Method for growing high-purity 4H-SiC single crystal by PVT method
By electrochemical etching pretreatment of the Si surface of SiC substrate, the problems of multiple inclusions and high nitrogen absorption in SiC single crystal growth are solved, and the growth and cost reduction of stable and high-purity 4H-SiC single crystal are achieved.
Patent Information
- Application Number
- CN202411150487.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
During the SiC single crystal growth process, especially in the growth of high-purity semi-insulating 4H-SiC, multiple inclusion symbiosis and excessive absorption of nitrogen elements are prone to occur, resulting in high production costs and difficult to achieve high purity.
Before growing SiC crystals by PVT method, the Si surface of the SiC substrate is subjected to electrochemical etching pretreatment to provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, reduce the absorption of nitrogen elements, and stabilize high-purity 4H -Growth of SiC single crystal.
Through electrochemical etching pretreatment, the Si surface is ensured to grow a single crystal form of 4H-SiC, which reduces nitrogen absorption, improves the quality of single crystals, reduces production costs, and simplifies the preparation of high-purity semi-insulated 4H-SiC.
Smart Images

Figure CN119028812A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for growing high-purity 4H-SiC single crystal using a PVT method. Background Art
[0002] SiC has stable physical and chemical properties, and has the characteristics of wide forbidden band, high saturated electron mobility, high breakdown electric field strength, and high thermal conductivity. It is regarded as one of the most promising materials in the field of semiconductor materials. SiC crystal is also an ideal substrate for epitaxial films such as gallium nitride and silicon carbide, and has the characteristics of high lattice matching and good thermal conductivity. Compared with the first-generation semiconductor materials represented by Si and the second-generation semiconductor materials represented by GaAs, it has obvious advantages. It is an ideal semiconductor material for manufacturing optoelectronic devices, high-frequency and high-power devices, and high-temperature electronic devices. It is currently widely used in white light lighting, optical storage, screen display, aerospace, high-temperature radiation environment, oil exploration, automation, radar and communication, and automotive electronics.
[0003] At present, physical vapor transport (PVT) is the mainstream growth method of SiC single crystals. The specific growth method is: place a seed crystal on the top of the crucible, add powder at the bottom of the crucible, place the crucible heat field in a crystal growth furnace, the bottom temperature of the crucible is high, and the top temperature is low. By controlling the temperature and pressure, the bottom powder gradually sublimates and is transferred to the top seed crystal for condensation and crystallization, thereby achieving the growth of SiC single crystals. At present, this method has become the mainstream method in the industry and has achieved large-scale production of SiC.
[0004] SiC has a variety of crystal structures and different crystal forms can transform into each other. The most common crystal forms are 3C-SiC, 4H-SiC, 6H-SiC and 15R-SiC. Due to the differences in crystal structures, different crystal forms have slightly different physical and chemical properties. Due to the influence of different polar surface energies, SiC has a lower surface energy on the C surface, which is more suitable for the growth of 4H single crystals with higher nucleation energy, while the Si surface has a higher surface energy, which is suitable for the growth of 6H single crystals with lower nucleation energy. However, there are partially overlapping growth windows between different SiC crystal forms, which leads to the phenomenon of polymorphic inclusions and coexistence during the single crystal growth process. For example, in the growth process of 4H-SiC single crystals, 6H and 15R crystal forms are likely to appear; in the growth process of 6H-SiC single crystals, 4H and 15R crystal forms are likely to appear, which seriously affects the growth quality of SiC single crystals and increases production costs.
[0005] SiC single crystals generally have N-type conductivity and high-purity semi-insulating type. Epitaxial structures such as gallium nitride grown on high-purity semi-insulating SiC can be used in microwave communications and radar fields. In addition, carbon electronics based on graphene on SiC also require high-purity semi-insulating SiC single crystals. However, it is very difficult to grow high-purity semi-insulating SiC single crystals. This is because high-purity semi-insulating requires the nitrogen concentration in the single crystal to be less than 1E16cm -3 However, in the SiC single crystal growth process (physical vapor transport method, PVT method for short), the graphite materials, powders, and thermal insulation materials used are all porous or powder materials with a large surface area, which will absorb a large amount of nitrogen (the nitrogen content in the atmosphere exceeds 78%), making the preparation of high-purity semi-insulating SiC very difficult and the cost high.
