Manufacturing method of deep groove structure
By adjusting the BOSCH etching process parameters, narrowing the cyclic morphology of the deep trench and enhancing side wall protection, the problem of depression defects at the bottom of the deep trench is solved, and the polysilicon filling quality and chip reliability are improved.
Patent Information
- Application Number
- CN202410958050.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing deep trench structure manufacturing method, there are depression defects in the bottom morphology of the deep trench, which affects the subsequent polysilicon filling quality and chip reliability.
By adjusting the process parameters of the deposition and etching stage in the BOSCH etching process, narrowing the cyclic morphology, reducing the bottom side excavation of deep trenches, and enhancing sidewall protection in the second dry etching to prevent depressions The formation of defects.
Effectively eliminate the side-extraction defects and depression defects at the bottom of deep trench, improve the quality of polysilicon, and improve the reliability of the chip.
Smart Images

Figure CN119028816A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a semiconductor integrated circuit manufacturing process method, in particular to a deep trench structure manufacturing method. Background Art
[0002] In the semiconductor field, the process technology pays great attention to morphology control. In the BCD deep trench isolation (DTI) process, if there are defects such as depressions in the bottom morphology of the deep trench, it will cause poor subsequent polysilicon (poly) filling, affecting device reliability, etc. The existing platform automotive DTI process has obvious depressions after etching the bottom of the DTI; the defective morphology of the depression will aggravate the subsequent poor poly filling in the DTI, which will have an adverse effect on the reliability of the subsequent chip.
[0003] like Figures 1A to 1C As shown, it is a schematic diagram of the device structure in each step of the existing deep trench structure manufacturing method; FIG. 2A to FIG. 2C , which are photos of devices in various steps of the existing method for manufacturing a deep trench structure; the existing method for manufacturing a deep trench structure includes the following steps:
[0004] Step S1: Figure 1A As shown, the first deep trench dry etching (DTIDRY1) is performed. DTIDRY1 adopts Bosch etching and uses C4F8 / SF6 base, i.e., C4F8 / SF6 based process gas. DTIDRY1 forms deep trenches 102 in selected areas of the silicon substrate 101.
[0005] Bosch etching includes a cyclic process of deposition (dep) and etching (etch), which will cause bottom undercutting. Figure 1A As shown, the cyclic steps of deposition and etching may generate fluctuations on the side of the deep trench 102 , and such fluctuations may eventually form bottom undercut defects 103 at the bottom region of the deep trench 102 .
[0006] like Figure 2A As shown, the actual photo after step S1 is completed, that is, the photo taken by an electron microscope such as a SEM photo, Figure 2A In the figure, the semiconductor substrate is individually marked with a mark 101a, the deep trench is individually marked with a mark 102a, and the bottom undercut defect is individually marked with a mark 103a.
[0007] Step S2: Figure 1B As shown, thermal oxidation of the DTI sidewall is performed to form an oxide layer 104. The area surrounded by the top surface of the oxide layer 104 forms a second deep trench 102'. It can be seen that Figure 1AThe bottom undercut defect 103 in the second deep trench 102' is transferred to the surface of the oxide layer 104 at the bottom area of the second deep trench 102' during the formation of the oxide layer 104 and forms a recessed defect 105. Moreover, the bottom surface of the second deep trench 102' is not flat and has an arc shape.
[0008] like Figure 2B As shown, the actual photo after step S2 is completed, Figure 2B In the figure, the oxide layer is individually marked with a label 104a, the second deep trench is individually marked with a label 102a', and the recess defect 105 is individually marked with a label 105a'.
[0009] Step S3: Figure 1C As shown, a second dry etching (dry2) is performed to etch the oxide layer 104, so that the oxide layer 104 at the bottom of the second deep trench 102' is removed and the oxide layer 104 on the sidewall is retained. The DRY2 etching uses a process gas of C5F8 / Ar / O2 base, and the low C5F8 ratio leads to insufficient sidewall protection; the arc bottom increases the etching of the sidewall by ion backsplash, which aggravates the sidewall depression and even expands the depression defect 105.
