Method for improving doping concentration uniformity of silicon carbide epitaxial wafer through double doping
By employing a dual doping scheme using N2 and NH3, the problem of non-uniform doping in silicon carbide epitaxial wafers was solved, achieving high-quality doping uniformity and efficient production, which is suitable for mass production of silicon carbide epitaxial wafers.
Patent Information
- Application Number
- CN202411129532.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing silicon carbide epitaxial wafers have the problem of uneven doping concentration, especially when doped with a single N2 or NH3, resulting in a U-shaped or A-shaped distribution of doping concentration within the wafer. This makes it difficult to meet the uniformity requirements of mass production and requires frequent adjustments to the process formulation.
By employing a dual-doping scheme of N2 and NH3, the flow rates of N2 and NH3 are calculated and optimized by measuring the doping efficiency at each coordinate point, thereby forming a linear doping concentration distribution and improving doping uniformity.
It achieves uniform control of doping concentration within silicon carbide wafers at <2%, reduces inter-furnace concentration drift, lowers production costs, improves production efficiency, and is suitable for mass epitaxial production.
Smart Images

Figure CN119028807A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductors, and in particular to a method for improving the uniformity of doping concentration of a silicon carbide epitaxial wafer by double doping. Background Art
[0002] Silicon carbide materials have excellent electrical properties such as wide bandgap, high breakdown electric field, high saturation drift rate, and high thermal conductivity. They are particularly suitable for making high-power, high-frequency, high-temperature, and radiation-resistant electronic devices. They are widely used in the fields of solar and wind power generation, rail transportation, smart grids, and electric vehicles. The thickness, doping concentration, and uniformity of silicon carbide epitaxial wafers play an important role in the specifications of silicon carbide devices such as withstand voltage and current. At present, the non-uniformity of doping concentration of silicon carbide epitaxial wafers produced by various manufacturers can be achieved to <5%.
[0003] Single-wafer and multi-wafer SiC epitaxial furnaces are mainly developed by changing the N 2 The uniformity of doping concentration can be adjusted by adjusting the flow rate and ratio, C / Si ratio, temperature, main hydrogen flow rate and other parameters. Although the uniformity of doping concentration can be adjusted relatively well, the uniformity can be controlled at <5%. However, due to the complex relationship between the epitaxial furnace air flotation structure and the temperature field, N 2 The single doping scheme makes the doping in the wafer uneven, and the doping concentration curve presents a U-shaped distribution, as shown in Figure 1 .
[0004] In addition to N 2 Outside, NH 3 It can also be used as an N-type dopant for silicon carbide epitaxy. 3 The dissociation energy of N 2 The dissociation energy of NH is different (945 kJ / mol). 3 The thermal decomposition temperature is 400-500℃, and N 2 The decomposition temperature of NH 3 The doping efficiency is much higher than that of N 2 NH 3 Although the doping efficiency of NH is high, when used as a single dopant, it is also limited by the complex relationship between the gas flotation structure and the temperature field of the epitaxial furnace. 3 The single doping scheme makes the doping in the wafer uneven, and the doping concentration curve shows an A-type distribution. Figure 2 .
[0005] In addition, the average doping concentration will drift significantly as the number of furnaces increases. Therefore, epitaxial process engineers need to adjust the process formula in real time and verify the concentration of the epitaxial wafer to control the doping concentration and uniformity. This often requires several growths to obtain a process formula that meets the requirements. Considering the cost and efficiency issues, N 2 or NH3 The single doping scheme is not conducive to the mass production of silicon carbide epitaxial wafers. Summary of the invention
[0006] The present invention aims at the above-mentioned problems, overcomes at least one disadvantage, and proposes a method for improving the uniformity of doping concentration of silicon carbide epitaxial wafers by double doping.
