Semiconductor structure and forming method thereof
By designing the implant doped region and the transition doped region in the semiconductor structure, the gate trench structure makes the implant doped region deeper, solving the problem of high on-resistance in the prior art, increasing the breakdown voltage and Reduced process costs.
Patent Information
- Application Number
- CN202411111987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
AI Technical Summary
The existing superjunction-trench gate metal oxide semiconductor field effect transistors have high on-resistance under medium and high voltages, making it difficult to deepen the depth of the injection region, resulting in insufficient depletion of the drift region.
Design a semiconductor structure in which the implanted doped region is located under the gate structure and corresponds to the gate structure position. By forming the implanted doped region and the transition doped region on the substrate surface, the implanted doped region is used to dopate the implanted doped region by using the gate trench structure. The depth of the zone is greater, and the bottom end is closer to the base of the base, thus more fully depleting the drift zone.
The breakdown voltage of semiconductor devices is increased and the photolithography process steps are reduced by using a shared mask, reducing process costs.
Smart Images

Figure CN119029037A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor structure and a forming method thereof. Background Art
[0002] Trench gate metal oxide semiconductor field effect transistor (MOSFET) devices are widely used in power conversion circuits. The on-resistance and breakdown voltage of trench gate metal oxide semiconductor field effect transistors are important parameter indicators. A higher breakdown voltage and lower on-resistance can improve the competitiveness of the product. In order to improve the on-resistance of medium and high voltage (50-200V) trench gates, the concept of super junction-trench gate realized by injection has been proposed. Usually, the bottom of the injection region that assists the depletion of the drift region will be as close as possible to the highly doped substrate to make the depletable drift region longer.
[0003] However, current superjunction-trench gate metal oxide semiconductor field effect transistors still have shortcomings. Summary of the invention
[0004] The problem solved by the present invention is how to deepen the depth of the implantation region so that the bottom end of the implantation region is as close to the bottom of the substrate as possible, thereby making the implantation region deplete the drift region as much as possible.
[0005] To solve the above problems, the present invention provides a semiconductor structure, comprising: a substrate, the substrate comprising a drift region; a gate structure partially located in the drift region; an injection doping region whose doping type is opposite to that of the drift region, the injection doping region is located under the gate structure, and the position of the injection doping region corresponds to the position of the gate structure.
[0006] Optionally, a projection of the implanted doped region on the substrate surface at least partially overlaps with a projection of the gate structure on the substrate surface.
[0007] Optionally, a projection of the gate structure on the substrate surface is located within a range of a projection of the implanted doping region on the substrate surface.
[0008] Optionally, it also includes: a transition doping region with the same doping type located between the gate structure and the injection doping region, the transition doping region is in electrical contact with the injection doping region and the position of the transition doping region corresponds to the injection doping region.
[0009] Optionally, the doping concentration of the transition doping region is greater than the doping concentration of the injection doping region.
[0010] Optionally, a projection of the implanted doping region on the substrate surface at least partially overlaps with a projection of the transitional doping region on the substrate surface.
[0011] Optionally, a projection of the implanted doping region on the substrate surface is located within a projection range of the transitional doping region on the substrate surface.
[0012] Optionally, the transition doping region further extends between the gate structure and the drift region.
[0013] Optionally, it also includes: a body doping region located on the drift region, the doping type of the body doping region is opposite to the doping type of the drift region; the gate structure penetrates the body doping region in a direction perpendicular to the substrate surface and the body doping region is electrically connected to the transition doping region.
[0014] Optionally, the transition doping region also extends between the gate structure and the body doping region.
[0015] Optionally, it also includes: a first heavily doped layer located on the body doped region, the doping type of the first heavily doped layer is opposite to the doping type of the body doped region; and the gate structure penetrates the first heavily doped layer in a direction perpendicular to the substrate surface.
[0016] Optionally, it also includes: a conductive plug penetrating the first heavily doped layer, the conductive plug being electrically connected to the body doped region; a second heavily doped layer located at the bottom of the conductive plug, the second heavily doped layer being electrically connected to the conductive plug, the doping type of the second heavily doped layer being the same as the doping type of the body doped region, and the doping concentration of the second heavily doped layer being greater than the doping concentration of the body doped region.
[0017] Correspondingly, the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate, the substrate comprising a substrate and an epitaxial layer located on the substrate; etching the substrate to form a gate trench located in the epitaxial layer; performing doping treatment on the substrate exposed by the gate trench to form an implanted doping region located under the gate trench, the position of the implanted doping region corresponding to the position of the gate trench; and forming a gate structure in the gate trench.