[0010] like Figure 2C As shown, this is the actual photo after step S3 is completed.
[0011] Step S4: Poly filling is performed, and the concave sidewall exacerbates the poor filling. Summary of the invention
[0012] The technical problem to be solved by the present invention is to provide a method for manufacturing a deep trench structure, which can eliminate the bottom undercut defect of the deep trench formed in the semiconductor substrate, and further eliminate the concave defect formed in the bottom area of the side wall in the subsequent filling after the deep trench is formed.
[0013] In order to solve the above technical problems, the present invention provides a method for manufacturing a deep trench structure, comprising:
[0014] A first dry etching process is performed to form deep trenches in selected areas of the semiconductor substrate.
[0015] The first dry etching adopts a BOSCH etching process and includes a deposition phase and an etching phase with multiple cycles.
[0016] The deposition phase and the etching phase in each cycle form a cyclic morphology on the sidewall of the deep trench.
[0017] In the first dry etching, the cyclic morphology of each layer is narrowed by simultaneously adjusting the process parameters of the deposition stage and the etching stage, and the cyclic morphology of each layer is narrowed to reduce the bottom undercut of the deep trench to below the first set value; in the deposition stage, the cyclic morphology is narrowed by increasing the deposition rate and reducing the deposition time; in the etching stage, the cyclic morphology is narrowed by increasing the etching softening effect and reducing the etching time.
[0018] A further improvement is that, in the first dry etching, the process parameters of the deposition stage include: deposition chamber pressure, deposition gas flow rate, deposition RF power and deposition time.
[0019] Process parameter adjustments to increase the deposition rate during the deposition phase include:
[0020] reducing the pressure of the deposition chamber;
[0021] increasing the deposition gas flow rate;
[0022] The deposition RF power is increased.
[0023] A further improvement is that, in the first dry etching, the process parameters of the etching stage include: etching chamber pressure, etching gas flow, etching RF power and etching time.
[0024] The process parameter adjustment for increasing the etching gentleness effect in the etching stage includes:
[0025] reducing the pressure of the etching chamber;
[0026] reducing the etching gas flow rate;
[0027] The etching RF power is reduced.
[0028] A further improvement is that the deposition gas is C4F8.
[0029] A further improvement is that, in the first dry etching, the adjusted process parameter value range of the deposition stage includes:
[0030] The deposition chamber pressure is 50mt to 60mt;
[0031] The deposition gas flow rate is 125 sccm to 150 sccm;
[0032] The deposition RF power is above 900W;
[0033] The deposition time is 1.6s to 2.5s.
[0034] A further improvement is that the etching gas is SF6.
[0035] A further improvement is that, in the first dry etching, the adjusted process parameter value range of the etching stage includes:
[0036] The etching chamber pressure is 50mt to 60mt;
[0037] The etching gas flow rate is 115 sccm to 145 sccm;
[0038] The etching RF power is below 700W;
[0039] The etching time is 2.5s to 3.8s.
[0040] Further improvements include:
[0041] Forming a first oxide layer on the inner surface of the deep trench, wherein a top surface of the first oxide layer surrounds the deep trench to form a second deep trench;
[0042] The first setting value ensures that the bottom area of the second deep trench has a flat topography without depressions.
[0043] A further improvement is that the process for forming the first oxide layer includes a thermal oxidation process.
[0044] Further improvements include:
[0045] A second dry etching is performed to remove the first oxide layer below the bottom surface of the second deep trench and expose the bottom surface of the first deep trench.
[0046] A further improvement is that, in the second dry etching, the process parameters of the second dry etching are adjusted in a manner to enhance the formation of polymer on the side of the second deep trench, so as to enhance the protection of the side of the second deep trench and prevent the formation of a recess defect in the bottom area of the side of the second deep trench.
