Method for removing cement in device at low temperature
By introducing fluorine-based gas CF4 in plasma treatment, the problem of removing through-hole cement at low temperature is solved, and effective removal is achieved under low temperature conditions, avoiding damage to etching film by high-temperature removal, and improving device quality and energy efficiency.
Patent Information
- Application Number
- CN202411480254.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-23
AI Technical Summary
Under low temperature conditions, it is difficult for the prior art to effectively remove cements around the through holes in semiconductor devices, resulting in residues affecting process quality, and high-temperature glue removal will cause damage to the etching film.
Introduce fluorine-based gas, especially CF4, to remove cement from the device at low temperature, control the temperature ≤65°C, and set the bias power at 100W≤U≤250W in the plasma treatment to ensure that The removal effect of cement and device performance.
Effectively remove cement around the through holes under low temperature conditions, improve device quality, avoid damage to the etching film by high-temperature glue removal, and lower energy consumption.
Smart Images

Figure CN119028819A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for removing adhesive in a device at low temperature. Background Art
[0002] Semiconductor photoresist removal processes are generally divided into two types, wet stripping and dry stripping. Compared with wet stripping, plasma dry stripping uses high-energy plasma to treat the surface of photoresist. It removes the photoresist thoroughly and quickly without the introduction of chemical substances, reducing corrosion and damage to wafer materials. It is the best method among existing stripping processes. Its working principle is to place the product wafer in a vacuum reaction system, introduce a small amount of oxygen and nitrogen, apply high pressure and high power, and generate a high-frequency signal from a high-frequency signal generator to generate an induced electromagnetic field in the vacuum system, ionize oxygen, and form a mixture of oxygen ions, activated oxygen atoms, oxygen molecules and electrons. Activated oxygen (active atomic oxygen) can quickly oxidize the photoresist into volatile gas, which is pumped away by a mechanical pump.
[0003] Since high-temperature degumming may damage certain etched films, a low-temperature plasma surface degumming process is introduced. However, the degumming activity will decrease as the temperature decreases, and some components may not be removed cleanly, resulting in unnecessary residues that affect the process. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for removing binders in devices at low temperature. By introducing fluorine-based gas, especially CF4, into the plasma-treated gas, the binders around the through holes can be removed at low temperature, thereby improving the product quality of the final device and having broad application prospects.
[0005] It is worth noting that the back-end through-hole etching structure behind the current chip has a through-hole, and the adhesive remaining in or around the through-hole is more difficult to remove than the adhesive in other places. On the one hand, it is necessary to ensure that the performance of the through-hole is not affected, and on the other hand, it is necessary to achieve effective removal of the adhesive inside the through-hole. In addition, the through-hole is more difficult to remove due to the limitation of the aperture itself. Therefore, the present invention has developed the following method for removing adhesive from the device at low temperature.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for removing cement in a device at low temperature, the method comprising:
[0008] At a first temperature, a cleaning gas is introduced to perform plasma treatment to remove adhesive in the device;
[0009] Wherein, the first temperature is ≤65° C.; and the cleaning gas contains fluorine-based gas.
[0010] It is worth noting that, in general, the process of removing the cement is above 70°C, and at such a high temperature, the etched film quality will be damaged, for example, when the material is LN and / or LT, it is easy to cause damage. Therefore, the present invention adopts a low-temperature etching process. However, due to the particularity of the device of the present invention, it is difficult to effectively remove the cement at low temperatures. Through various studies, it is found that the use of a cleaning gas containing a fluorine-based gas can effectively remove the cement without having a negative impact on the device.
[0011] Specifically, the first temperature is ≤65°C, for example, it can be 10°C, 12°C, 15°C, 21°C, 27°C, 32°C, 38°C, 43°C, 49°C, 54°C, 60°C or 65°C.
[0012] Preferably, the fluorine-based gas includes CF4.