[0006] In order to reduce the incorporation of nitrogen, some people have adopted a method of growing 6H-SiC single crystals on the Si surface. This is because it is more difficult to incorporate nitrogen on the Si surface of the SiC seed crystal. However, in the traditional PVT process, it is impossible to grow 4H-SiC single crystals on the Si surface, and generally only 6H-SiC single crystals can be grown on the Si surface seed crystal. However, the band gap width of the 6H-SiC single crystal is smaller than that of 4H-SiC, and the performance is worse than that of 4H. In response to this problem, the present invention proposes a method for growing high-purity semi-insulating 4H-SiC single crystals on Si surface SiC seed crystals by a PVT method. Summary of the invention
[0007] The purpose of the present invention is to provide a method for growing high-purity 4H-SiC single crystals by a PVT method, which can reduce the absorption of nitrogen while ensuring the growth of a single crystal form of 4H-SiC on the Si surface, thereby achieving the purpose of reducing costs and increasing efficiency.
[0008] To achieve the above-mentioned purpose, the present invention provides a method for growing high-purity 4H-SiC single crystal by PVT method. Before growing SiC crystal by PVT method, the Si surface of SiC substrate is pretreated by electrochemical etching to provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for 4H-SiC nucleation growth, reduce the absorption of nitrogen element, and stabilize the growth of high-purity 4H-SiC single crystal.
[0009] Preferably, the specific steps of performing electrochemical etching pretreatment on the Si surface of the SiC substrate are:
[0010] (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface;
[0011] (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;
[0012] (3) The anode and cathode are placed symmetrically, the SiC substrate is placed in the electrolyte, the power supply is connected and the Si surface of the substrate is electrochemically etched;
[0013] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
[0014] Preferably, in step (2), the C surface of the substrate and the graphite electrode are connected by conductive adhesive bonding or vacuum adsorption.
[0015] Preferably, in step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.
[0016] Preferably, in step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.
[0017] Preferably, in step (4), the electrolyte is immersed for 0-12 hours, and the ultrasonic immersion is performed in deionized water for 0-10 hours.
[0018] Preferably, in step (4), the inert gas is Ar or He.
[0019] The electrochemical etching process basically includes two parts: In the first part, holes are generated during the etching process, current is formed at the SiC-electrolyte interface, and SiC is oxidized to SiO x Thin Films, Part II, SiO x The film is dissolved in the electrolyte. The type / concentration of the electrolyte, electrochemical etching time / temperature, additional auxiliary conditions (such as ultraviolet light irradiation, ultrasonic vibration, etc.), load voltage / current, and electrode spacing will all affect the electrochemical etching effect.
[0020] The main method of the present invention is to perform electrochemical etching pretreatment on the Si surface of the SiC substrate before crystal growth and before growing SiC crystal by PVT method, and then perform PVT method 4H-SiC single crystal growth on the Si surface after the electrochemical etching pretreatment. The basic principle of electrochemical etching pretreatment is: electrochemical etching can provide more nucleation sites on the substrate, reduce the nucleation energy of 4H on the Si surface, provide a suitable window for 4H-SiC nucleation growth, break the current situation that only 6H-SiC can be grown on the Si surface and 4H-SiC can only grow on the C surface, make full use of the characteristic that nitrogen is less likely to be incorporated when growing on the Si surface, reduce the absorption of nitrogen, improve the quality of single crystal growth, avoid the generation of grain boundaries and polymorphs, thereby stabilizing the growth of high-purity 4H-SiC single crystals, and making the preparation of high-purity semi-insulating 4H-SiC easier.
[0021] Therefore, the present invention provides a method for growing high-purity 4H-SiC single crystals by the PVT method, selects a suitable substrate pretreatment scheme, utilizes electrochemical etching to reduce the surface nucleation energy of the Si surface, and reduces the absorption of nitrogen while ensuring the growth of a single crystal of 4H-SiC on the Si surface, thereby achieving the purpose of reducing costs and increasing efficiency.
[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A diagram of the device used for electrochemical etching of the present invention;
[0024] Figure 2 The thermal field structure diagram used for growing high-purity 4H-SiC single crystal by the PVT method of the present invention;
[0025] Figure 3 This is the Raman mapping image of SiC single crystal grown by PVT method without processing the Si surface of SiC substrate;
[0026] Figure 4 The Raman mapping image of SiC single crystal grown by the same round of PVT method is shown in Figure 1. The Si surface of the SiC substrate is pre-treated by electrochemical etching to form an etched area and an unetched area.
