Semiconductor structure and forming method of semiconductor structure
By forming an epitaxial stress layer with opposite stress directions on the non-functional surface of the wafer, the warping problem caused by mismatch of thermal expansion coefficients in the three-dimensional integrated circuit is solved, and the adjustment of the wafer warpage is achieved within the preset range, which improves the Processing stability and reduce manufacturing costs.
Patent Information
- Application Number
- CN202411132691.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
In existing three-dimensional integrated circuits, due to the mismatch of thermal expansion coefficients of different stacking materials, the wafer generates residual stress when the temperature drops, resulting in wafer warping, affecting processing and device manufacturing costs.
An epitaxial stress layer is formed on the non-functional surface surface of the wafer, and the stress direction is opposite to the stress direction generated by the warping of the wafer, so as to neutralize and offset the stress of the wafer and improve the warping situation. The material of the epitaxial stress layer can be carbon silicon or silicon germanium, and is prepared by an epitaxial growth process, and the stress direction and strength are adjusted in segments according to the warpage of the wafer.
It effectively improves the warpage of the wafer, so that its warpage meets the preset range, and improves the processing stability of the wafer and device manufacturing cost.
Smart Images

Figure CN119028809A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor structure and a method for forming the semiconductor structure. Background Art
[0002] As technology development follows Moore's Law, three-dimensional integrated circuits (3D ICs) are attracting more and more attention from researchers. The development direction of existing 3D integrated circuits has shifted from the horizontal plane to the vertical plane, such as 3D memory, 3D through-silicon vias, and monolithic 3D.
[0003] Due to the mismatch in the coefficient of thermal expansion (CTE) between different stacked materials deposited on the wafer, as the temperature decreases, the film and the wafer shrink at different rates, and the residual stress generated in the wafer causes the wafer to bend up or down, resulting in wafer warpage.
[0004] If the curvature or warping of the wafer is too large or the warping is different in different directions, the wafer processing will be restricted or even the wafer cannot be processed on the same machine, thereby increasing the device manufacturing cost.
[0005] Therefore, improving the warpage of wafers is an ongoing issue that needs to be addressed. Summary of the invention
[0006] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the semiconductor structure to improve the warping of a wafer.
[0007] To solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, comprising: providing a wafer, the wafer comprising a functional surface and a non-functional surface; forming a functional layer structure on the surface of the functional surface; obtaining the warping condition of the wafer; and forming an epitaxial stress layer on the surface of the non-functional surface according to the warping condition, the stress direction generated by the epitaxial stress layer being opposite to the stress direction generated by the warping of the wafer.
[0008] Optionally, the warping of the wafer includes: the wafer is bent toward a non-functional surface, or the wafer is bent toward a functional surface.
[0009] Optionally, when the wafer is bent toward the functional surface, the non-functional surface has tensile stress; and the epitaxial stress layer has compressive stress.
[0010] Optionally, the material of the epitaxial stress layer includes: carbon silicon.
[0011] Optionally, when the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress; and the epitaxial stress layer has tensile stress.
[0012] Optionally, the material of the epitaxial stress layer includes: silicon germanium.
[0013] Optionally, according to the warping condition, an epitaxial stress layer is formed on the non-functional surface, including: obtaining the warping of the wafer; if the warping of the wafer is within a first preset value range, an epitaxial stress layer having a first stress is formed; if the warping of the wafer is within a second preset value range, an epitaxial stress layer having a second stress is formed, the second preset value range is greater than the first preset value range, and the second stress is greater than the second stress.
[0014] Optionally, the first preset value range is less than 200 microns; the second preset value range is 200 microns to 500 microns.
[0015] Optionally, the wafer is bent toward the non-functional surface, and the material of the epitaxial stress layer includes silicon germanium; the mass range of the germanium element in the epitaxial stress layer having the first stress is smaller than the mass range of the germanium element in the epitaxial stress layer having the second stress.
[0016] Optionally, the mass range of germanium element in the epitaxial stress layer with the first stress is 5% to 10%; the mass range of germanium element in the epitaxial stress layer with the second stress is 10% to 25%.