[0013] The preferred fluorine-based gas in the present invention is CF4. Compared with other fluorine-containing gases such as CH2F2, CH3F, CHF3, C2H3F3 and the like, CF4 in the present invention has the advantage of stronger desiliconization ability. The use of gases such as CH2F2 not only has relatively weak desiliconization ability, but also produces heavier deposits.
[0014] Preferably, the volume proportion of the fluorine-based gas in the cleaning gas is 5-10‰, for example, it can be 5‰, 5.5‰, 5.8‰, 5.6‰, 6.0‰, 6.5‰, 6.8‰, 7.0‰, 7.4‰, 7.5‰, 8.0‰, 8.3‰, 8.5‰, 9.0‰, 9.2‰ or 10‰, etc.
[0015] The present invention preferably controls the volume ratio of the fluorine-based gas within the above range. When the volume ratio of the fluorine-based gas is too large, there may be a negative impact on the device. When the volume ratio of the fluorine-based gas is too small, the silicon slag may not be completely removed.
[0016] Preferably, the cleaning gas further contains oxygen and / or nitrogen.
[0017] Preferably, the volume ratio of oxygen to nitrogen in the cleaning gas is 4-10:1, for example, it can be 4:1, 4.7:1, 5.4:1, 6:1, 6.7:1, 7.4:1, 8:1, 8.7:1, 9.4:1 or 10:1.
[0018] And / or, the flow rate of the cleaning gas is 5000-10000 sccm, for example, 5000 sccm, 6660 sccm, 8330 sccm or 10000 sccm.
[0019] Preferably, the first temperature is 15-65°C, for example, it can be 15°C, 20°C, 25°C, 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 65°C, etc., preferably 15-30°C.
[0020] In the present invention, the temperature can be further reduced to 15-30° C., which has almost no effect on the device and can effectively remove the cement in the device.
[0021] Preferably, the bias power of the plasma treatment is 100W≤U≤250W, for example, it can be 250W, 245W, 240W, 230W, 220W, 200W, 180W, 170W, 160W, 150W, 140W, 130W, 120W, 110W or 100W, etc.
[0022] It is worth noting that another core invention of the present invention is that the bias power setting during the plasma treatment process is critical, because in the process of removing the binder, it is necessary to consider not only the removal of the binder, but also the fact that the device will not be damaged or negatively affected during the process. After the fluorine-based gas is introduced into the present invention, the bias power of the plasma treatment needs to be strictly controlled within the above range, otherwise it is easy to react with the silicon nitride film layer to produce by-products, and it will also cause damage to the silicon nitride film layer, affecting the device performance.
[0023] The present invention has no special restrictions on other parameters of the plasma treatment, and the process parameters well known to those skilled in the art may be used, and may also be adjusted according to actual conditions.
[0024] For example, the power of the plasma treatment is 2000-2500 W, for example, 2000 W, 2050 W, 2100 W, 2150 W, 2200 W, 2250 W, 2300 W, 2350 W, 2400 W, 2450 W or 2500 W, etc.
[0025] Preferably, the device comprises a membrane layer and a through-hole layer which are stacked.
[0026] The material of the film layer is a nitrogen-containing layer, preferably a silicon nitride layer.
[0027] The device of the present invention may be, for example, a back-end through-hole etching structure behind a chip.
[0028] Preferably, the thickness of the film layer is 100-300 nm, for example, it may be 100 nm, 120 nm, 130 nm, 140 nm, 150 nm, 180 nm, 200 nm, 220 nm, 230 nm, 250 nm, 280 nm or 300 nm.
[0029] Preferably, the thickness of the through-hole layer is 10-30 nm, for example, it may be 10 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 22 nm, 23 nm, 24 nm, 27 nm or 30 nm.
[0030] Preferably, the through-hole layer has a through-hole, and the periphery of the through-hole has a binder.
[0031] Preferably, the material of the through-hole layer is a silicon-containing compound, preferably silicon oxide.