[0047] A further improvement is that the process parameters of the second dry etching include: a second etching gas flow rate and a second etching time;
[0048] The second etching gas includes C5F8, Ar and O2;
[0049] The formation of the polymer on the side of the second deep trench is enhanced by increasing the flow ratio of C5F8 and O2 and reducing the over-etching time of the second dry etching.
[0050] A further improvement is that, in the second dry etching, the adjusted process parameter value range includes:
[0051] The flow ratio of C5F8 and O2 is 1.3:1;
[0052] The etching RF power is below 700W;
[0053] The over-etching time of the second dry etching is 15s to 20s.
[0054] Further improvements include:
[0055] The second deep trench is filled with polysilicon.
[0056] A further improvement is that the material of the semiconductor substrate includes silicon.
[0057] The first dry etching for etching a semiconductor substrate to form a deep groove in the present invention adopts a BOSCH etching process. The present invention adjusts the cyclic morphology of the side wall of the deep groove by adjusting the process parameters of the deposition stage and the etching stage in each cycle to narrow the cyclic morphology, and reduces the bottom side excavation of the deep groove and reduces it to below a first set value by narrowing the cyclic morphology. This ensures that the remaining bottom side excavation of the deep groove will no longer form a bottom side excavation defect. Therefore, the present invention can ultimately eliminate the bottom side excavation defect of the deep trench formed in the semiconductor substrate.
[0058] After the deep trench, the present invention can further form a first oxide layer on the inner surface of the deep trench. Since the bottom side excavation amount of the deep trench is controlled, after the first oxide layer is formed, the bottom morphology of the second deep trench surrounded by the top surface of the first oxide layer is smooth, and the concave defect caused by the bottom side excavation defect of the deep trench disappears in the bottom area of the second deep trench.
[0059] At the same time, the present invention can further adjust the process parameters in the second dry etching of the first oxide layer at the bottom of the second deep trench to enhance the amount of polymer formed on the side of the second deep trench, thereby increasing the protection of the side of the second deep trench; coupled with the second deep trench having a flat bottom morphology, i.e., a smooth bottom morphology, it can reduce the bombardment of the side walls by ion backsplash during the second dry etching, i.e., reduce the bombardment of the side walls by ion backsplash on the second deep trench. Therefore, combined with the increase in the side protection of the second deep trench by the polymer and the reduction in the bombardment of the side walls by ion backsplash, it can further improve the morphology of the bottom area of the second deep trench after the second dry etching to prevent the occurrence of recessed defects.
[0060] Elimination of the concave defect in the bottom area of the second deep trench can improve the quality of subsequent filling in the second deep trench, such as polysilicon filling, and prevent poor filling from affecting chip reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0062] Figure 1A-Figure 1C It is a schematic diagram of the device structure in each step of the existing deep trench structure manufacturing method;
[0063] Figure 2A-2C It is a device photo in each step of the existing deep trench structure manufacturing method;
[0064] Figure 3 is a flow chart of a method for manufacturing a deep trench structure according to an embodiment of the present invention;
[0065] Figure 4A-4C is a schematic diagram of the device structure in each step of the method for manufacturing a deep trench structure according to an embodiment of the present invention;
[0066] Figure 5A-5C These are photos of devices in various steps of the method for manufacturing a deep trench structure according to an embodiment of the present invention. DETAILED DESCRIPTION
[0067] like Figure 3 As shown, it is a flow chart of a method for manufacturing a deep trench 202 structure according to an embodiment of the present invention; FIG. 4A to FIG. 4C As shown, it is a schematic diagram of the device structure in each step of the manufacturing method of the deep trench 202 structure according to an embodiment of the present invention; FIG. 5A to FIG. 5C , which are device photos in each step of the method for manufacturing a deep trench structure according to an embodiment of the present invention; the method for manufacturing a deep trench 202 structure according to an embodiment of the present invention includes:
[0068] Step S101 : performing a first dry etching to form a deep trench 202 in a selected area of a semiconductor substrate 201 .