[0017] Optionally, the process of forming an epitaxial stress layer having a first stress includes a first epitaxial growth process, and parameters of the first epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of the silane and germane ranges from 10:1 to 20:1; the process of forming an epitaxial stress layer having a second stress includes a second epitaxial growth process, and parameters of the second epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of the silane and germane ranges from 4:1 to 10:1.
[0018] Optionally, the wafer is bent toward the functional surface, and the material of the epitaxial stress layer includes carbon silicon; the mass range of carbon elements in the epitaxial stress layer having the first stress is smaller than the mass range of carbon elements in the epitaxial stress layer having the second stress.
[0019] Optionally, the mass range of carbon elements in the epitaxial stress layer with the first stress is 1% to 1.5%; the mass range of carbon elements in the epitaxial stress layer with the second stress is 1.5% to 2%.
[0020] Optionally, the process of forming an epitaxial stress layer having a first stress includes a first epitaxial growth process, and parameters of the first epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 75:1 to 100:1; the process of forming an epitaxial stress layer having a second stress includes a second epitaxial growth process, and parameters of the second epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 50:1 to 75:1.
[0021] Optionally, before the initial stress layer is formed on the surface of the non-functional surface, the method further includes: forming a protective layer on the surface of the functional layer structure.
[0022] Optionally, the method further includes: obtaining a warping condition of the wafer, wherein the warping degree of the wafer is within a preset range.
[0023] Correspondingly, the technical solution of the present invention also provides a semiconductor structure, including: a wafer, the wafer including a functional surface and a non-functional surface; a functional layer structure located on the surface of the functional surface; an epitaxial stress layer located on the surface of the non-functional surface, the stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the warping of the wafer, and the warping degree of the wafer is within a preset range.
[0024] Optionally, the warping of the wafer includes: the wafer is bent toward a non-functional surface, or the wafer is bent toward a functional surface.
[0025] Optionally, when the wafer is bent toward the functional surface, the non-functional surface has tensile stress; and the epitaxial stress layer has compressive stress.
[0026] Optionally, the material of the epitaxial stress layer includes carbon silicon.
[0027] Optionally, when the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress; and the epitaxial stress layer has tensile stress.
[0028] Optionally, the material of the epitaxial stress layer includes: silicon germanium.
[0029] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0030] The formation method of the present invention forms an epitaxial stress layer on the surface of the non-functional surface. The stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping, and the stress on the wafer surface can be neutralized and offset, so that the warping of the wafer is improved and the warping degree of the wafer meets the preset range.
[0031] Further, when the wafer is bent toward the functional surface, the surface of the non-functional surface has tensile stress, the epitaxial stress layer has compressive stress, and the material of the epitaxial stress layer includes carbon silicon. When the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress, the epitaxial stress layer has tensile stress, and the material of the epitaxial stress layer includes silicon germanium. The epitaxial stress layer is set according to the warping of the wafer, so that the epitaxial stress layer can neutralize and offset the stress on the surface of the wafer, so that the warping of the wafer is improved, and the warping degree of the wafer meets the preset range.
[0032] Furthermore, when the warpage of the wafer is within a first preset value range, an epitaxial stress layer having a first stress is formed; when the warpage of the wafer is within a second preset value range, an epitaxial stress layer having a second stress is formed, the second preset value range is greater than the first preset value range, and the second stress is greater than the second stress. By setting the stress of the epitaxial stress layer in sections according to the specific conditions of the warpage of the wafer, the warpage of the wafer can be better adjusted, so that the warpage of the wafer is improved, and the warpage of the wafer meets the preset range. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a schematic flow chart of a method for forming a semiconductor structure in an embodiment of the present invention;
[0034] Figures 2 to 4 is a structural schematic diagram of a formation process of a semiconductor structure in one embodiment of the present invention;
[0035] Figure 5 and Figure 6 It is a structural schematic diagram of a formation process of a semiconductor structure in another embodiment of the present invention. DETAILED DESCRIPTION
[0036] As described in the background art, improving the warpage of wafers is a problem that needs to be solved continuously.