[0007] The technical solution adopted by the present invention is as follows:
[0008] A method for improving the uniformity of doping concentration of a silicon carbide epitaxial wafer by dual doping comprises the following steps:
[0009] Using a single N 2 Doped epitaxy, N 2 The flow rate is A sccm, and the N at the selected x coordinate points on the silicon carbide wafer is measured. 2 Doping concentration Bi, get N at each coordinate point 2 Doping efficiency Ci, Ci = Bi / A;
[0010] Use single NH 3 Doped epitaxy, NH 3 The flow rate is D sccm, and the NH 3 Doping concentration Ei, get NH at each coordinate point 3 Doping efficiency Fi, Fi = Ei / D;
[0011] Calculate N 2 and NH 3 When double doped N 2 and NH 3 Flow rate: doping concentration target value is set to G, doping concentration tolerance is set to M, N 2 The flow rate is set to I sccm, NH 3 The flow rate is set to J sccm. At this time, the selected x coordinate points on the silicon carbide wafer are N 2 and NH 3 The double doping concentration is Ki, Ki = Ci*I + Fi*J, which is determined by N at x different coordinate points on the silicon carbide wafer. 2 and NH 3 The double doping concentration is N 2 and NH 3 The average value of the dual doping concentration L, The N at different coordinate points on the silicon carbide wafer 2 and NH 3 Maximum value of dual doping concentration Max(Ki), N 2 and NH 3 Minimum value of dual doping concentration Min(Ki) and N 2 and NH 3The average value of the dual doping concentration L is used to obtain the doping concentration tolerance M. By setting two constraints, we can get N 2 The specific value of flow I and NH 3 The specific value of the flow rate J, one of the constraints is that L reaches the doping concentration target value G, and the other constraint is that the doping concentration tolerance M takes the minimum value;
[0012] Using N 2 and NH 3 Double doping for epitaxy, where N 2 The flow rate is I sccm, NH 3 The flow rate is J sccm, and the x different coordinate points N on the silicon carbide wafer are measured. 2 and NH 3 The actual doping concentration average value L' and the actual doping concentration tolerance M' are obtained, and it is judged whether the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than the first set value, and the deviation rate = (L'-G) / G×100%. Whether the actual doping concentration tolerance M' is less than the second set value, if the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than the first set value and the actual doping concentration tolerance M' is less than the second set value, continuous production can be repeated, otherwise the concentration correction factor N is used to adjust N 2 Flow and NH 3 The flow rate is adjusted, and the specific value of the concentration correction factor N is obtained by the formula G = N*L'. 2 The flow rate is adjusted to N*I sccm, and NH 3 The flow rate was adjusted to N*J sccm.
[0013] This application proposes N 2 +NH 3 The dual-doping solution combines single-doped N 2 The U-shaped concentration profile and single-doped NH 3 The resulting type A concentration distribution, using N 2 +NH 3 The dual-doping solution can flatten the concentration distribution in the silicon carbide wafer to form a linear distribution, thereby completely improving the uniformity of the doping concentration, and the uniformity can be controlled to <2%. In addition, the concentration drift between furnaces is very small, and there is no need to adjust the epitaxial process recipe in real time to ensure that the concentration average and uniformity are within the required range. This application has the advantages of saving costs, improving production efficiency, ensuring high-quality epitaxial uniformity, and being suitable for large-scale epitaxial production.
[0014] In one embodiment of the present invention, the first setting value is 2%-3%.
[0015] In one embodiment of the present invention, the first setting value is 1%-2%.
[0016] In one embodiment of the present invention, the doping concentration on the silicon carbide wafer is measured by a mercury probe CV device.
[0017] In one embodiment of the present invention, the x is any value between 5 and 25.
[0018] In one embodiment of the present invention, silicon carbide wafers are doped and epitaxially grown using epitaxial equipment, and the epitaxial equipment is a horizontal single-wafer or multi-wafer epitaxial furnace, a vertical single-wafer or multi-wafer epitaxial furnace, a hot-wall horizontal CVD, a warm-wall planetary CVD, or a quasi-hot-wall vertical CVD.
[0019] In one embodiment of the present invention, the size of the silicon carbide wafer is 4 inches to 12 inches.
[0020] In one embodiment of the present invention, the size of the silicon carbide wafer is 4 inches, 6 inches, 8 inches or 12 inches.