[0032] Preferably, the diameter of the through hole is 50-1000 nm, for example, it may be 50 nm, 150 nm, 260 nm, 360 nm, 470 nm, 570 nm, 680 nm, 780 nm, 890 nm or 1000 nm.
[0033] Preferably, the depth of the through hole is 50-500 nm, for example, it may be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm.
[0034] The diameter and depth of the through hole in the present invention also bring great difficulty to the removal of the cement. It is precisely because the diameter and depth of the through hole are small that the removal of the cement remaining therein is completely incomparable to the removal of the cement in the flat layer. In this regard, the present invention adopts a combination of low temperature and fluorine-based gas cleaning gas for removal, which can not only not affect the diameter and depth of the through hole, but also effectively remove the cement.
[0035] Preferably, the cross-section of the through hole is an inverted T-shape, wherein the acute angle between the hypotenuse and the bottom of the inverted T-shape is in the range of 75~90°, for example, it can be 75°, 78°, 79°, 80°, 82°, 84°, 85°, 86°, 87°, 88° or 90°, etc.
[0036] Preferably, the material of the binder includes photoresist.
[0037] The present invention has no special requirements on the material of the photoresist, and photoresist materials familiar to those skilled in the art may be used, or may be adjusted according to actual conditions. Generally, the photoresist is composed of three main components: photosensitive resin, sensitizer and solvent.
[0038] There are no special requirements for the materials of the photosensitive resin, sensitizer and solvent in the present invention. Photoresist materials familiar to those skilled in the art can be used and can be adjusted according to actual conditions. The photosensitive resin can be, for example, polymethacrylate and / or polyimide, the sensitizer can be, for example, aromatic aldehydes and / or ketones, and the solvent can be, for example, any one of acetone, ethanol, isopropanol or butanone, or a combination of at least two thereof.
[0039] Preferably, the binder contains silicon slag.
[0040] It is precisely because the binder contains silicon slag and the binder remains in the through-hole that conventional cleaning gases are difficult to effectively remove the binder in the device. The main reason is that the presence of silicon slag requires high temperature to remove it, and high temperature can easily cause damage to the etching film. The present invention effectively removes the binder in the through-hole by adopting a fluorine-based gas method at low temperature.
[0041] Preferably, the source of the silicon slag includes silicon slag generated when etching silicon oxide through holes and remaining on the surface of the binder.
[0042] Compared with the prior art, the present invention has at least the following beneficial effects:
[0043] The present invention provides a method for removing adhesive from a device at low temperature, which can remove adhesive around the holes of the device at low temperature without causing damage to the device, with lower energy consumption, and solves the problem of damage to the etched film caused by removing adhesive at high temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a distribution diagram of through holes in the device after the binder is removed in Example 1 of the present invention.
[0045] Figure 2 yes Figure 1 A magnified schematic diagram of a single through hole in the .
[0046] Figure 3 yes Figure 2 Schematic cross-section of the through hole.
[0047] Figure 4 This is a distribution diagram of through holes in the device after the binder is removed in Example 4 of the present invention.
[0048] Figure 5 yes Figure 4 A magnified schematic diagram of a single through hole in the .
[0049] Figure 6 yes Figure 5 Schematic cross-section of the through hole.
[0050] Figure 7 This is a distribution diagram of through holes in the device after the binder is removed in Comparative Example 1 of the present invention.
[0051] Figure 8 yes Figure 7 A magnified schematic diagram of a single through hole in the .
[0052] Fig. 9 yes Figure 8 Schematic cross-section of the through hole.
[0053] Fig.10 It is a schematic diagram of a device for removing adhesive in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0054] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0055] For the convenience of experiment, the preparation process of the device for which the binder needs to be removed in the following embodiments and comparative examples includes the following steps:
[0056] A layer of photoresist is disposed on the surface of the device (a stacked silicon oxide layer and a silicon nitride layer), and the desired photoresist pattern is obtained by exposure and development, and then the photoresist pattern is transferred to the silicon oxide layer by etching to form a through hole on the silicon oxide layer (the device with a through hole is shown in FIG. Fig.10 As shown), the photoresist needs to be removed finally.