[0069] In the embodiment of the present invention, the material of the semiconductor substrate 201 includes silicon.
[0070] The first dry etching adopts a BOSCH etching process and includes a deposition phase and an etching phase with multiple cycles.
[0071] The deposition phase and the etching phase in each cycle form a cyclic morphology on the sidewall of the deep trench 202 . Figure 4A In the figure, the dotted box 203 shows the sidewall area of the deep trench 202 corresponding to one cycle, which corresponds to one cycle morphology. It can be seen that the sidewall of the entire deep trench 202 is formed by the accumulation of multiple cycle morphologies in the vertical direction.
[0072] In the first dry etching, the process parameters of the deposition stage and the etching stage are simultaneously adjusted to narrow the cyclic morphology of each layer, and the cyclic morphology of each layer is narrowed to reduce the bottom undercut of the deep trench 202 to below the first set value; the narrowing of the cyclic morphology means that the thickness corresponding to the dotted line box 203 becomes thinner. In the embodiment of the present invention, the cyclic morphology is narrowed to reduce the bottom undercut of the deep trench 202 to below the first set value. Figure 4A The bottom area in the Figure 1A The bottom undercut defect 103 appears in the corresponding existing method.
[0073] In the embodiment of the present invention, in the deposition stage, the cyclic morphology is narrowed by increasing the deposition rate and reducing the deposition time; in the etching stage, the cyclic morphology is narrowed by increasing the etching softening effect and reducing the etching time.
[0074] In the first dry etching, the process parameters of the deposition stage include: deposition chamber pressure, deposition gas flow, deposition RF power and deposition time.
[0075] Process parameter adjustments to increase the deposition rate during the deposition phase include:
[0076] reducing the pressure of the deposition chamber;
[0077] increasing the deposition gas flow rate;
[0078] The deposition RF power is increased.
[0079] In some embodiments, the deposition gas is C4F8. In the first dry etching, the adjusted process parameter value range of the deposition stage includes:
[0080] The deposition chamber pressure is 50mt to 60mt;
[0081] The deposition gas flow rate is 125 sccm to 150 sccm;
[0082] The deposition RF power is above 900W;
[0083] The deposition time is 1.6s to 2.5s.
[0084] In the first dry etching, the process parameters of the etching stage include: etching chamber pressure, etching gas flow, etching RF power and etching time.
[0085] The process parameter adjustment for increasing the etching gentleness effect in the etching stage includes:
[0086] reducing the pressure of the etching chamber;
[0087] reducing the etching gas flow rate;
[0088] The etching RF power is reduced.
[0089] In some embodiments, the etching gas is SF6. In the first dry etching, the adjusted process parameter value range of the etching stage includes:
[0090] The etching chamber pressure is 50mt to 60mt;
[0091] The etching gas flow rate is 115 sccm to 145 sccm;
[0092] The etching RF power is below 700W;
[0093] The etching time is 2.5s to 3.8s.
[0094] like Figure 5A As shown, the actual photo after step S101 is completed, that is, the photo taken by an electron microscope such as a SEM photo, Figure 5A In FIG. 1 , the semiconductor substrate is marked with a marker 201a, and the deep trench is marked with a marker 202a. Figure 5A There is no bottom side hollowing defect.
[0095] Step S102: Figure 4B As shown, a first oxide layer 204 is formed on the inner surface of the deep trench 202, and a top surface of the first oxide layer 204 surrounds and forms a second deep trench 202' in the deep trench 202;
[0096] The first setting value ensures that the bottom area of the second deep trench 202 ′ has a flat topography without depressions.
[0097] In the embodiment of the present invention, the formation process of the first oxide layer 204 includes a thermal oxidation process.
[0098] like Figure 5B As shown, the actual photo after step S102 is completed, Figure 5B In the figure, the first oxide layer is individually marked with a reference numeral 204a, and the second deep trench is individually marked with a reference numeral 202a'.
