AR film with better film surface physical performance and preparation process thereof
Patent Information
- Application Number
- CN202411176335.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing AR films have shortcomings in wear resistance and high temperature resistance, and cannot meet the increasingly high performance requirements.
The AR film design adopts a multi-layer structure, including a substrate layer, an upper coating layer, a silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon aluminum hybrid layer and a scratch-resistant layer , and a base layer and a protective film are installed in the preparation process, and each layer is plated through magnetron sputtering technology, and the thickness and molar ratio of each layer are controlled to optimize optical and physical properties.
It significantly improves the optical performance, wear resistance and high temperature resistance of the AR film, ensures its stability and safety in use, and meets the needs of future automotive products to improve the performance of AR films.
Smart Images

Figure CN119024469A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of optical films, and in particular relates to an AR film with better film surface physical properties and a preparation process thereof. Background Art
[0002] AR film, or anti-reflection film, can improve transmittance and optical performance by reducing reflection loss. The main principle is to use the interference effect produced by different optical materials to eliminate incident light and reflected light, thereby achieving anti-reflection function. In the application of AR film, with the increase in the application fields of AR technology, AR products will gradually become the mainstream of the automotive product market in the future, so the development and production of AR film is the general trend.
[0003] Applying AR film to the car screen can reduce the reflectivity of light reaching the screen and block ultraviolet light in sunlight. At the same time, it can improve the transmittance of the car display and increase the contrast, allowing the driver to clearly see the content on the screen while driving, free from the influence of screen light reflection, thus ensuring driving safety.
[0004] With the continuous development of AR film applications, people's requirements for AR films are no longer just high transmittance and low reflectivity, but also have higher requirements on the wear resistance and high temperature resistance of the film surface. Therefore, it is necessary to further improve the performance of AR films.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] The purpose of the present invention is to provide an AR film with better physical properties on the film surface and a preparation process thereof. The AR film has excellent wear resistance and high temperature resistance and has high overall performance.
[0007] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0008] The AR film with better physical properties on the film surface comprises a substrate layer, on which an upper coating layer, a silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer are sequentially arranged, and the silicon nitride layer has a thickness of 1 to 30 nm.
[0009] In one or more embodiments of the present invention, a base layer is provided between the upper coating layer and the silicon nitride layer, and the base layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y.
[0010] In one or more embodiments of the present invention, the thickness of the primer layer is 0.1-10 nm.
[0011] In one or more embodiments of the present invention, the thickness of the first niobium oxide layer is 1-50 nm.
[0012] In one or more embodiments of the present invention, the silicon dioxide layer has a thickness of 10 to 260 nm.
[0013] In one or more embodiments of the present invention, the thickness of the second niobium oxide layer is 5-280 nm.
[0014] In one or more embodiments of the present invention, the thickness of the silicon-aluminum mixed layer is 50-310 nm; and / or,
[0015] The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms.
[0016] In one or more embodiments of the present invention, the anti-scratch layer is formed by coating an AF coating liquid and has a thickness of 2 to 190 nm.
[0017] Another specific embodiment of the present invention provides a technical solution as follows:
[0018] The preparation process of the AR film with better physical properties on the film surface includes the following steps:
[0019] A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer;
[0020] A silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; wherein the thickness of the silicon nitride layer is 1 to 30 nm;
[0021] Disposing an anti-scratch layer on the silicon-aluminum mixed layer;
[0022] A positive protective film is provided on the anti-scratch layer.
[0023] In one or more embodiments of the present invention, a primer layer is disposed between the upper coating layer and the silicon nitride layer.
[0024] Compared with the prior art, the present invention provides a silicon nitride layer and combines the coordination between the layers, so that the prepared AR film has better optical properties, excellent wear resistance and high temperature resistance, and presents better performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 It is a schematic diagram of the structure of an AR film with better film surface physical properties in Example 1 of the present invention;
[0027] Figure 2 It is a schematic diagram of the structure of an AR film with better film surface physical properties in Example 6 of the present invention;
[0028] Figure 3 It is a comparison chart of the reflection curves of 1380-780nm of Example 1, Example 6 and Comparative Example of the present invention;
[0029] Figure 4 It is a comparison chart of the reflection curves of Example 1, Example 6 and the comparative example at 1400-700nm of the present invention.