[0057] Example 1
[0058] This embodiment provides a method for removing adhesive from a device at low temperature. The device for removing adhesive from the device includes a stacked silicon oxide layer and a silicon nitride layer.
[0059] The thickness of the silicon oxide layer is 200 nm, the thickness of the silicon nitride layer is 20 nm, the silicon oxide layer is a through-hole layer, the through-hole layer has a through-hole, and the periphery of the through-hole has a binder.
[0060] The material of the binder is photoresist (TOK20A), and the binder contains silicon slag. The source of the silicon slag includes the silicon slag generated when etching silicon oxide through holes and remaining on the surface of the binder. The diameter of the through hole in the silicon oxide layer is 470nm and the depth is 216nm. The cross-section of the through hole is an inverted T shape, and the acute angle between the hypotenuse and the bottom of the inverted T shape is 81.4°.
[0061] The method comprises the following steps:
[0062] At 25°C, cleaning gas (oxygen:nitrogen = 6000sccm:1000sccm, CF4 volume ratio is 5‰) is introduced for plasma treatment to remove the binder in the device. The bias power of the plasma treatment is 250W, the power is 2500W, and the pressure is 740mT.
[0063] Example 2
[0064] This embodiment provides a method for removing adhesive from a device at low temperature. The device for removing adhesive from the device includes a stacked silicon oxide layer and a silicon nitride layer.
[0065] The thickness of the silicon oxide layer is 300 nm, the thickness of the silicon nitride layer is 30 nm, the silicon oxide layer is a through-hole layer, the through-hole layer has a through-hole, and the periphery of the through-hole has a binder.
[0066] The binder is made of photoresist (KMPR101), which contains silicon slag. The source of the silicon slag includes the silicon slag generated when etching silicon oxide through holes and remaining in the binder. The diameter of the through hole in the silicon oxide layer is 500nm and the depth is 320nm. The cross-section of the through hole is an inverted T-shape, and the acute angle between the hypotenuse and the bottom of the inverted T-shape is 85.2°.
[0067] The method comprises the following steps:
[0068] At 15°C, cleaning gas (oxygen:nitrogen = 7000sccm:1000sccm, CF4 volume ratio is 7‰) is introduced for plasma treatment to remove the binder in the device. The bias power of the plasma treatment is 250W, the power is 2000W, and the pressure is 730mT.
[0069] Example 3
[0070] This embodiment provides a method for removing adhesive from a device at low temperature. The device for removing adhesive from the device includes a stacked silicon oxide layer and a silicon nitride layer.
[0071] The thickness of the silicon oxide layer is 110 nm, the thickness of the silicon nitride layer is 20 nm, the silicon oxide layer is a through-hole layer, the through-hole layer has a through-hole, and the periphery of the through-hole has a binder.
[0072] The material of the binder is photoresist (TOK50A), and the binder contains silicon slag. The source of the silicon slag includes the silicon slag generated when etching silicon oxide through holes and remaining in the binder. The diameter of the through hole in the silicon oxide layer is 300nm and the depth is 125nm. The cross-section of the through hole is an inverted T shape, and the acute angle between the hypotenuse and the bottom of the inverted T shape is 79.6°.
[0073] The method comprises the following steps:
[0074] At 30°C, cleaning gas (oxygen:nitrogen = 4000sccm:1000sccm, CF4 volume ratio is 10‰) is introduced for plasma treatment to remove the binder in the device. The bias power of the plasma treatment is 100W, the power is 2400W, and the pressure is 740mT.
[0075] Example 4
[0076] This embodiment provides a method for removing adhesive in a device at low temperature. Except that the bias power is 300 W, the rest of the method is the same as that of Embodiment 1, and will not be described again here.