[0037] Specifically, methods for improving the wafer warpage problem generally include: (1) thermal annealing: usually used to solve isotropic wafer warpage, with the property of heating the whole wafer, so that the speed of rapid heating of different areas of the wafer is inconsistent, resulting in uneven temperature field distribution, which leads to uneven thermal deformation of the wafer; (2) ion implantation: by doping ions to generate stress opposite to the warpage, the degree of warpage is reduced, but at the same time, it is necessary to add a back mask and implantation process, which is complicated; (3) thin film deposition: an auxiliary film with the opposite stress type to the wafer is formed on the back to offset the stress of the wafer. Conventional PECVD can prepare thin films through a high-frequency power source, but the stress of the obtained thin film is low and cannot effectively improve the warpage of the wafer.
[0038] In order to solve the above problems, the technical solution of the present invention provides a semiconductor structure and a method for forming a semiconductor structure, by forming an epitaxial stress layer on the surface of a non-functional surface. The stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping, and the stress on the surface of the wafer can be neutralized and offset, so that the warping of the wafer is improved, and the warping degree of the wafer meets the preset range.
[0039] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0040] Figure 1 It is a schematic flow chart of a method for forming a semiconductor structure in an embodiment of the present invention.
[0041] Please refer to Figure 1 , the process of the method for forming the semiconductor structure includes:
[0042] Step S10: providing a wafer, wherein the wafer includes a functional surface and a non-functional surface;
[0043] Step S20: forming a functional layer structure on the surface of the functional surface;
[0044] Step S30: obtaining the warpage condition of the wafer;
[0045] Step S40: forming an epitaxial stress layer on the surface of the non-functional surface according to the warping condition, wherein the stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping.
[0046] The formation method forms an epitaxial stress layer on the surface of the non-functional surface. The stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping, and the stress on the surface of the wafer can be neutralized and offset, so that the warping of the wafer is improved and the warping degree of the wafer meets the preset range.
[0047] The warping of the wafer includes: the wafer is bent toward the non-functional surface, or the wafer is bent toward the functional surface.
[0048] In one embodiment, when the wafer is bent toward the functional surface, the non-functional surface has tensile stress; and the epitaxial stress layer has compressive stress.
[0049] In this embodiment, when the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress; and the epitaxial stress layer has tensile stress.
[0050] Next, combine Figures 2 to 4 Each step is analyzed and explained. Figures 2 to 4 It is a structural schematic diagram of a formation process of a semiconductor structure in one embodiment of the present invention.
[0051] Please combine Figure 2 Execute step S10: provide a wafer 100, wherein the wafer 100 includes a functional surface S1 and a non-functional surface S2; execute step S20: form a functional layer structure on the surface of the functional surface S1.
[0052] The functional layer structure includes a stack of multiple thin films, the stresses between the multiple thin films are mismatched, and the stresses between the functional layer structure and the wafer 100 are mismatched.
[0053] In this embodiment, the material of the wafer includes silicon.
[0054] In other embodiments, the material of the wafer includes silicon carbide, silicon germanium, a multi-component semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multi-component semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.
[0055] Please continue to refer to Figure 2 , further comprising: forming a protective layer 101 on the surface of the functional layer structure.
[0056] The protective layer 101 is used to protect the surface of the functional layer structure.
[0057] In this embodiment, the material of the protection layer 101 includes silicon oxide.
[0058] Please continue to combine Figure 2 Execute step S30: obtain the warping condition of the wafer 100 .
[0059] In this embodiment, the warping condition of the wafer 100 includes: the wafer 100 is bent toward the non-functional surface S2.
[0060] In this embodiment, the warping condition of the wafer 100 also includes: the warping degree of the wafer 100 toward the non-functional surface S2 is greater than a preset value.