[0030] Description of main reference numerals:
[0031] 1-high temperature protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-silicon nitride layer, 6-first niobium oxide layer, 7-silicon dioxide layer, 8-second niobium oxide layer, 9-silicon aluminum mixed layer, 10-anti-scratch layer, 11-positive protective film, 12-base layer. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] A specific embodiment of the present invention provides an AR film with better physical properties on the film surface, including a substrate layer, on which are sequentially provided an upper coating layer, a silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer, and the thickness of the silicon nitride layer is 1 to 30 nm.
[0034] Specifically, in terms of optical properties, silicon nitride has a high refractive index and excellent light transmittance, which can effectively reduce the reflectivity of the AR film and improve the transmittance of the AR film; in terms of chemical and physical properties, silicon nitride has high strength, high thermal stability and good chemical corrosion resistance, and its hardness and wear resistance are excellent, which can greatly improve the wear resistance and high temperature resistance of the AR film. The present invention selects to set a silicon nitride layer between the upper coating layer and the first niobium oxide layer, and at the same time controls the thickness of the silicon nitride layer, so that the AR film has both good optical properties and good physical properties.
[0035] In addition, regarding the specific composition of the AR film, the present invention selects a first niobium oxide layer to increase transmittance, a silicon dioxide layer to reduce reflection is arranged on the first niobium oxide layer, a second niobium oxide layer to increase transmittance is arranged on the silicon dioxide layer, and a silicon-aluminum mixed layer to reduce reflection is arranged on the second niobium oxide layer. Through the coordination between the layers, the AR film exhibits excellent optical properties. In addition, an anti-scratch layer is arranged on the surface of the AR film to further improve the physical properties of the AR film.
[0036] In a specific embodiment, a primer layer is provided between the upper coating layer and the silicon nitride layer. The material of the primer layer is selected from SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y. The thickness of the primer layer is 0.1 to 10 nm.
[0037] Specifically, SiO2 (silicon dioxide), Ti (titanium), Si (silicon), Al (aluminum), MgF2 (magnesium fluoride), SiO (silicon monoxide), Sn (tin) and Y (yttrium) are selected to set a base layer on the upper coating layer, which can improve the adhesion of the silicon nitride layer and enable the coating layers to be tightly bonded, thereby effectively ensuring that the AR film has excellent optical and physical properties.
[0038] In a specific embodiment, the thickness of the first niobium oxide layer is 1 to 50 nm, the thickness of the silicon dioxide layer is 10 to 260 nm, and the thickness of the second niobium oxide layer is 5 to 280 nm.
[0039] Specifically, by controlling the thicknesses of the first niobium oxide layer, the silicon dioxide layer, and the second niobium oxide layer, it is possible to ensure that the AR film has better optical properties.
[0040] In a specific embodiment, the thickness of the silicon-aluminum mixed layer is 50-310 nm, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms.
[0041] Specifically, the silicon-aluminum mixed layer is located on the surface of the AR film and plays a role in reducing reflection. By controlling the silicon-aluminum molar ratio, the density and uniformity of the silicon-aluminum mixed layer can be improved, thereby ensuring the optical stability of the AR film.
[0042] In a specific embodiment, the anti-scratch layer is formed by coating the AF coating liquid and has a thickness of 2 to 190 nm.
[0043] Specifically, AF coating liquid is also called anti-fingerprint liquid, anti-scratch liquid, and anti-oil liquid. Its main component is perfluoropolyether polymer. It is an existing product. Setting it on the top layer of AR film can effectively reduce the possibility of scratching the AR film surface, thereby ensuring the stability of the optical and physical properties of the AR film.
[0044] In a specific embodiment, the thickness of the substrate layer is 5.7-250 μm; the substrate layer is selected from a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer.
[0045] Specifically, the PET layer is a polyethylene terephthalate layer, the PI layer is a polyimide layer, the SRF layer is a super-reflective polyester film, the TAC layer is a triacetyl cellulose layer, the COP layer is a cycloolefin polymer layer, and the PC layer is a polycarbonate layer. Selecting the above types of substrate layers can make the AR film have a stable structure and optical properties.
