0010] 2. Preparation of N-type semiconductor composite layer and P-type semiconductor composite layer: bisphenol A epoxy resin: glycerol epoxy resin: acrylic epoxy resin: curing agent = 2:2:2:1-4:4:4:3 resin, CNTs: conductive carbon black: chopped carbon fiber = 2:1:1-4:3:3 conductive filler, stabilizer and aromatic hydrocarbon are mixed in a ratio of 4:3:1:1-8:6:3:3, stabilizer and aromatic hydrocarbon are mixed first, conductive filler and resin are added in sequence, and the indoor temperature is controlled at 25-30°C to form a conductive coating; N-type semiconductor powder with a mesh size of more than 300 formed by doping bismuth telluride, main component, conductive filler A conductive adhesive formed by mixing a certain proportion of boron-doped P-type semiconductor powder with a mesh size of 300 or more, a main component, a conductive filler, a toughening agent, a solvent and other additives is mixed in a ratio of 3:1 to 4:1, and is fully mixed in an environment with a temperature of 20 to 25°C and a humidity of 40 to 50%, and is allowed to stand for 5 to 10 minutes to form a flexible N-type semiconductor composite layer; a conductive adhesive formed by mixing a certain proportion of boron-doped P-type semiconductor powder with a mesh size of 300 or more, a main component, a conductive filler, a toughening agent, a solvent and other additives is mixed in a ratio of 3:1 to 5:1, and is fully mixed in an environment with a temperature of 20 to 25°C and a humidity of 40 to 50%, and is allowed to stand for 5 to 10 minutes to form a flexible P-type semiconductor composite layer.
[0011] 3. Prepare conductive filler: add 10 to 25 parts of deionized water and 1 to 5 parts of conductive enhancer in batches at a temperature of 20 to 25°C and a humidity of 40 to 50%, mix and grind according to the proportion, and obtain product a; add 1 to 2 parts of defoamer, 10 to 20 parts of aqueous emulsion, 10 to 50 parts of conductive carbon powder and 1 to 3 parts of dispersant in batches at a temperature of 30 to 35°C and a humidity of 40 to 50%, mix and grind according to the proportion, and obtain product b; mix products a and b in batches at different proportions at a temperature of 30 to 35°C and a humidity of 40 to 50%, and grind again, take out and vacuum degasse to obtain water-based conductive slurry.
[0012] 4. Semiconductor module manufacturing method: On a piece of flexible fabric with a thickness of 2-3mm, a layer of naturally degradable waterproof coating is covered on its surface using screen printing technology and a special template. After the operation is completed, there will be 2n circular blocks on the flexible fabric, where n is an integer greater than 1, and the blocks are spaced 5cm apart and at an angle of 60°. The conductive filler obtained above is atomized by a spray gun, and then embedded into the flexible fabric along the blocks by spraying. The air pressure is controlled at 0.3-0.4MPa, and the nozzle is flat on the surface of the object and sprayed at a distance of 20-30mm from the surface at a uniform speed of 2-3mm / s. The spraying is divided into three times, each lasting 5s. After each spraying is completed, the next spraying begins after standing for 1 to 2 minutes. The overlap of the spray gun is 1 / 2 for the first spraying, and the overlap of the spray gun is 2 / 3 to 3 / 4 for the second and third spraying, so that the depth of the conductive filler embedded in the flexible fabric reaches 1.5 ~2mm, both sides of the flexible fabric are treated with this process, so that the conductive filler and the flexible fabric are evenly mixed and the two sides overlap to form a conductive path; then the N-type semiconductor composite layer is printed on one side of the flexible fabric using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric, and the position relationship is that the upper part is completely covered, and the thickness is 3mm. The P-type semiconductor composite layer is printed on the other side of the flexible fabric using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric, and the position relationship is that the upper part is completely covered, and the thickness is 3mm. After standing for 10 to 12 minutes, a semiconductor refrigeration module is formed.