[0077] Example 5
[0078] This embodiment provides a method for removing binders in a device at low temperature. The method is the same as that of Embodiment 1 except that CF4 is replaced by CH2F2, and thus will not be described in detail here.
[0079] Example 6
[0080] This embodiment provides a method for removing cement in a device at low temperature. The method is the same as that of Embodiment 1 except that CF4 is replaced by C2H3F3, and will not be described in detail here.
[0081] Example 7
[0082] This embodiment provides a method for removing adhesive in a device. The method is the same as that of Embodiment 1 except that it does not contain oxygen, and thus will not be described in detail here.
[0083] Example 8
[0084] This embodiment provides a method for removing adhesive in a device. The method is the same as that of Embodiment 1 except that the method does not contain nitrogen, and will not be described in detail here.
[0085] Comparative Example 1
[0086] This comparative example provides a method for removing adhesive in a device. The method is the same as Example 1 except that it does not contain CF4, and will not be described in detail here.
[0087] Comparative Example 2
[0088] This comparative example provides a method for removing adhesive in a device. The method is the same as comparative example 1 except that the temperature is changed to 70° C., and will not be described in detail here.
[0089] Comparative Example 3
[0090] This comparative example provides a method for removing adhesive in a device. The method is the same as Example 1 except that the temperature is changed to 70° C., and will not be described in detail here.
[0091] Comparative Example 4
[0092] This comparative example provides a method for removing cement in a device at low temperature. The method is the same as Example 1 except that the volume proportion of CF4 is 15‰, and the details will not be repeated here.
[0093] Comparative Example 5
[0094] This comparative example provides a method for removing cement in a device at low temperature. The method is the same as Example 1 except that the volume proportion of CF4 is 1‰, and the details will not be repeated here.
[0095] TEM test was used to observe the removal of adhesive in the through-hole and its impact on the device.
[0096] The through hole diagrams after removing the adhesive in Example 1 are as follows: Figure 1~Figure 3 As shown, from Figure 1~Figure 3 It can be seen that the adhesive is completely removed in this embodiment, and has no negative impact on the through hole and the device.
[0097] The through hole diagrams after removing the adhesive in Example 4 are as follows: Figure 4~Figure 6 As shown, from Figure 4~Figure 6 It can be seen that although the binder is completely removed in this embodiment, impurity byproducts are generated in the through holes, and the byproducts are silicon slag.
[0098] The through-hole diagrams after removing the cement in Comparative Example 1 are as follows: Figure 7~Figure 9 As shown, from Figure 7~Figure 9 It can be seen that in this comparative example, the binder is completely removed, but a lot of silicon slag still remains on the surface.
[0099] The test results of the above embodiments and comparative examples are summarized in Table 1.
[0100] Table 1
[0101]
[0102] From Table 1, we can see the following points:
[0103] (1) It can be seen from Examples 1 to 3 that the method for removing cement in a device at low temperature provided by the present invention can effectively remove cement in a through hole at a temperature of ≤65°C without damaging the device performance and without generating impurity byproducts in the through hole;
[0104] (2) It can be seen from Example 1 and Example 4 that the bias power in Example 1 is 250 W. Compared with the bias power in Example 4 of 300 W, the adhesive around the through hole in Example 1 is completely removed, and no impurity by-products are generated in the through hole. However, in Example 4, due to the high bias power, although the adhesive around the through hole is completely removed, impurity by-products are generated around the through hole, which have a negative impact on the performance of the device. This shows that the present invention preferably sets the bias power within a reasonable range, which can remove the adhesive while ensuring the performance of the device;