[0046] Another specific embodiment of the present invention provides a process for preparing an AR film having better physical properties on the film surface, comprising the following steps:
[0047] A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer;
[0048] A silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; wherein the thickness of the silicon nitride layer is 1 to 30 nm;
[0049] Disposing an anti-scratch layer on the silicon-aluminum mixed layer;
[0050] A positive protective film is provided on the anti-scratch layer.
[0051] Specifically, during the preparation process, magnetron sputtering technology is used for plating. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid, the thickness of the upper coating layer is 50 to 500 nm, and the thickness of the lower coating layer is 0.2 to 4.1 μm. The high-temperature protective film and the positive protective film are both PET films, and the thickness of the high-temperature protective film is 30 to 188 μm.
[0052] In a specific embodiment, a primer layer is further disposed between the upper coating layer and the silicon nitride layer.
[0053] Specifically, the base layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y, and the thickness of the base layer is 0.1 to 10 nm.
[0054] The present invention is further described in detail below in conjunction with specific embodiments.
[0055] Example 1
[0056] The AR film with better physical properties on the film surface includes, from bottom to top, a 30μm thick high-temperature protective film, a 0.2μm thick lower coating layer, a 38μm thick substrate layer, a 100nm thick upper coating layer, a 30nm thick silicon nitride layer, a 40nm thick first niobium oxide layer, a 100nm thick silicon dioxide layer, an 80nm thick second niobium oxide layer, a 120nm thick silicon-aluminum mixed layer, a 50nm thick anti-scratch layer and a 45μm thick positive protective film.
[0057] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a PC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0058] Example 2
[0059] The AR film with better physical properties on the film surface includes, from bottom to top, a 90μm thick high-temperature protective film, a 2μm thick lower coating layer, an 80μm thick substrate layer, a 50nm thick upper coating layer, a 1nm thick silicon nitride layer, a 1nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 45μm thick positive protective film.
[0060] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a PET layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 85:15 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0061] Example 3
[0062] The AR film with better physical properties on the film surface includes, from bottom to top, a high-temperature protective film with a thickness of 110μm, a lower coating layer with a thickness of 3μm, a substrate layer with a thickness of 188μm, an upper coating layer with a thickness of 300nm, a silicon nitride layer with a thickness of 20nm, a first niobium oxide layer with a thickness of 50nm, a silicon dioxide layer with a thickness of 150nm, a second niobium oxide layer with a thickness of 150nm, a silicon-aluminum mixed layer with a thickness of 310nm, a scratch-resistant layer with a thickness of 110nm and a positive protective film with a thickness of 45μm.
[0063] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a TAC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0064] Example 4
[0065] The AR film with better physical properties on the film surface includes, from bottom to top, a high-temperature protective film with a thickness of 188μm, a lower coating layer with a thickness of 4.1μm, a substrate layer with a thickness of 250μm, an upper coating layer with a thickness of 500nm, a silicon nitride layer with a thickness of 15nm, a first niobium oxide layer with a thickness of 20nm, a silicon dioxide layer with a thickness of 260nm, a second niobium oxide layer with a thickness of 280nm, a silicon-aluminum mixed layer with a thickness of 250nm, a scratch-resistant layer with a thickness of 190nm and a positive protective film with a thickness of 45μm.
[0066] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a COP layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0067] Example 5
[0068] The AR film with better physical properties on the film surface includes, from bottom to top, a 30μm thick high-temperature protective film, a 0.2μm thick lower coating layer, a 38μm thick substrate layer, a 100nm thick upper coating layer, a 1nm thick silicon nitride layer, a 40nm thick first niobium oxide layer, a 100nm thick silicon dioxide layer, an 80nm thick second niobium oxide layer, a 120nm thick silicon-aluminum mixed layer, a 50nm thick anti-scratch layer and a 45μm thick positive protective film.
[0069] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a PC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0070] Example 6
[0071] The AR film with better physical properties on the film surface includes, from bottom to top, a 30μm thick high-temperature protective film, a 0.2μm thick lower coating layer, a 38μm thick substrate layer, a 100nm thick upper coating layer, a 0.1nm thick primer layer, a 30nm thick silicon nitride layer, a 40nm thick first niobium oxide layer, a 100nm thick silicon dioxide layer, an 80nm thick second niobium oxide layer, a 120nm thick silicon-aluminum mixed layer, a 50nm thick anti-scratch layer and a 45μm thick positive protective film.
[0072] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the base layer material is MgF2, the substrate layer is PC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2, and the anti-scratch layer is formed by coating AF coating liquid.