[0013] 5. Overall structural design method:
[0014] On a piece of flexible fabric with a thickness of 2-3mm, 2n semiconductor refrigeration modules are evenly arranged, n is an integer greater than 1, and are placed side by side on the flexible fabric at an angle of 60° with an interval of 5cm. The semiconductor refrigeration modules form an interval arrangement effect. The conductive coating is printed on the N-type semiconductor composite layer and the P-type semiconductor composite layer using screen printing technology, with a thickness of 2mm; the power lead includes a positive power lead and a negative power lead, wherein the positive power lead is connected to the conductive coating on one side of the P-type semiconductor composite layer, and the negative power lead is connected to the conductive coating on one side of the N-type semiconductor composite layer; 2n semiconductor refrigeration modules are connected in series, and a path is formed if current is applied. The power supply voltage and the overall resistance are selected based on the specific heating temperature of the flexible semiconductor refrigeration thermostatic fabric. After the conduction test, it is encapsulated with thermal conductive glue. After encapsulation, a layer of metal film is vacuum-plated on the upper and lower surfaces. In order to improve the safety of power use, a flexible tempered film is wrapped on the outside of the power supply to prevent accidents. Finally, a flexible semiconductor refrigeration thermostatic fabric is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1It is a structural schematic diagram of the flexible semiconductor refrigeration temperature regulating fabric of the present invention.
[0016] Figure 2 This is a connection diagram of a semiconductor module.
[0017] 1. P-type semiconductor composite layer; 2. Conductive coating; 3. Conductive filler; 4. N-type semiconductor composite layer; 5. Flexible fabric; 6. Positive power lead; 7. Negative power lead; 8. Semiconductor refrigeration module; DETAILED DESCRIPTION
[0018] The specific implementation method of the present invention is further described below in conjunction with the accompanying drawings:
[0019] As shown in the figure, this is a method for making a flexible semiconductor refrigeration and temperature-regulating fabric.
[0020] Preparation of conductive coatings (2)
[0021] 4 grams of diethylaminomethyltriethoxysilane were added to 30 grams of ethanol, mixed thoroughly and stirred at room temperature of 25°C for 17 minutes; then 17 grams of nano-conductive carbon black were added first, stirred for 3 minutes, and then 3 grams of carbon nanotubes were added, stirred for 4 minutes, and allowed to stand for 1 hour; the mixture was placed in a water bath and mechanically stirred at 70°C for 80 minutes to allow the three to react fully; the mixture was filtered, the filter residue was taken, and the filter residue was washed with ethanol to remove the unreacted silane coupling agent. This step was repeated 3 times; finally, the modified filler was placed in a vacuum drying oven at 120°C and dried to obtain a preliminary product. 4 grams of diethylaminomethyltriethoxysilane were added to 120 grams of solvent for mechanical stirring, and 170 grams of 1 micron spherical nickel powder were added to the above solvent in 3 batches and stirred evenly to obtain nickel powder slurry. 32 grams of polyester resin were dissolved in the solvent to obtain a resin solution with a content of 30±0.5%. The above-mentioned silane coupling agent-modified nano-conductive carbon black, carbon nanotubes and metal powder are added to a resin solution with a content of 30±0.5%, and ground and dispersed to obtain a conductive coating (2).