[0018] Optionally, the step of etching the substrate to form a gate trench located in the epitaxial layer includes: forming a hard mask layer having an opening on the substrate; and etching the substrate using the hard mask layer as a mask to form a gate trench located in the epitaxial layer.
[0019] Optionally, in the process of performing a doping treatment on the substrate exposed by the gate trench to form an implanted doping region under the gate trench, the substrate exposed by the gate trench is doped using the hard mask layer as a mask.
[0020] Optionally, after doping the substrate exposed by the gate trench to form an injection doping region located under the gate trench and before forming a gate structure in the gate trench, it also includes: doping the substrate located between the gate trench and the injection doping region to form a transition doping region located between the bottom of the gate trench and the injection doping region, the transition doping region is electrically connected to the injection doping region and the position of the transition doping region corresponds to the position of the injection doping region.
[0021] Optionally, in the process of doping the substrate between the gate trench and the injection doping region to form a transition doping region between the bottom of the gate trench and the injection doping region, the hard mask layer is used as a mask to dope the substrate between the gate trench and the injection doping region.
[0022] Optionally, the substrate exposed by the gate trench is doped to form an implanted doping region located under the gate trench, and the doping dose is smaller than the doping dose of the substrate between the gate trench and the implanted doping region to form a transitional doping region located between the bottom of the gate trench and the implanted doping region.
[0023] Optionally, in the process of performing doping treatment on the substrate between the gate trench and the implanted doping region to form a transitional doping region between the bottom of the gate trench and the implanted doping region, the angle between the implantation direction of the doping treatment and the normal direction of the substrate is in the range of 15° to 45°.
[0024] Optionally, it also includes: after etching the substrate to form a gate trench located in the epitaxial layer, before doping the substrate exposed by the gate trench to form an injection doping region located under the gate trench, the gate trench is oxidized and repaired to form a sacrificial protective layer located on the surface of the gate trench; in the step of doping the substrate exposed by the gate trench to form an injection doping region located under the gate trench, the substrate exposed by the gate trench with the sacrificial protective layer on the trench surface is doped to form an injection doping region located under the gate trench.
[0025] Optionally, the method further includes: after forming the transition doping region and before forming a gate structure in the gate trench, removing the hard mask layer and the sacrificial protection layer.
[0026] Optionally, the step of forming a gate structure in the gate trench includes: forming a first gate oxide layer on the sidewalls of the gate trench and the bottom of the gate trench using a low-temperature thermal oxidation process; forming a second gate oxide layer on the first gate oxide layer using a deposition process; and forming a gate layer in the gate trench having the first gate oxide layer and the second gate oxide layer located on the first gate oxide layer to form the gate structure.
[0027] Optionally, before etching the substrate to form a gate trench in the epitaxial layer, the method further includes: performing doping treatment on the epitaxial layer to form a drift region and an initial body doping region on the drift region.
[0028] Optionally, the method further includes: after forming the gate structure, performing a doping treatment on the initial body doping regions located on both sides of the gate structure to form a first heavily doped layer.
[0029] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0030] In the semiconductor structure of the technical solution of the present invention, the injection doping region is located under the gate structure and corresponds to the position of the gate structure. The depth of the injection doping region is greater, and the bottom of the injection doping region is closer to the bottom of the substrate, which can deplete the drift region to a greater extent and improve the breakdown voltage of the semiconductor device.
[0031] In the method for forming a semiconductor structure of the technical solution of the present invention, the substrate exposed by the gate groove is doped to form an implanted doped region located under the gate groove. The existence of the gate groove makes the implanted doped region embedded in the drift region at a depth greater than the implanted doped region formed by injection from the surface of the epitaxial layer under the same injection energy. The bottom of the implanted doped region is closer to the bottom of the substrate, and the implanted doped region can deplete the drift region to a greater extent, thereby improving the breakdown voltage of the semiconductor device. In addition, the implanted doped region is located under the gate groove, and the position of the implanted doped region corresponds to the position of the gate groove. The same mask is used to form the implanted doped region and the gate groove, thereby reducing one photolithography process, saving one mask, and reducing process costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 to Figure 2 is a schematic structural diagram of a semiconductor structure according to an embodiment;
[0033] Figures 3 to 16 It is a structural schematic diagram of each step of the method for forming a semiconductor structure according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] As can be seen from the background technology, there are many problems with the existing super junction-trench gate. Now, the causes of the problems are analyzed in combination with a super junction-trench gate:
[0035] Please refer to Figure 1 and Figure 2 , Figure 2 yes Figure 1 In the cross-sectional view at position AA1, the semiconductor structure includes: a substrate 100, wherein the substrate 100 includes a drift region; a gate structure 103 partially located in the drift region; an implanted doping region 104 having a doping type opposite to that of the drift region, wherein the implanted doping region 104 is located between two adjacent gate structures 103.