[0073] Example 7
[0074] The AR film with better physical properties on the film surface includes, from bottom to top, a 30μm thick high-temperature protective film, a 0.2μm thick lower coating layer, a 38μm thick substrate layer, a 100nm thick upper coating layer, a 5nm thick primer layer, a 30nm thick silicon nitride layer, a 40nm thick first niobium oxide layer, a 100nm thick silicon dioxide layer, an 80nm thick second niobium oxide layer, a 120nm thick silicon-aluminum mixed layer, a 50nm thick anti-scratch layer and a 45μm thick positive protective film.
[0075] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the base layer material is SiO, the substrate layer is PC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0076] Example 8
[0077] The AR film with better physical properties on the film surface includes, from bottom to top, a 30μm thick high-temperature protective film, a 0.2μm thick lower coating layer, a 38μm thick substrate layer, a 100nm thick upper coating layer, a 10nm thick primer layer, a 30nm thick silicon nitride layer, a 40nm thick first niobium oxide layer, a 100nm thick silicon dioxide layer, an 80nm thick second niobium oxide layer, a 120nm thick silicon-aluminum mixed layer, a 50nm thick anti-scratch layer and a 45μm thick positive protective film.
[0078] Among them, the high-temperature protective film and the positive protective film are both PET films, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the base layer material is Si, the substrate layer is PC layer, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF coating liquid.
[0079] Comparative Example 1
[0080] The only difference between this comparative example and Example 1 is that the silicon nitride layer is removed.
[0081] Comparative Example 2
[0082] The only difference between this comparative example and Example 1 is that the thickness of the silicon nitride layer is 0.2 nm.
[0083] Comparative Example 3
[0084] The only difference between this comparative example and Example 1 is that the thickness of the silicon nitride layer is 50 nm.
[0085] The AR films in the examples and comparative examples were prepared by the above-mentioned preparation method, and their performances were tested.
[0086] (1) The total light transmittance and 400-700 nm spectrophotometer light transmittance of the AR films in Example 1, Example 6 and Comparative Example 1 were tested. The results are shown in Table 1.
[0087] Table 1 Optical test data
[0088]
[0089] According to the optical test requirements, the total light transmittance needs to reach more than 95%, and the 400-700nm spectrophotometer light transmittance needs to reach more than 93%. It can be seen from Table 1 that the optical properties of the AR films in Example 1, Example 6 and Comparative Example 1 all meet the requirements.
[0090] (2) The reflection curves of the AR films in Example 1, Example 6 and Comparative Example 1 at 380-780 nm and 400-700 nm were tested. The results are as follows: Figure 3 and Figure 4 As shown, Figure 3 and Figure 4 In the figure, the old scheme refers to comparative example 1, the existing scheme 1 refers to example 6, and the existing scheme 2 refers to example 1.
[0091] According to the optical test requirements, the reflectivity of 380-780nm needs to be below 1.0%, and the reflectivity of 400-700nm needs to be below 0.5%. Figure 3It can be seen that the reflectivity at 380-780 nm of Example 1, Example 6 and Comparative Example 1 are 0.84%, 0.77% and 0.82% respectively, and the reflectivity at 400-700 nm of Example 1, Example 6 and Comparative Example 1 are 0.36%, 0.33% and 0.31% respectively, indicating that the optical properties of the AR films in Example 1, Example 6 and Comparative Example 1 all meet the requirements.
[0092] (3) Place the AR film on the glass panel and divide it into three sections, left, middle and right, according to the width of the film surface. Use a pencil hardness tester with a weight of 500g and 750g respectively, and use a 3H hardness pencil and a 4H hardness pencil to test the hardness of the coating surface. Draw 5 lines at each position during the test, and record the number of lines without scratches among the 5 lines. Result judgment: If there are 3 or more (including 3) lines without scratches among the 5 lines, it is judged as OK, and if there are less than 3 lines, it is judged as NG. The results are shown in Table 2.
[0093] Table 2 Pencil hardness test results
[0094]
[0095]
[0096] It can be seen from Table 2 that the hardness of the AR film in the embodiment of the present invention is better than that in the comparative example, indicating that by providing a silicon nitride layer or providing a silicon nitride layer and a primer layer at the same time, it can be effectively ensured that the AR film has a better hardness.