[0061] The preset value is a standard value for determining whether wafer warpage will affect production and yield. Wafers with a warpage within the preset range meet production and yield requirements.
[0062] Please combine Figure 3 Executing step S40 : forming an epitaxial stress layer 102 on the surface of the non-functional surface S2 according to the warping condition, wherein the stress direction generated by the epitaxial stress layer 102 is opposite to the stress direction generated by the warping of the wafer 100 .
[0063] In this embodiment, according to the warping condition, an epitaxial stress layer 102 is formed on the surface of the non-functional surface S2, including: obtaining the warping of the wafer 100; if the warping of the wafer 100 is within a first preset value range, an epitaxial stress layer 102 with a first stress is formed; if the warping of the wafer 100 is within a second preset value range, an epitaxial stress layer 102 with a second stress is formed, the second preset value range is greater than the first preset value range, and the second stress is greater than the second stress.
[0064] By setting the stress of the epitaxial stress layer 102 in segments according to the specific conditions of the warpage of the wafer 100 , the warpage of the wafer 100 can be better adjusted, so that the warpage of the wafer 100 is improved and the warpage of the wafer 100 meets a preset range.
[0065] In this embodiment, the first preset value range is less than 200 microns; the second preset value range is 200 microns to 500 microns.
[0066] Preferably, the first preset value range is greater than 20 microns and less than 200 microns.
[0067] That is, when the warping degree of the wafer 100 toward the non-functional surface S2 is small, an epitaxial stress layer 102 with small stress is formed; when the warping degree of the wafer 100 toward the non-functional surface S2 is large, an epitaxial stress layer 102 with large stress is formed.
[0068] In this embodiment, the wafer 100 is bent toward the non-functional surface S2 , and compressive stress is generated on the surface of the non-functional surface S2 of the wafer 100 ; and the epitaxial stress layer 102 has tensile stress.
[0069] In this embodiment, the material of the epitaxial stress layer 102 includes silicon germanium. The process of forming the epitaxial stress layer 102 includes an epitaxial growth process.
[0070] The lattice constant of silicon is The lattice constant of germanium is The mismatch rate between silicon and germanium is 4.09%, which makes the lattice constant of silicon germanium greater than that of pure silicon. Silicon germanium strained material is grown epitaxially on a silicon substrate. A portion of germanium forms a silicon germanium structure with the silicon substrate at the interface, and the distance between atoms is larger than that between pure silicon atoms, so that the substrate silicon is subjected to outward tensile stress.
[0071] In this embodiment, when the first preset value range is less than 200 micrometers, an epitaxial stress layer 102 with a first stress is formed; when the first preset value range is 200 micrometers to 500 micrometers, an epitaxial stress layer 102 with a second stress is formed.
[0072] In this embodiment, the mass range of the germanium element in the epitaxial stress layer 102 having the first stress is smaller than the mass range of the germanium element in the epitaxial stress layer 102 having the second stress.
[0073] In this embodiment, the mass range of germanium element in the epitaxial stress layer 102 with the first stress is 5% to 10%; the mass range of germanium element in the epitaxial stress layer 102 with the second stress is 10% to 25%.
[0074] The process of forming the epitaxial stress layer 102 with the first stress includes a first epitaxial growth process, and the parameters of the first epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of silane to germane ranges from 10:1 to 20:1.
[0075] The process of forming the epitaxial stress layer 102 with the second stress includes a second epitaxial growth process, and the parameters of the second epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of silane to germane is in the range of 4:1 to 10:1.
[0076] In this embodiment, the flow rate ratio range of silane and germane for forming the epitaxial stress layer 102 with the first stress is greater than the flow rate ratio range of silane and germane for forming the epitaxial stress layer 102 with the second stress, so that the mass range of the germanium element in the epitaxial stress layer 102 with the first stress is smaller than the mass range of the germanium element in the epitaxial stress layer 102 with the second stress.
[0077] Please continue to refer to Figure 4 In this embodiment, it also includes: obtaining the warping condition of the wafer 100, and the warping degree of the wafer is within a preset range.