[0099] Step S103: Figure 4C As shown, a second dry etching is performed to remove the first oxide layer 204 below the bottom surface of the second deep trench 202 ′ and expose the bottom surface of the first deep trench 202 .
[0100] In an embodiment of the present invention, during the second dry etching, the process parameters of the second dry etching are adjusted in a manner to enhance the formation of a polymer on the side of the second deep trench 202', so as to enhance the protection of the side of the second deep trench 202' and prevent the formation of a recess defect in the bottom area of the side of the second deep trench 202'.
[0101] The process parameters of the second dry etching include: a second etching gas flow rate and a second etching time;
[0102] The second etching gas includes C5F8, Ar and O2;
[0103] The formation of the polymer on the side of the second deep trench 202' is enhanced by increasing the flow ratio of C5F8 and O2 and reducing the over-etching time of the second dry etching.
[0104] In some embodiments, in the second dry etching, the adjusted process parameter value range includes:
[0105] The flow ratio of C5F8 and O2 is 1.3:1;
[0106] The etching RF power is below 700W;
[0107] The over-etching time of the second dry etching is 15s to 20s.
[0108] like Figure 5C As shown, the actual photo after step S103 is completed. It can be seen that there is no concave defect.
[0109] Step S104 , filling the second deep trench 202 ′ with polysilicon (not shown).
[0110] In the embodiment of the present invention, the first dry etching for etching the semiconductor substrate 201 to form the deep trench 202 adopts the BOSCH etching process. The embodiment of the present invention adjusts the cyclic morphology of the side wall of the deep trench 202 by adjusting the process parameters of the deposition stage and the etching stage in each cycle to narrow the cyclic morphology, and the bottom side excavation amount of the deep trench 202 is reduced and reduced to below the first set value through the narrowing of the cyclic morphology, thereby ensuring that the remaining bottom side excavation amount of the deep trench 202 will no longer form a bottom side excavation defect. Therefore, the embodiment of the present invention can ultimately eliminate the bottom side excavation defect of the deep trench 202 formed in the semiconductor substrate 201.
[0111] After the deep trench 202, the embodiment of the present invention can further form a first oxide layer 204 on the inner surface of the deep trench 202. Since the bottom side excavation amount of the deep trench 202 is controlled, after the first oxide layer 204 is formed, the bottom morphology of the second deep trench 202' surrounded by the top surface of the first oxide layer 204 is smooth, and the concave defect caused by the bottom side excavation defect of the deep trench 202 disappears.
[0112] At the same time, the embodiment of the present invention can further adjust the process parameters in the second dry etching of the first oxide layer 204 at the bottom of the second deep trench 202' to enhance the amount of polymer formed on the side of the second deep trench 202', thereby increasing the protection of the side of the second deep trench 202'; in addition, the second deep trench 202' has a flat bottom morphology, i.e., the bottom morphology is flat, which can reduce the bombardment of the side walls by ion backsplash during the second dry etching, i.e., reduce the bombardment of the side walls by ion backsplash on the second deep trench 202'. Therefore, combined with the increase in the side protection of the second deep trench 202' by the polymer and the reduction in the bombardment of the side walls by ion backsplash, the morphology of the bottom area of the second deep trench 202' after the second dry etching can be further improved to prevent the occurrence of recessed defects.
[0113] Elimination of the concave defect in the bottom area of the second deep trench 202 ′ can improve the quality of subsequent filling in the second deep trench 202 ′, such as polysilicon filling, and prevent poor filling from affecting chip reliability.
[0114] The present invention has been described in detail above through specific embodiments, but these do not constitute limitations of the present invention. Without departing from the principle of the present invention, those skilled in the art may also make many variations and improvements, which should also be considered as the protection scope of the present invention.