[0021] The beneficial effects of the present invention are: the present application proposes N 2 +NH 3 The dual-doping solution combines single-doped N 2 The U-shaped concentration profile and single-doped NH 3 The resulting type A concentration distribution, using N 2 +NH 3 The dual-doping solution can flatten the concentration distribution in the silicon carbide wafer to form a linear distribution, thereby completely improving the uniformity of the doping concentration, and the uniformity can be controlled to <2%. In addition, the concentration drift between furnaces is very small, and there is no need to adjust the epitaxial process recipe in real time to ensure that the concentration average and uniformity are within the required range. This application has the advantages of saving costs, improving production efficiency, ensuring high-quality epitaxial uniformity, and being suitable for large-scale epitaxial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Single doping N 2 Schematic diagram of the U-shaped curve of epitaxial wafer doping concentration;
[0023] Figure 2 Is a single doped NH 3 Schematic diagram of type A curve of epitaxial wafer doping concentration;
[0024] Figure 3 Double doped N 2 and NH 3 Schematic diagram of the linear curve of epitaxial wafer doping concentration;
[0025] Figure 4 Is to use N 2 and NH 3Double-doped SiC epitaxial doping process, repeated continuous production of 4 runs of on-chip doping concentration distribution curve;
[0026] Figure 5 Is to use N 2 and NH 3 Dual-doped SiC epitaxial doping process, summary of the mean and uniformity data of the on-wafer doping concentration for four consecutive runs;
[0027] Figure 6 The present invention is a flowchart schematic diagram of a method for improving the uniformity of doping concentration of silicon carbide epitaxial wafers by double doping. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0029] In the description of this application, it should be noted that the terms "inside", "outside", etc. indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the application is usually placed when in use, which is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0030] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "disposed" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0031] The present invention is described in detail below in conjunction with the accompanying drawings.
[0032] like Figure 6 As shown, a method for improving the uniformity of doping concentration of a silicon carbide epitaxial wafer by dual doping comprises the following steps:
[0033] Using a single N 2 Doped epitaxy, N 2The flow rate is A sccm, and the N 2 Doping concentration Bi, get N at each coordinate point 2 Doping efficiency Ci (i = 1, 2, 3, 4, 5), Ci = Bi / A, see Table 1 for details;
[0034] Table 1 (different coordinate points N 2 Doping concentration and doping efficiency)
[0035]
[0036] Use single NH 3 Doped epitaxy, NH 3 The flow rate is D sccm, and the NH 3 Doping concentration Ei, get NH at each coordinate point 3 Doping efficiency Fi (i = 1, 2, 3, 4, 5), Fi = Ei / D, see Table 2 for details;
[0037] Table 2 (NH at different coordinate points 3 Doping concentration and doping efficiency)
[0038]
[0039] Calculate N 2 and NH 3 When double doped N 2 and NH 3 Traffic volume:
[0040] The doping concentration target value is set to G, and the doping concentration tolerance is set to M, N 2 The flow rate is set to I sccm, NH 3 The flow rate is set to Jsccm. At this time, the x coordinate points selected on the silicon carbide wafer are N 2 and NH 3 The double doping concentration is Ki, Ki = Ci*I + Fi*J (i = 1, 2, 3, 4, 5), see Table 3 for details; N at x different coordinate points on the silicon carbide wafer 2 and NH 3 The double doping concentration is N 2 and NH 3 The average value of the dual doping concentration L, The N at different coordinate points on the silicon carbide wafer 2 and NH 3 Maximum value of dual doping concentration Max(Ki), N 2 and NH 3 Minimum value of dual doping concentration Min(Ki) and N 2 and NH3 The average value of the dual doping concentration L is used to obtain the doping concentration tolerance M. By setting two constraints, we can get N 2 The specific value of flow I and NH 3 The specific value of the flow rate J, one of the constraints is that L reaches the doping concentration target value G, and the other constraint is that the doping concentration tolerance M takes the minimum value;
[0041] Table 3.N 2 and NH 3 Doping concentration at different coordinate points during double doping.