[0078] In this embodiment, the preset range includes: less than or equal to 20 micrometers.
[0079] Accordingly, a semiconductor structure is also provided in an embodiment of the present invention, please continue to refer to Figure 4 ,include:
[0080] Wafer 100, the wafer 100 comprises a functional surface S1 and a non-functional surface S2;
[0081] A functional layer structure located on the surface of the functional surface S1;
[0082] The epitaxial stress layer 102 is located on the surface of the non-functional surface S2 . The stress direction generated by the epitaxial stress layer 102 is opposite to the stress direction generated by the warping of the wafer 100 . The warping degree of the wafer 100 is within a preset range.
[0083] In this embodiment, when the wafer 100 is bent toward the non-functional surface S2 , the surface of the non-functional surface S2 has compressive stress; and the epitaxial stress layer 102 has tensile stress.
[0084] In this embodiment, the material of the epitaxial stress layer 102 includes silicon germanium.
[0085] Figure 5 and Figure 6 It is a structural schematic diagram of a formation process of a semiconductor structure in another embodiment of the present invention.
[0086] Please refer to Figure 5 , Figure 5 and Figure 2 The difference is that, in this embodiment, the warping condition of the wafer 100 includes: the wafer 100 is bent toward the functional surface S1.
[0087] In this embodiment, the warping condition of the wafer 100 also includes: the warping degree of the wafer 100 toward the functional surface S1 is greater than a preset value.
[0088] Please refer to Figure 6 According to the warping condition, an epitaxial stress layer 202 is formed on the surface of the functional surface S1 , and the stress direction generated by the epitaxial stress layer 202 is opposite to the stress direction generated by the warping of the wafer 100 .
[0089] In this embodiment, according to the warping condition, an epitaxial stress layer 202 is formed on the surface of the non-functional surface S2, including: obtaining the warping of the wafer 100; if the warping of the wafer 100 is within a first preset value range, an epitaxial stress layer 202 with a first stress is formed; if the warping of the wafer 100 is within a second preset value range, an epitaxial stress layer 202 with a second stress is formed, the second preset value range is greater than the first preset value range, and the second stress is greater than the second stress.
[0090] By setting the stress of the epitaxial stress layer 202 in segments according to the specific conditions of the warpage of the wafer 100 , the warpage of the wafer 100 can be better adjusted, so that the warpage of the wafer 100 is improved and the warpage of the wafer 100 meets a preset range.
[0091] In this embodiment, the first preset value range is less than 200 microns; the second preset value range is 200 microns to 500 microns.
[0092] Preferably, the first preset value range is greater than 20 microns and less than 200 microns.
[0093] That is, when the warping degree of the wafer 100 toward the functional surface S1 is small, an epitaxial stress layer 202 with small stress is formed; when the warping degree of the wafer 100 toward the functional surface S1 is large, an epitaxial stress layer 202 with large stress is formed.
[0094] In this embodiment, the wafer 100 is bent toward the functional surface S1 , and tensile stress is generated on the surface of the non-functional surface S2 of the wafer 100 ; the epitaxial stress layer 202 has compressive stress.
[0095] In this embodiment, the material of the epitaxial stress layer 202 includes carbon silicon. The process of forming the epitaxial stress layer 202 includes an epitaxial growth process.
[0096] The lattice constant of silicon is The lattice constant of carbon is The mismatch rate between carbon and silicon is 34.27%, which makes the lattice constant of carbon silicon smaller than that of pure silicon, and the lattice constant of carbon is much smaller than that of pure silicon. Carbon silicon only needs a few carbon atoms to obtain high stress. When carbon silicon strained material is epitaxially grown on a silicon substrate, a part of the carbon atoms at the interface and the silicon substrate form a carbon silicon structure. The distance between atoms is larger than that between pure silicon atoms, and the substrate silicon is subjected to inward compressive stress.
[0097] In this embodiment, when the first preset value range is less than 200 micrometers, an epitaxial stress layer 202 with a first stress is formed; when the first preset value range is 200 micrometers to 500 micrometers, an epitaxial stress layer 202 with a second stress is formed.