[0027] Reference Numbers
[0028] 1-anode electrode; 2-cathode electrode; 3-tetrafluoroethylene cover plate; 4-power supply; 5-electrolyte; 6-SiC substrate; 7-graphite threaded rod; 8-conducting wire; 9-upper temperature measuring hole; 10-lower temperature measuring hole; 11-upper insulation; 12-lower insulation; 13-side insulation; 14-seed crystal holder; 15-seed crystal; 16-crystal growth crucible; 17-high purity SiC powder. DETAILED DESCRIPTION
[0029] The present invention provides a method for growing high-purity 4H-SiC single crystal by a PVT method. Before growing SiC crystal by the PVT method, the Si surface of a SiC substrate is pretreated by electrochemical etching to provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for the nucleation growth of 4H-SiC, reduce the absorption of nitrogen elements, and stabilize the growth of high-purity 4H-SiC single crystal.
[0030] In the present invention, the specific steps of electrochemical etching pretreatment of the Si surface of the SiC substrate are:
[0031] (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface;
[0032] (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;
[0033] (3) The anode and cathode are placed symmetrically, and the SiC substrate with the exposed Si surface is placed in an electrolyte, and a power supply is connected to perform electrochemical etching on the Si surface of the substrate;
[0034] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
[0035] In the present invention, the device used for electrochemical etching is as follows Figure 1 As shown, it includes an anode electrode 1, a cathode electrode 2, a tetrafluoroethylene cover plate 3, a power source 4, an electrolyte 5, a SiC substrate 6, a graphite threaded rod 7, and a wire 8, wherein the anode and the cathode are placed symmetrically up and down, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the two electrodes, the distance between the cathode and the anode is 1-20 cm, the masking surface of the SiC substrate 6 is bonded to the anode electrode 1 by conductive glue or vacuum adsorption, the pre-etched surface is in contact with the electrolyte 5, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the anode electrode 1 (graphite electrode) and the cathode electrode 2 (graphite electrode), the graphite threaded rod 7 is tightened with the graphite electrodes 1 and 2 for conduction, and the wire 8 is connected to the graphite threaded rod 7 by a conductive clamp for conduction.
[0036] The power supply is powered on, the power supply voltage is 0-50V, the current is 0-500mA, and the hydroxide (OH) is generated by electrolysis of water. - ) gather at the anode, and hydroxide (OH - ) and holes (h + ) forms free radicals ( . OH), the free radical is unstable and easily diffuses to the interface between the anode SiC and the electrolyte, oxidizing SiC to SiO x and CO x , and then the oxidation product SiO x and CO x Dissolved in HF electrolyte. The process can be expressed as:
[0037] 4OH - -4e - →2H2O+O2;
[0038] OH - +h + → . OH;
[0039] SiC+4 . OH+O2→SiO2+CO2+2H2O;
[0040] SiO2+6HF→2H + +SiF62- +2H2O.
[0041] In the present invention, the specific steps of electrochemical etching + high-purity 4H-SiC single crystal growth are as follows:
[0042] Step 1: expose the Si surface of the SiC substrate to be pretreated and cover the C surface;
[0043] Step 2: The C surface of the substrate is connected to a graphite electrode as an anode, and a graphite electrode or a platinum electrode is selected as a cathode (the C surface of the substrate is preferably conductive glue or vacuum adsorbed on the graphite electrode);
[0044] Step 3: The anode and the cathode are placed symmetrically, and the SiC substrate with the exposed Si surface is placed in an electrolyte with a concentration of 0-60wt%, and a power supply is connected to perform electrochemical etching on the growth surface of the substrate for 0-5h;
[0045] The electrolyte temperature is controlled at 0-50°C, and auxiliary conditions can be added, such as ultraviolet light irradiation, ultrasonic vibration, etc. The electrolyte type can be neutral (such as NaCl solution), alkaline (such as KOH solution), acidic (such as HF solution). In the present invention, HF solution is preferably selected as the electrolyte.
[0046] Step 4: Soak the electrochemically etched substrate in an electrolyte for 0-12 hours, then soak it in deionized water for several times with ultrasonic vibrations for 0-10 hours, and finally dry it with an inert gas such as Ar or He for later use.