[0042]
[0043] Using N 2 and NH 3 Double doping for epitaxy, where N 2 The flow rate is I sccm calculated in the previous step, NH 3 The flow rate is J sccm calculated in the previous step. The actual N at five different coordinate points on the silicon carbide wafer is measured by mercury probe CV and other equipment. 2 and NH 3 The specific coordinates of the dual doping concentration K'i are the same as above, and the actual average doping concentration L' is obtained. and the actual doping concentration tolerance M', determine whether the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than the first set value, the deviation rate = (L'-G) / G × 100%, whether the actual doping concentration tolerance M' is less than the second set value, if the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than the first set value and the actual doping concentration tolerance M' is less than the second set value, then continuous production can be repeated, otherwise the concentration correction factor N is used to adjust N 2 Flow and NH 3 The flow rate is adjusted, and the specific value of the concentration correction factor N is obtained by the formula G = N*L'. 2 The flow rate is adjusted to N*I sccm, and NH 3 The flow rate was adjusted to N*J sccm.
[0044] like Figure 3 , Figure 4 and Figure 5 As shown, this embodiment proposes N 2 +NH 3 The dual-doping solution combines single-doped N 2 The U-shaped concentration profile and single-doped NH 3 The resulting type A concentration distribution, using N 2 +NH 3The dual-doping solution can flatten the concentration distribution in the silicon carbide wafer to form a linear distribution (see Figure 3 ), thereby thoroughly improving the uniformity of doping concentration, and the uniformity can be controlled to <2%. In addition, the concentration drift between furnaces is very small, and there is no need to adjust the epitaxial process recipe in real time to ensure that the concentration average value and uniformity are within the required range. The present application has the advantages of saving costs, improving production efficiency, ensuring high-quality epitaxial uniformity, and being suitable for large-scale epitaxial production.
[0045] The N mentioned in this embodiment 2 The flow rate is Asccm, which is not a normal production value but a set value, so that the corresponding doping concentration range is 1E16~6E16 (a high concentration is selected to reduce the error of mercury probe CV concentration test). It is mainly used to calculate the N corresponding to different positions on the chip. 2 Doping efficiency, the same as the NH 3 The flow rate is D sccm, which is the set value.
[0046] It should be noted that “single N 2 Doped epitaxy", "single NH 3 Doped epitaxy", "N 2 and NH 3 Double doping epitaxy", among these three doping process parameters, only N 2 Flow, NH 3 The flow rates are different, but other parameters are the same (other parameters include C / Si ratio, chamber pressure, temperature, main hydrogen flow rate, etc.).
[0047] In actual use, the first set value is 1% to 3%, preferably 2%. The x is any value between 5 and 25.
[0048] In actual use, silicon carbide wafers are doped and epitaxially grown through epitaxial equipment, which may be a horizontal single-wafer or multi-wafer epitaxial furnace, a vertical single-wafer or multi-wafer epitaxial furnace, a hot-wall horizontal CVD, a warm-wall planetary CVD or a quasi-hot-wall vertical CVD.
[0049] In actual application, this embodiment can be applied to the manufacture of 4-inch, 6-inch, 8-inch or 12-inch silicon carbide wafers. When the embodiment is used for specific epitaxy, a buffer layer is first epitaxially grown on the silicon carbide substrate. The buffer layer is only doped with N 2 (temperature 1550℃~1670℃, chamber pressure 80mbar~120mbar, carbon-silicon ratio 0.9~1.5, growth rate 2um / h~15um / h, growth time 4min~30min), and then epitaxially grow a voltage-resistant layer, which is doped with N 2 and NH 3(temperature 1550°C~1670°C, chamber pressure 80mbar~120mbar, carbon-silicon ratio 0.3~1.3, growth rate 20um / h~90um / h, growth time 8min~36min).
[0050] The above description is only a preferred embodiment of the present invention, and does not limit the patent protection scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention and the drawings, directly or indirectly used in other related technical fields, is also included in the protection scope of the present invention.