[0098] In this embodiment, the mass range of carbon elements in the epitaxial stress layer 202 having the first stress is smaller than the mass range of carbon elements in the epitaxial stress layer 202 having the second stress.
[0099] In this embodiment, the mass range of carbon elements in the epitaxial stress layer 202 with the first stress is 1% to 1.5%; the mass range of carbon elements in the epitaxial stress layer 202 with the second stress is 1.5% to 2%.
[0100] The process of forming the epitaxial stress layer 202 with the first stress includes a first epitaxial growth process, and the parameters of the first epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 75:1 to 100:1.
[0101] The process of forming the epitaxial stress layer 202 with the second stress includes a second epitaxial growth process, and the parameters of the second epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 50:1 to 75:1.
[0102] In this embodiment, the flow rate ratio range of neopentasilane and SiCH6 for forming the epitaxial stress layer 202 with the first stress is greater than the flow rate ratio range of neopentasilane and SiCH6 for forming the epitaxial stress layer 202 with the second stress, so that the mass range of carbon elements in the epitaxial stress layer 202 with the first stress is smaller than the mass range of carbon elements in the epitaxial stress layer 202 with the second stress.
[0103] Please continue to refer to Figure 6 In this embodiment, it also includes: obtaining the warping condition of the wafer 100, and the warping degree of the wafer is within a preset range.
[0104] In this embodiment, the preset range includes: less than or equal to 20 micrometers.
[0105] Accordingly, a semiconductor structure is also provided in an embodiment of the present invention, please continue to refer to Figure 6 ,include:
[0106] Wafer 100, the wafer 100 comprises a functional surface S1 and a non-functional surface S2;
[0107] A functional layer structure located on the surface of the functional surface S1;
[0108] The epitaxial stress layer 202 is located on the surface of the non-functional surface S2 . The stress direction generated by the epitaxial stress layer 202 is opposite to the stress direction generated by the warping of the wafer 100 . The warping degree of the wafer 100 is within a preset range.
[0109] In this embodiment, when the wafer 100 is bent toward the functional surface S1 , the surface of the non-functional surface S2 has tensile stress; and the epitaxial stress layer 102 has compressive stress.
[0110] In this embodiment, the material of the epitaxial stress layer 102 includes carbon silicon.
[0111] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a wafer, wherein the wafer comprises a functional surface and a non-functional surface; forming a functional layer structure on the surface of the functional surface; Obtaining a warpage condition of the wafer; According to the warping condition, an epitaxial stress layer is formed on the surface of the non-functional surface, and the stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping.
2. The method for forming a semiconductor structure according to claim 1, wherein: The warping of the wafer includes: the wafer is bent toward the non-functional surface, or the wafer is bent toward the functional surface.
3. The method for forming a semiconductor structure according to claim 2, wherein: When the wafer is bent toward the functional surface, the surface of the non-functional surface has tensile stress; and the epitaxial stress layer has compressive stress.
4. The method for forming a semiconductor structure according to claim 3, wherein: The material of the epitaxial stress layer includes: carbon silicon.
5. The method for forming a semiconductor structure according to claim 2, wherein: When the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress; and the epitaxial stress layer has tensile stress.
6. The method for forming a semiconductor structure according to claim 5, wherein: The material of the epitaxial stress layer includes silicon germanium.
7. The method for forming a semiconductor structure according to claim 1, wherein: According to the warping condition, an epitaxial stress layer is formed on the surface of the non-functional surface, including: obtaining the warping of the wafer; if the warping of the wafer is within a first preset value range, an epitaxial stress layer with a first stress is formed; if the warping of the wafer is within a second preset value range, an epitaxial stress layer with a second stress is formed, the second preset value range is greater than the first preset value range, and the second stress is greater than the second stress.
8. The method for forming a semiconductor structure according to claim 7, wherein: The first preset value range is less than 200 microns; the second preset value range is 200 microns to 500 microns.