[0105] (3) It can be seen from Example 1 and Comparative Examples 4-5 that the volume proportion of CF4 in Example 1 is 5‰, while the volume proportions of CF4 in Comparative Examples 4-5 are 15‰ and 1‰ respectively. In Example 1, the cement around the through hole is completely removed, and no impurity by-products are generated in the through hole. However, in Comparative Example 4, the volume proportion of CF4 is relatively high, the lower silicon nitride layer will be damaged, and impurity by-products will be generated in the through hole. In Comparative Example 5, due to the low volume proportion of CF4, it is difficult to remove the silicon slag completely, and there will be silicon slag residue. This shows that the present invention preferably sets the volume proportion of CF4 within a reasonable range, which can ensure the performance of the device while removing the cement;
[0106] (4) It can be seen from the combination of Example 1 and Examples 5-6 that CH2F2 and C2H3F3 are used in Examples 5-6, and there are serious silicon slag residues in Examples 5-6, and the sediment is too heavy, which affects the debonding efficiency. This shows that the present invention has the advantages of higher debonding efficiency and better protection of device performance by preferably using CF4 to remove the binder;
[0107] (5) It can be seen from the combination of Example 1 and Examples 7 to 8 that Example 7 does not contain oxygen, resulting in a decrease in the degumming efficiency. Within the same processing time, the adhesive residue is serious. Although the adhesive can be completely removed after the plasma treatment time is extended, the long plasma treatment time causes damage to the device. Example 8 does not contain nitrogen, and the degumming efficiency is seriously reduced. Within the same processing time, the adhesive residue is serious. Although the adhesive can be completely removed after the plasma treatment time is extended, the long plasma treatment time causes damage to the device. This shows that the present invention preferably adds oxygen and nitrogen to the cleaning gas, which has a better adhesive removal effect and more effective device performance guarantee.
[0108] (6) It can be seen from Example 1 and Comparative Examples 1 to 3 that Comparative Example 1 does not contain CF4, and all silicon slag remains, which is difficult to completely remove at such a low temperature; Comparative Examples 2 to 3 use a high temperature condition of 70°C, which causes damage to the device and the presence of impurity by-products in the through-holes. This shows that the present invention uses fluorine-based gas and performs cleaning at a low temperature, which can remove the binder and silicon slag and prevent the device from being damaged.
[0109] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for removing cement from a device at low temperature, characterized in that: The method comprises: At a first temperature, a cleaning gas is introduced to perform plasma treatment to remove adhesive in the device; Wherein, the first temperature is ≤65°C; the cleaning gas contains fluorine-based gas; The volume proportion of fluorine-based gas in the cleaning gas is 5-10‰; The cleaning gas further contains oxygen and / or nitrogen.
2. The method according to claim 1, characterized in that The fluorine-based gas includes CF4.
3. The method according to claim 1 or 2, characterized in that: The volume ratio of oxygen to nitrogen in the cleaning gas is 4-10:1; and / or the flow rate of the cleaning gas is 5000-10000 sccm.
4. The method according to claim 1, characterized in that: The first temperature is 15-65°C.
5. The method according to claim 1, characterized in that: The bias power of the plasma treatment is 100W≤U≤250W.
6. The method according to claim 1, characterized in that The device comprises a film layer and a through-hole layer which are stacked; The material of the film layer is a nitrogen-containing layer.
7. The method according to claim 6, characterized in that The through-hole layer has a through-hole, and the periphery of the through-hole has a binder; and / or the material of the through-hole layer is a silicon-containing compound.
8. The method according to claim 7, characterized in that The diameter of the through hole is 50-1000 nm, and / or the depth of the through hole is 50-500 nm.
9. The method according to claim 1, characterized in that: The material of the binder includes photoresist.
10. The method according to claim 1, characterized in that The cement contains silicon slag; The source of the silicon slag includes the silicon slag generated when etching the silicon compound-containing through hole and remaining on the surface of the cement.
Citation Information
Patent Citations
Removing method of photoresist used as masking layer of plasma injection
CN103092009A
Photoresist removal method and semiconductor device manufacturing method
CN105824202A
Method for removing residual polymer in polysilicon etching technology
CN1848383A
Cleaning method, method of manufacturing semiconductor device, substrate processing apparatus and recording medium
TW201324655A
Method for removing photoresist from low-k films in a downstream plasma system
US6693043B1