[0047] Step 5: The Si surface of the pretreated seed crystal 15 is used as the growth surface and fixed on the seed crystal holder 14 (the fixing method is not limited, it can be: adhesive bonding, mechanical fixing, chemical fixing, etc.), and the high-purity SiC powder 17 is placed at the bottom of the crystal growth crucible 16. The crucible is tightened and placed in a corresponding heat preservation field (the material of the crystal growth crucible can be selected from isostatic graphite, tantalum carbide, tantalum carbide coating or metal tungsten, etc.).
[0048] Step 6: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10^ -6 mbar, set the corresponding temperature and pressure control programs.
[0049] Step seven: under vacuum conditions, set the temperature rising program, after heating to 1100-1450°C for 2-6 hours, open the argon gas inlet (gas flow rate is controlled at 0-5L / min), increase the pressure to 200-900mbar for 0.5-3 hours, under the condition of flowing argon constant pressure, increase the temperature to 2000-2300°C for 2-6 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 0.1-50mbar within 0.5-50 hours. Under the growth conditions of temperature: 2000-2300°C, pressure: 0.1-50mbar, the crystal grows for 3-15 days.
[0050] Step 8: Before increasing the pressure and lowering the temperature, keep the argon gas inlet open (gas flow rate controlled at 0-5L / min), increase the pressure to 200-900mbar for 0.5-3 hours, and lower the temperature to 700-1400℃ for 10-20 hours, then cool naturally, and the entire crystal growth is completed.
[0051] In the present invention, the thermal field device used for crystal growth is as follows Figure 2 As shown, it includes an upper temperature measuring hole 9; a lower temperature measuring hole 10; an upper insulation 11; a lower insulation 12; a side insulation 13; a seed crystal holder 14; a seed crystal 15; a crystal growth crucible 16; and a high-purity SiC powder 17, which are composed of an upper insulation 11, a side insulation 13 and a lower insulation 12 from top to bottom, wherein the upper and lower temperature measuring holes 9 and 10 are respectively located in the middle of the upper and lower insulations, the crystal growth crucible 16 is placed in the middle of the lower insulation 12, the high-purity SiC powder 17 is placed at the bottom of the crystal growth crucible 16, the seed crystal 15 is fixed on the seed crystal holder 14, and the seed crystal holder 14 is connected to the crystal growth crucible by a threaded knob.
[0052] The present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0053] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0054] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.
[0055] Example
[0056] This embodiment provides a method for growing a high-purity 4H-SiC single crystal on the Si surface of a SiC substrate by a PVT method after pre-treating the Si surface of the SiC substrate by electrochemical etching. The specific steps are as follows:
[0057] Step 1: The Si surface of the SiC substrate 6 is exposed, and the C surface is connected to the graphite electrode 1 using a conductive adhesive so that the SiC substrate 6 and the graphite electrode 1 are in full contact.
[0058] Step 2: SiC substrate 6 and graphite electrode 1 are used as anodes and connected to the positive pole of the power supply. Graphite electrode 2 of the same size and thickness is used as cathode and connected to the negative pole of the power supply. The distance between the two electrodes is 6 cm. The output voltage of power supply 4 is 15 V and the current is 50 mA.
[0059] Step 3: electrochemically etch the SiC substrate with exposed Si surface in HF electrolyte 5 with a concentration of 10 wt% for 10 minutes, and the temperature of the electrolyte 5 is controlled at 30°C.
[0060] Step 4: The electrochemically etched substrate is first immersed in electrolyte 5 for 12 hours, then immersed in deionized water for 2 hours by ultrasonic wave, and finally dried with Ar gas for later use.
[0061] Step 5: Use the Si surface of the pretreated seed crystal 15 as the growth surface and fix it on the seed crystal holder 14 (the fixing method is not limited, it can be: adhesive bonding, mechanical fixing, chemical fixing, etc.), high-purity SiC powder 17 is placed at the bottom of the crystal growth crucible 16, the crucible is tightened, and placed in a corresponding heat preservation field.
[0062] Step 6: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0063] Step 7: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the argon inlet line (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, and under the condition of flowing argon constant pressure, increase the temperature to 2100°C in 3 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour. Under the growth conditions of temperature: 2100°C and pressure: 5mbr, the crystal is grown for 5 days.