9. The method for forming a semiconductor structure according to claim 7, wherein: The wafer is bent toward the non-functional surface, the material of the epitaxial stress layer includes silicon germanium, and the mass range of the germanium element in the epitaxial stress layer with the first stress is smaller than the mass range of the germanium element in the epitaxial stress layer with the second stress.
10. The method for forming a semiconductor structure according to claim 9, wherein: The mass range of germanium element in the epitaxial stress layer with the first stress is 5% to 10%; the mass range of germanium element in the epitaxial stress layer with the second stress is 10% to 25%.
11. The method for forming a semiconductor structure according to claim 10, wherein: The process of forming an epitaxial stress layer with a first stress includes a first epitaxial growth process, and the parameters of the first epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of the silane and germane ranges from 10:1 to 20:1; the process of forming an epitaxial stress layer with a second stress includes a second epitaxial growth process, and the parameters of the second epitaxial growth process include: the reaction gas includes silane and germane, and the flow rate ratio of the silane and germane ranges from 4:1 to 10:
1.
12. The method for forming a semiconductor structure according to claim 7, wherein: The wafer is bent toward the functional surface, the material of the epitaxial stress layer includes carbon silicon, and the mass range of carbon elements in the epitaxial stress layer with the first stress is smaller than the mass range of carbon elements in the epitaxial stress layer with the second stress.
13. The method for forming a semiconductor structure according to claim 12, wherein: The mass range of carbon elements in the epitaxial stress layer with the first stress is 1% to 1.5%; the mass range of carbon elements in the epitaxial stress layer with the second stress is 1.5% to 2%.
14. The method for forming a semiconductor structure according to claim 13, wherein: The process of forming an epitaxial stress layer having a first stress includes a first epitaxial growth process, and the parameters of the first epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 75:1 to 100:1; the process of forming an epitaxial stress layer having a second stress includes a second epitaxial growth process, and the parameters of the second epitaxial growth process include: the reaction gas includes neopentasilane and SiCH6, and the flow rate ratio of the neopentasilane and SiCH6 ranges from 50:1 to 75:
1.
15. The method for forming a semiconductor structure according to claim 1, wherein: Before the initial stress layer is formed on the surface of the non-functional surface, the method further includes: forming a protective layer on the surface of the functional layer structure.
16. The method for forming a semiconductor structure according to claim 1, wherein: Also includes: The warping condition of the wafer is obtained, and the warping degree of the wafer is within a preset range.
17. A semiconductor structure, characterized in that: include: A wafer, wherein the wafer comprises a functional surface and a non-functional surface; A functional layer structure located on the surface of the functional surface; The epitaxial stress layer is located on the surface of the non-functional surface, and the stress direction generated by the epitaxial stress layer is opposite to the stress direction generated by the wafer warping. The warping degree of the wafer is within a preset range.
18. The semiconductor structure according to claim 17, wherein: The warping of the wafer includes: the wafer is bent toward the non-functional surface, or the wafer is bent toward the functional surface.
19. The semiconductor structure according to claim 18, wherein: When the wafer is bent toward the functional surface, the surface of the non-functional surface has tensile stress; and the epitaxial stress layer has compressive stress.
20. The semiconductor structure according to claim 19, wherein: The material of the epitaxial stress layer includes carbon silicon.
21. The semiconductor structure according to claim 18, wherein: When the wafer is bent toward the non-functional surface, the surface of the non-functional surface has compressive stress; and the epitaxial stress layer has tensile stress.
22. The semiconductor structure according to claim 21, wherein: The material of the epitaxial stress layer includes silicon germanium.
Citation Information
Patent Citations
Semiconductor wafer, flattening method therefor, and packaging method
CN105810557A
Semiconductor structure and formation method thereof
CN108054177A
Method for improving warpage of semiconductor structure
CN108766913A
Epitaxial structure manufacturing method and epitaxial structure
CN111554563A
Method for reducing warping degree of epitaxial wafer and epitaxial wafer
CN111725051A