[0036] The base 100 includes a substrate 101 and an epitaxial layer 102 located on the substrate 101. The epitaxial layer 102 is doped to form the drift region.
[0037] The step of forming a gate structure 103 partially located in the drift region includes: forming a first mask layer having an opening on the substrate 100; etching the substrate 100 using the first mask layer as a mask to form a gate trench located in the epitaxial layer 102; and forming the gate structure 103 in the gate trench.
[0038] The opening of the first mask layer is suitable for defining the position of the gate structure 103 .
[0039] The step of forming an implantation doping region 104 whose doping type is opposite to that of the drift region includes: forming a second mask layer having an opening on the substrate 100; and doping the substrate 100 using the second mask layer as a mask to form an implantation doping region 104 located between two adjacent gate structures 103.
[0040] The opening of the second mask layer is suitable for defining the position of the implanted doping region 104 .
[0041] The injection doping region 104 uses the second mask layer as a mask, and the gate trench uses the first mask layer as a mask. Two masks and two photolithography processes are required to form the injection doping region 104 and the gate trench, which makes the process cost relatively high. In addition, the injection energy of the injection doping region 104 needs to be greater than 2500KeV to make the bottom of the injection doping region 104 as close as possible to the bottom of the highly doped substrate 100, but the high-energy injection brings great difficulty to process integration.
[0042] In order to solve the technical problem, the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, wherein the substrate comprises a substrate and an epitaxial layer located on the substrate; etching the substrate to form a gate trench located in the epitaxial layer; performing doping treatment on the substrate exposed by the gate trench to form an implanted doping region located under the gate trench, wherein the position of the implanted doping region corresponds to the position of the gate trench; and forming a gate structure in the gate trench.
[0043] In the method for forming a semiconductor structure of the technical solution of the present invention, compared with first forming a gate structure and then forming an injection doping region located between the two gate structures, the present invention performs a doping treatment on the substrate exposed by the gate groove to form an injection doping region located under the gate groove. The existence of the gate groove makes the depth of the injection doping region embedded in the drift region under the same injection energy greater than the depth of the injection doping region formed by injection from the surface of the epitaxial layer. The injection doping region can deplete the drift region to a greater extent, thereby improving the breakdown voltage of the semiconductor device. In addition, the injection doping region is located under the gate groove, and the position of the injection doping region corresponds to the position of the gate groove. The same mask is used to form the injection doping region and the gate groove, which reduces one photolithography process, saves one mask, and reduces the process cost.
[0044] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0045] Please refer to Figure 3 , providing a substrate 200 , wherein the substrate 200 includes a substrate 201 and an epitaxial layer 202 located on the substrate 201 .
[0046] The material of the substrate 201 includes: silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium; the material of the epitaxial layer 202 includes: silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium. Specifically, in some embodiments of the present invention, the material of the substrate 201 is silicon, and the material of the epitaxial layer 202 is silicon.
[0047] Specifically, in some embodiments of the present invention, after providing the substrate 200 , the method further includes: performing a doping treatment on the epitaxial layer 202 to form a drift region 203 and an initial body doping region 204 located on the drift region 203 .
[0048] Specifically, in some embodiments of the present invention, the substrate 201 is N-type doped, the drift region 203 is N-type doped, and the doping concentration of the drift region 203 is in the range of 5E15atom / cm 3 ~1E17atom / cm 3The initial body doping region 204 is P-type doped. In other embodiments, the substrate further includes P-type doping, the drift region further includes P-type doping, and the initial body doping region further includes N-type doping.
[0049] After forming the initial body doping region 204, the method further includes: performing a thermal advancement process on the initial body doping region 204. Compared with performing the thermal advancement process after forming the implanted doping region 209, the thermal advancement process is performed before forming the implanted doping region 209, so as to avoid excessive lateral diffusion of the implanted doping region 209 under the thermal advancement process, and is conducive to controlling the morphology of the implanted doping region 209.
[0050] Please refer to Figures 4 to 5 , the substrate 200 is etched to form a gate trench 207 located in the epitaxial layer 202.
[0051] The step of etching the substrate 200 to form a gate trench 207 in the epitaxial layer 202 includes: Figure 4 As shown, a hard mask layer 206 having an opening is formed on the substrate 200; Figure 5 As shown, the substrate 200 is etched using the hard mask layer 206 as a mask to form a gate trench 207 located in the epitaxial layer 202 .
[0052] Specifically, in some embodiments of the present invention, before forming the hard mask layer 206 having an opening on the substrate 200, the method further includes: forming a barrier layer 205 on the substrate 200. The material of the barrier layer 205 includes silicon nitride. The method of forming the barrier layer 205 includes deposition. The barrier layer 205 is used as an etch stop layer when the hard mask layer 206 is subsequently removed to reduce the loss of the substrate 200.