[0064] Step 8: Before increasing the pressure and lowering the temperature, keep the Ar gas inlet open (gas flow rate is 1L / min), increase the pressure to 800mbar for 1 hour, and lower the temperature to 1100℃ in 15 hours, then cool naturally, and the entire crystal growth is completed.
[0065] SIMS test was performed on two high-purity 4H-SiC single crystals grown as seed crystals after electrochemical etching pretreatment on two N-type 4H-SiC substrates with different crystal planes. The results are shown in Table 1.
[0066] Table 1
[0067] Growing conditions Nitrogen concentration Growth of 4H-SiC on Si Surface of N-type 4H Seed Crystal 3.0E17—5.0E17 Growth of 4H-SiC on C-surface of N-type 4H Seed Crystal 1.0E18—3.0E18
[0068] It can be seen from the data in Table 1 that the absorption of nitrogen by 4H-SiC single crystal grown on the Si surface is one order of magnitude smaller than that by 4H-SiC single crystal grown on the C surface. If the growth of 4H-SiC single crystal is stabilized on the Si surface, it is beneficial to reduce the absorption of nitrogen and is conducive to the growth of high-purity semi-insulating 4H-SiC single crystal.
[0069] Raman mapping scanning tests were performed on SiC single crystals grown by PVT method without treating the Si surface of SiC substrate and on SiC single crystals grown by PVT method after electrochemical etching pretreatment to form etched area and unetched area on the Si surface of SiC substrate.
[0070] Raman mapping scan test can determine the distribution of SiC crystal types. The same color means the same characteristic peaks, which means the same crystal type. The blue characteristic peaks are 204 and 776, which represent 4H-SiC; the green characteristic peaks are 150 and 789, which represent 6H-SiC; and the red characteristic peaks are 173 and 785, which represent 15R-SiC. Figure 3 In the case of SiC substrate, the Si surface is not treated and the single crystal is grown directly. The Raman mapping image is not uniform in color, indicating the presence of 6H, 4H, and 15R crystal types, and the presence of polymorphic inclusions. Figure 4 This is the Raman mapping image of the same round of single crystal growth in the etched area and the unetched area after the Si surface of the SiC substrate is pre-treated by electrochemical etching. The etched area has a single color, indicating that 4H-SiC is the main crystal type in the etched area, while the unetched area has more different color points and the crystal type difference is greater than that in the etched area. There is a polymorphic inclusion phenomenon, which indicates that the electrochemical etching pretreatment can promote and stabilize the growth of a single crystal of 4H-SiC on the Si surface.
[0071] In summary, before growing SiC crystals by the PVT method, electrochemical etching pretreatment is performed on the Si surface of the SiC substrate, which can provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, and provide a window for the nucleation and growth of 4H-SiC. While stabilizing the single crystal growth of 4H-SiC on the Si surface, it can reduce the absorption of nitrogen, which is beneficial to solving the problem of excessive nitrogen content in high-purity semi-insulating SiC single crystals, breaking the technical barriers of growing 4H on the C surface and 6H on the Si surface, and making the preparation of high-purity semi-insulating 4H-SiC simpler.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for growing high-purity 4H-SiC single crystals by a PVT method, characterized in that: Before the growth of SiC crystal by PVT method, the Si surface of SiC substrate is pretreated by electrochemical etching to provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for the nucleation growth of 4H-SiC, reduce the absorption of nitrogen, and stabilize the growth of high-purity 4H-SiC single crystal.
2. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 1, characterized in that: The specific steps of electrochemical etching pretreatment of the Si surface of the SiC substrate are: (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface; (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode; (3) The anode and cathode are placed symmetrically, the SiC substrate is placed in the electrolyte, the power supply is connected and the Si surface of the substrate is electrochemically etched; (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
3. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (2), the C surface of the substrate and the graphite electrode are connected by conductive adhesive bonding or vacuum adsorption.
4. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.
5. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.
6. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (4), the sample is immersed in the electrolyte for 0-12 hours, and immersed in deionized water for 0-10 hours.
7. The method for growing high-purity 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (4), the inert gas is Ar or He.
Citation Information
Patent Citations
Method for preparing graphene and graphene device by epitaxy of pretreated SiC substrate
CN110556283A
Composite silicon carbide substrate and preparation method thereof
CN115101584A
Electrochemical etching device and etching method thereof
CN116288641A
Method for growth of crystal surfaces and growth of heteroepitaxial single crystal films thereon
US5915194A