Claims
1. A method for manufacturing a deep trench structure, characterized in that: include: Performing a first dry etching process to form deep trenches in selected areas of the semiconductor substrate; The first dry etching adopts a BOSCH etching process and includes a deposition phase and an etching phase for multiple cycles; The deposition phase and the etching phase in each cycle form a cyclic morphology on the sidewall of the deep trench; In the first dry etching, the cyclic morphology of each layer is narrowed by simultaneously adjusting the process parameters of the deposition stage and the etching stage, and the cyclic morphology of each layer is narrowed to reduce the bottom undercut of the deep trench to below the first set value; in the deposition stage, the cyclic morphology is narrowed by increasing the deposition rate and reducing the deposition time; in the etching stage, the cyclic morphology is narrowed by increasing the etching softening effect and reducing the etching time.
2. The method for manufacturing a deep trench structure according to claim 1, wherein: In the first dry etching, the process parameters of the deposition stage include: deposition chamber pressure, deposition gas flow rate, deposition RF power and deposition time; Process parameter adjustments to increase the deposition rate during the deposition phase include: reducing the pressure of the deposition chamber; increasing the deposition gas flow rate; The deposition RF power is increased.
3. The method for manufacturing a deep trench structure according to claim 2, wherein: In the first dry etching, the process parameters of the etching stage include: etching chamber pressure, etching gas flow, etching RF power and etching time; The process parameter adjustment for increasing the etching gentleness effect in the etching stage includes: reducing the pressure of the etching chamber; reducing the etching gas flow rate; The etching RF power is reduced.
4. The method for manufacturing a deep trench structure according to claim 2, wherein: The deposition gas is C4F8.
5. The method for manufacturing a deep trench structure according to claim 4, wherein: In the first dry etching, the adjusted process parameter value range of the deposition stage includes: The deposition chamber pressure is 50mt to 60mt; The deposition gas flow rate is 125 sccm to 150 sccm; The deposition RF power is above 900W; The deposition time is 1.6s to 2.5s.
6. The method for manufacturing a deep trench structure according to claim 3, wherein: The etching gas is SF6.
7. The method for manufacturing a deep trench structure according to claim 6, wherein: In the first dry etching, the adjusted process parameter value range of the etching stage includes: The etching chamber pressure is 50mt to 60mt; The etching gas flow rate is 115 sccm to 145 sccm; The etching RF power is below 700W; The etching time is 2.5s to 3.8s.
8. The method for manufacturing a deep trench structure according to claim 1, wherein: Also includes: Forming a first oxide layer on the inner surface of the deep trench, wherein a top surface of the first oxide layer surrounds the deep trench to form a second deep trench; The first setting value ensures that the bottom area of the second deep trench has a flat topography without depressions.
9. The method for manufacturing a deep trench structure according to claim 8, wherein: The forming process of the first oxide layer includes a thermal oxidation process.
10. The method for manufacturing a deep trench structure according to claim 8, wherein: Also includes: A second dry etching is performed to remove the first oxide layer below the bottom surface of the second deep trench and expose the bottom surface of the first deep trench.
11. The method for manufacturing a deep trench structure according to claim 10, wherein: In the second dry etching, the process parameters of the second dry etching are adjusted in a manner to enhance the formation of polymer on the side of the second deep trench, so as to enhance the protection of the side of the second deep trench and prevent the formation of a recess defect in the bottom area of the side of the second deep trench.
12. The method for manufacturing a deep trench structure according to claim 11, wherein: The process parameters of the second dry etching include: a second etching gas flow rate and a second etching time; The second etching gas includes C5F8, Ar and O2; The formation of the polymer on the side of the second deep trench is enhanced by increasing the flow ratio of C5F8 and O2 and reducing the over-etching time of the second dry etching.
13. The method for manufacturing a deep trench structure according to claim 12, wherein: In the second dry etching, the adjusted process parameter value range includes: The flow ratio of C5F8 and O2 is 1.3:1; The etching RF power is below 700W; The over-etching time of the second dry etching is 15s to 20s.
14. The method for manufacturing a deep trench structure according to claim 10, wherein: Also includes: The second deep trench is filled with polysilicon.
15. The method for manufacturing a deep trench structure according to claim 1, wherein: The material of the semiconductor substrate includes silicon.