[0022] Preparation of N-type semiconductor composite layer (4) and P-type semiconductor composite layer (1)
[0023] The resin of bisphenol A epoxy resin: glycerol epoxy resin: acrylic epoxy resin: curing agent = 2:2:2:1, CNTs: conductive carbon black: chopped carbon fiber = 2:1:1 conductive filler, stabilizer and aromatic hydrocarbon are mixed in a ratio of 4:3:1:1, the stabilizer and aromatic hydrocarbon are mixed first, and the conductive filler and resin are added in sequence, and the indoor temperature is controlled at 23±0.5°C to form a conductive coating; N-type semiconductor powder with a mesh size of more than 300 formed by doping bismuth telluride, the main component, the conductive filler, the toughening agent, the solvent and other additives are mixed in a certain proportion The conductive adhesive formed by mixing the boron-doped P-type semiconductor powder with a mesh size of 300 or more, the main component, the conductive filler, the toughening agent, the solvent and other additives in a certain proportion are mixed in a ratio of 3:1, and the mixture is fully mixed in an environment with a temperature of 22±0.5°C and a humidity of 42±0.5%, and the mixture is left to stand for 8 minutes to form a flexible N-type semiconductor composite layer (4). The conductive adhesive formed by mixing the boron-doped P-type semiconductor powder with a mesh size of 300 or more, the main component, the conductive filler, the toughening agent, the solvent and other additives in a certain proportion are mixed in a ratio of 3:1, and the mixture is fully mixed in an environment with a temperature of 22±0.5°C and a humidity of 43±0.5%, and the mixture is left to stand for 9 minutes to form a flexible P-type semiconductor composite layer (1).
[0024] Preparation of conductive fillers (3)
[0025] 20 grams of deionized water and 2 grams of conductive enhancer were added twice in a ratio of 1:10 at a temperature of 22±0.5°C and a humidity of 42±0.5%, with the order of adding deionized water first and then adding the conductive enhancer for mixed grinding. The grinding speed was 500 rpm and the grinding time was 5 hours to obtain product a. 1 gram of organic fluorine silicon compound, 15 grams of pure acrylic emulsion, 40 grams of conductive graphite and 2 grams of hydroxyethyl cellulose were mixed at a temperature of 30±0.5°C and a humidity of The mixture was added twice in a ratio of 1:15:40:2 at a temperature of 22±0.5°C and a humidity of 42±0.5%, and mixed and ground at a speed of 600 rpm for 6 h to obtain product b; products a and b were mixed twice in a ratio of 2:5 at a temperature of 22±0.5°C and a humidity of 43±0.5%, first adding product a and then product b and grinding again at a speed of 300 rpm for 2 h. After taking out, vacuum degassing was performed to obtain an aqueous conductive slurry.
[0026] Semiconductor module manufacturing method
[0027] A layer of naturally degradable waterproof coating is coated on the surface of a piece of flexible fabric (5) having a thickness of 2-3 mm using screen printing technology and a special template. After the operation, there will be 2n circular blocks on the flexible fabric (5), where n is an integer greater than 1, arranged side by side at an interval of 5 cm and an angle of 60°, which are not sprayed with waterproof coating. After the conductive filler (3) obtained above is atomized by a spray gun, the conductive filler (3) is embedded into the flexible fabric (5) along the block by spraying. The air pressure is controlled at 0.3-0.4MPa. The nozzle is flat on the surface of the object and the distance between the nozzle and the surface is 20-30mm. The spraying is carried out evenly at a speed of 2-3mm / s. The spraying is divided into three times, and each time the duration is 5s. After each spraying is completed, the next spraying is started after standing for 1-2 minutes. The overlap of the spray gun during the first spraying is 1 / 2, and the overlap of the spray gun during the second and third spraying is 2 / 3-3 / 4, so that the depth of the conductive filler (3) embedded in the flexible fabric (5) reaches 1.5-2mm. Both sides of the flexible fabric (5) are treated with this process, so that the conductive filler and the flexible fabric (5) are evenly mixed and the two sides overlap to form a conductive path; then the N-type semiconductor composite layer (4) is printed on one side of the flexible fabric (5) using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric (5) and the position relationship is that the upper part completely covers the lower part, and the thickness is 3mm; the P-type semiconductor composite layer (1) is printed on the other side of the flexible fabric (5) using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric (5) and the position relationship is that the upper part completely covers the lower part, and the thickness is 3mm. After standing for 10 to 12 minutes, a semiconductor refrigeration module (8) is formed.