[0097] (4) Steel wool wear test: The AR film was placed on a glass panel and the wear tester was loaded with 1000 g. The number of scratches after 2000, 3000 and 5000 frictions was recorded. A scratch number ≥ 4 was judged as NG and a scratch number ≤ 3 was judged as OK. The results are shown in Table 3.
[0098] Table 3 Steel wool wear test
[0099]
[0100]
[0101] It can be seen from Table 3 that the AR film in the embodiment of the present invention has better wear resistance and can withstand 5000 frictions, and has good wear resistance.
[0102] (5) The back of the AR film was bonded with OCA optical adhesive and then bonded to the transparent glass. After bonding, the film was degassed with a degassing machine. After degassing, the surface was wiped clean. The AR film was then boiled in 100°C water for 3h and 5h, placed at double 85 (i.e., high temperature 85°C, high humidity 85%) for 32 days and 36 days, placed at 95°C for 32 days and 36 days, placed at -40°C for 32 days and 36 days, and exposed to sunlight (light intensity 0.55w / (m 2·nm), wavelength 340nm, filter Extended UV-Q / B, 3.8h of light + 1h of darkness as one cycle. The temperature of the blackboard during the light exposure was set at 89℃, the temperature of the box was 63℃, and the humidity was 50%; the temperature of the box and blackboard was set at 38℃ and the humidity was 95% during the dark stage) for 32 days and 36 days, and then a hundred grids were cut with a hundred grid knife, and then 3M company 681 type tape was used. After pressing and sticking, the tape was pulled off after standing for more than 30s. No peeling was 5B, slight peeling was 3-4B, barely OK, and NG was judged below 2B. The results are shown in Table 4.
[0103] Table 4 Comparison of various environmental tests
[0104]
[0105] It can be seen from Table 4 that the AR film in the embodiment of the present invention only slightly peeled off during the test, while the AR film in the comparative example peeled off more seriously, indicating that the high temperature resistance of the AR film can be improved by providing a silicon nitride layer, and at the same time, providing a base layer can improve the adhesion of the coating, thereby further improving the high temperature resistance of the AR film.
[0106] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0107] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An AR film with better physical properties on the film surface, characterized in that: The invention comprises a substrate layer, on which an upper coating layer, a silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer are arranged in sequence, and the thickness of the silicon nitride layer is 1-30nm.
2. The AR film with better film surface physical properties according to claim 1, characterized in that: A primer layer is also provided between the upper coating layer and the silicon nitride layer, and the primer layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y.
3. The AR film with better film surface physical properties according to claim 2, characterized in that: The thickness of the base layer is 0.1-10 nm.
4. The AR film with better film surface physical properties according to claim 1, characterized in that: The first niobium oxide layer has a thickness of 1-50 nm.
5. The AR film with better film surface physical properties according to claim 1, characterized in that: The thickness of the silicon dioxide layer is 10 to 260 nm.
6. The AR film with better film surface physical properties according to claim 1, characterized in that: The second niobium oxide layer has a thickness of 5 to 280 nm.
7. The AR film with better film surface physical properties according to claim 1, characterized in that: The thickness of the silicon-aluminum mixed layer is 50 to 310 nm; and / or, The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms.
8. The AR film with better film surface physical properties according to claim 1, characterized in that: The anti-scratch layer is formed by coating the AF coating liquid and has a thickness of 2 to 190 nm.
9. A process for preparing an AR film with better physical properties on the film surface, characterized in that: The following steps are involved: A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer; A silicon nitride layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; wherein the thickness of the silicon nitride layer is 1 to 30 nm; Disposing an anti-scratch layer on the silicon-aluminum mixed layer; A positive protective film is provided on the anti-scratch layer.
10. The process for preparing an AR film with better film surface physical properties according to claim 9, characterized in that: A primer layer is also plated between the upper coating layer and the silicon nitride layer.
Citation Information
Patent Citations
High-weather-resistance high-reflection film and preparation process thereof
CN118465899A
Low-reflection and low-transmission optical thin film with ink layer and preparation method of low-reflection and low-transmission optical thin film
CN118483775A
Anti-reflection AR film
CN217385868U
Superhard low-reflection film, display device and electronic equipment
CN221199977U
Screen protection film and manufacturing method therefor
WO2022134197A1