Claims
1. A method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping, characterized in that: The following steps are involved: Using single N2 doping epitaxy, the N2 flow rate is A sccm, and the N2 doping concentration Bi at the selected x coordinate points on the silicon carbide wafer is measured to obtain the N2 doping efficiency Ci at each coordinate point, Ci = Bi / A; Using single NH3 doping epitaxy, the NH3 flow rate is D sccm, and the NH3 doping concentration Ei at the selected x coordinate points on the silicon carbide wafer is measured to obtain the NH3 doping efficiency Fi at each coordinate point, Fi = Ei / D; Calculate the flow rates of N2 and NH3 when N2 and NH3 are co-doped: the doping concentration target value is set to G, the doping concentration tolerance is set to M, the N2 flow rate is set to I sccm, and the NH3 flow rate is set to J sccm. At this time, the N2 and NH3 co-doping concentrations at the x selected coordinate points on the silicon carbide wafer are Ki, Ki = Ci*I + Fi*J. The average value L of the N2 and NH3 co-doping concentrations is obtained from the N2 and NH3 co-doping concentrations at x different coordinate points on the silicon carbide wafer. The doping concentration tolerance M is obtained from the maximum value Max(Ki) of the dual doping concentration of N2 and NH3, the minimum value Min(Ki) of the dual doping concentration of N2 and NH3 and the average value L of the dual doping concentration of N2 and NH3 at different coordinate points on the silicon carbide wafer. By setting two constraints, the specific values of the N2 flow rate I and the NH3 flow rate J are obtained through optimization. One constraint is that L reaches the doping concentration target value G, and the other constraint is that the doping concentration tolerance M takes the minimum value. N2 and NH3 dual doping is used for epitaxy, wherein the N2 flow rate is I sccm and the NH3 flow rate is J sccm. The dual doping concentrations of N2 and NH3 at x different coordinate points on the silicon carbide wafer are measured to obtain an actual doping concentration average value L' and an actual doping concentration tolerance M'. It is determined whether the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than a first set value, and whether the actual doping concentration tolerance M' is less than a second set value. If the deviation rate between the actual doping concentration average value L' and the doping concentration target value G is less than the first set value and the actual doping concentration tolerance M' is less than the second set value, continuous production can be repeated. Otherwise, the N2 flow rate and the NH3 flow rate are adjusted by a concentration correction factor N. The specific value of the concentration correction factor N is obtained by the formula G=N*L'. The N2 flow rate is adjusted to N*I sccm, and the NH3 flow rate is adjusted to N*J sccm.
2. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The first set value is 2% to 3%.
3. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The first set value is 1% to 2%.
4. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The doping concentration on the silicon carbide wafer was measured using a mercury probe CV device.
5. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The x is any value between 5 and 25.
6. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The silicon carbide wafer is doped and epitaxially grown by epitaxial equipment, which is a horizontal single-wafer or multi-wafer epitaxial furnace, a vertical single-wafer or multi-wafer epitaxial furnace, a hot-wall horizontal CVD, a warm-wall planetary CVD or a quasi-hot-wall vertical CVD.
7. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 1, characterized in that: The size of silicon carbide wafers ranges from 4 inches to 12 inches.
8. The method for improving the uniformity of doping concentration of silicon carbide epitaxial wafer by dual doping as claimed in claim 7, characterized in that: The sizes of silicon carbide wafers are 4 inches, 6 inches, 8 inches or 12 inches.
Citation Information
Patent Citations
Light-emitting diode epitaxial growth method
CN103560181A
Epitaxial wafer
CN103789822A
Triaxial test method for doping concentration of silicon carbide epitaxial wafer
CN110783218A
Method and device for correcting doping concentration, electronic equipment and storage medium
CN116858854A
Epitaxial growth control method
CN117438348A
Cited By
Ammonia doping system for epitaxy and doping method
CN123063852A
Method and system for growing crystal by means of epitaxy, and method and system for growing epitaxial wafer by means of epitaxy
WO2026112819A1