[0028] Overall structural design method
[0029] On a flexible fabric (5) with a thickness of 2-3 mm, 2n semiconductor refrigeration modules (8) are evenly arranged, n is an integer greater than 1, and are placed side by side on the flexible fabric at an angle of 60° with an interval of 5 cm, so that the semiconductor refrigeration modules (8) form an interval arrangement effect. The conductive coating (3) is printed on the N-type semiconductor composite layer (4) and the P-type semiconductor composite layer (1) using screen printing technology, with a thickness of 2 mm; the power lead includes a positive power lead (6) and a negative power lead (7), wherein the positive power lead (6) is connected to the conductive coating (2) on one side of the P-type semiconductor composite layer (1), and the negative power lead (7) is connected to the conductive coating (2) on one side of the N-type semiconductor composite layer (4); the 2n semiconductor refrigeration modules (8) are connected in series, and a current is added to form a path. The power supply voltage and the overall resistance are selected based on the specific heating temperature of the flexible semiconductor refrigeration temperature regulating fabric. After the conduction test, it is encapsulated with thermal conductive glue. After packaging, a metal film is vacuum plated on the upper and lower surfaces. In order to improve the safety of power supply, a flexible tempered film is wrapped on the outside of the power supply to prevent accidents. Finally, a flexible semiconductor refrigeration temperature regulating fabric is obtained.
Claims
1. A method for making a flexible semiconductor refrigeration temperature regulating fabric; The following steps are involved: (1) Preparation of conductive coating: 4-5 parts of silane coupling agent are added to 30 grams of ethanol, mixed thoroughly and stirred at room temperature of 25 degrees Celsius for 15-20 minutes; then 12-15 parts of nano-conductive carbon black are added, stirred for 2-3 minutes, and then 2-4 parts of carbon nanotubes are added, stirred for 3-5 minutes, and allowed to stand for 1 hour; the mixture is placed in a water bath and mechanically stirred for 70-85 minutes to allow the three to react fully; the mixture is filtered, the filter residue is taken, and the filter residue is washed with ethanol to remove the unreacted silane coupling agent; finally, the modified filler is added. The method comprises placing the mixture in a vacuum drying oven and drying it to obtain a preliminary product; adding 5 to 8 parts of a silane coupling agent to 50 to 60 parts of a solvent and mechanically stirring the mixture; adding 60 to 70 parts of a conductive metal powder to the solvent and stirring the mixture to obtain a metal powder slurry; dissolving 15 to 25 parts of a film-forming resin in the solvent to obtain a resin solution with a solid content of 25% to 40%; adding the nano-conductive carbon black, carbon nanotubes and metal powder modified by the silane coupling agent to the film-forming resin solution with a solid content of 25% to 40%, grinding and dispersing the mixture to obtain a conductive coating; (2) Preparation of N-type semiconductor composite layer and P-type semiconductor composite layer: a resin prepared by mixing three kinds of epoxy resins (bisphenol A type, glycerol, acrylic acid) and a curing agent in a ratio of about 2:2:2:1, a conductive filler prepared by mixing CNTs: conductive carbon black: chopped carbon fiber in a ratio of about 4:3:3, a stabilizer and an aromatic hydrocarbon in a ratio of about 4:3:1:1, the stabilizer and the aromatic hydrocarbon are mixed first, and the conductive filler and the resin are added in sequence, and the room temperature is controlled at 25 to 30° C. to form a conductive coating; an N-type semiconductor powder of 300 mesh or more formed by doping bismuth telluride, the main component, the conductive filler, the toughening agent, the solvent A conductive adhesive formed by mixing a conductive filler and other additives in a certain proportion is mixed in a ratio of about 3:1 under a temperature of 20 to 25°C and a humidity of 40 to 50%, and is allowed to stand for 5 to 10 minutes to form a flexible N-type semiconductor composite layer; a conductive adhesive formed by mixing a boron-doped P-type semiconductor powder with a mesh size of more than 300, a main component, a conductive filler, a toughening agent, a solvent and other additives in a certain proportion is mixed in a ratio of 3:1 to 5:1 under a temperature of 20 to 25°C and a humidity of 40 to 50%, and is allowed to stand for 5 to 10 minutes to form a flexible P-type semiconductor composite layer; (3) Preparing a conductive filler: adding 10 to 25 parts of deionized water and 1 to 5 parts of a conductive enhancer in batches in a temperature of 20 to 25° C. and a humidity of 40 to 50%, mixing and grinding them in proportion to obtain a product a; adding 1 to 2 parts of a defoamer, 10 to 20 parts of an aqueous emulsion, 10 to 50 parts of a conductive carbon powder and 1 to 3 parts of a dispersant in batches in a temperature of 30 to 35° C. and a humidity of 40 to 50%, mixing and grinding them in proportion to obtain a product b; mixing products a and b in batches in different proportions in a temperature of 30 to 35° C. and a humidity of 40 to 50%, grinding them again, taking them out and vacuum degassing them to obtain an aqueous conductive slurry; (4) Semiconductor module manufacturing method: a piece of flexible fabric with a thickness of 2-3 mm is coated with a layer of naturally degradable waterproof coating using screen printing technology and a special template. After the operation, there will be 2n circular blocks on the flexible fabric, where n is an integer greater than 1, arranged side by side with an interval of 5 cm and an angle of 60°, which are not sprayed with waterproof coating; the conductive filler obtained above is atomized by a spray gun, and the conductive filler is embedded into the flexible fabric along the blocks by spraying, the air pressure is controlled at 0.3-0.4 MPa, the nozzle is flat on the surface of the object, the distance between the nozzle and the surface is 20-30 mm, and the speed is uniformly operated at 2-3 mm / s. The spraying is divided into three times, each lasting 5 seconds. After each spraying is completed, it is left to stand for 1-2 minutes before starting the next spraying. During the first spraying, the spray gun is sprayed at a speed of 20-30 mm / s. The overlap is 1 / 2, and the overlap of the spray gun during the second and third spraying is 2 / 3 to 3 / 4, so that the depth of the conductive filler embedded in the flexible fabric reaches 1.5 to 2 mm. Both sides of the flexible fabric are treated with this process, so that the conductive filler and the flexible fabric are evenly mixed and the two sides are overlapped to form a conductive path; then the N-type semiconductor composite layer is printed on one side of the flexible fabric using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric, and the position relationship is that the upper part is completely covered, and the thickness is 3 mm. The P-type semiconductor composite layer is printed on the other side of the flexible fabric using screen printing technology, and the shape and size correspond to the shape of the conductive filler on the surface of the flexible fabric, and the position relationship is that the upper part is completely covered, and the thickness is 3 mm; after standing for 10 to 12 minutes, a semiconductor refrigeration module is formed; (5) Overall structural design method: On a piece of flexible fabric with a thickness of 2-3 mm, 2n semiconductor refrigeration modules are evenly arranged, where n is an integer greater than 1, and are placed side by side on the flexible fabric at an angle of 60° with an interval of 5 cm, so that the semiconductor refrigeration modules form an interval arrangement effect; a conductive coating is printed on the N-type semiconductor composite layer and the P-type semiconductor composite layer using screen printing technology, with a thickness of 2 mm; a power lead includes a positive power lead and a negative power lead, wherein the positive power lead is connected to the conductive coating on one side of the P-type semiconductor composite layer, and the negative power lead is connected to the conductive coating on one side of the N-type semiconductor composite layer; 2n semiconductor refrigeration modules are connected in series, and a path is formed if an electric current is applied; wherein the power supply voltage and the overall resistance are selected based on the specific heating temperature of the flexible semiconductor refrigeration temperature regulating fabric; after a conduction test, they are packaged with thermal conductive glue; after packaging, a metal film is vacuum plated on the upper and lower surfaces, and in order to improve the safety of power use, a flexible tempered film is wrapped around the outside of the power supply; finally, a flexible semiconductor refrigeration temperature regulating fabric is obtained.