[0053] The step of forming the hard mask layer 206 includes: forming a hard mask material layer on the barrier layer 205; forming a photoresist material layer on the hard mask material layer; performing photolithography on the photoresist material layer to form a photoresist layer; and etching the hard mask material layer using the photoresist layer as a mask to form a hard mask layer 206 having an opening. Specifically, in some embodiments of the present invention, after forming the hard mask layer 206 having an opening, the step further includes: removing the photoresist layer.
[0054] The opening position of the hard mask layer 206 defines the position of the gate trench 207 .
[0055] Specifically, in some embodiments of the present invention, the material of the hard mask layer 206 includes silicon oxide, and the method of forming the hard mask material layer includes deposition.
[0056] Specifically, in some embodiments of the present invention, the width of the gate trench 207 is less than 1 μm. The width of the gate trench 207 is the size of the gate trench 207 in the direction from one gate trench 207 to an adjacent gate trench 207 .
[0057] Please refer to Figure 6 After etching the substrate 200 to form a gate trench 207 located in the epitaxial layer 202 , the gate trench 207 is oxidized and repaired to form a sacrificial protection layer 208 located on the surface of the gate trench 207 .
[0058] Specifically, in some embodiments of the present invention, the hard mask layer 206 is not removed during the oxidation repair process. The oxidation repair process is used to repair the damage and defects on the surface of the gate trench 207 .
[0059] Specifically, in some embodiments of the present invention, the material of the sacrificial protection layer 208 includes silicon oxide.
[0060] Please refer to Figure 7 , the substrate 200 exposed by the gate trench 207 is doped to form an implanted doping region 209 located under the gate trench 207 , and the position of the implanted doping region 209 corresponds to the position of the gate trench 207 .
[0061] The substrate 200 exposed by the gate trench 207 is doped to form an implanted doped region 209 located under the gate trench 207. With the help of the depth of the gate trench 207, the maximum implantation depth of the implanted doped region 209 is deeper under the same implantation energy, and the bottom of the implanted doped region 209 is closer to the bottom of the substrate 200. The implanted doped region 209 can deplete the drift region 203 to a greater extent, thereby improving the breakdown voltage of the semiconductor device.
[0062] The position of the implanted doping region 209 corresponds to the position of the gate trench 207, that is, the projection of the implanted doping region 209 on the surface of the substrate 200 at least partially overlaps with the projection of the gate trench 207 on the surface of the substrate 200. Specifically, in some embodiments of the present invention, the projection of the gate trench 207 on the surface of the substrate 200 is located within the range of the projection of the implanted doping region 209 on the surface of the substrate 200.
[0063] The hard mask layer 206 is not removed during the oxidation repair process, so that in the process of doping the substrate 200 exposed by the gate trench 207 to form an implanted doping area 209 located under the gate trench 207, the hard mask layer 206 is used as a mask to dope the substrate 200 exposed by the gate trench 207.
[0064] The implanted doping region 209 is located under the gate trench 207 , and the position of the implanted doping region 209 corresponds to the position of the gate trench 207 . The implanted doping region 209 and the gate trench 207 are formed using the same mask, which reduces one photolithography process, saves one mask, and reduces process costs.
[0065] Specifically, in some embodiments of the present invention, in the step of doping the substrate 200 exposed by the gate trench 207 to form an implanted doping region 209 located under the gate trench 207, the substrate 200 exposed by the gate trench 207 having a sacrificial protective layer 208 on the groove surface is doped to form an implanted doping region 209 located under the gate trench 207.
[0066] In the process of doping the substrate 200 exposed by the gate trench 207 to form an implanted doping region 209 under the gate trench 207 , the sacrificial protection layer 208 is suitable for serving as a protection liner of the gate trench 207 to protect the surface of the gate trench 207 .
[0067] Specifically, in some embodiments of the present invention, during the process of performing a doping treatment on the substrate 200 exposed by the gate groove 207 to form an implanted doping region 209 under the gate groove 207, the angle between the implantation direction of the doping treatment and the normal direction of the substrate 200 is in the range of 0° to 7°.
[0068] Specifically, in some embodiments of the present invention, the doping ions implanted into the doping region 209 are boron ions; the implantation dose of the doping region 209 is in the range of 1E12atom / cm 2 ~1E13atom / cm 2 The injection energy range of the doped region 209 is 50KeV to 4000KeV.
[0069] Please refer to Figures 8 to 10 , Figure 8 for Fig. 9 and Fig.10 A top view of Fig. 9 for Figure 8 Cross-sectional view at BB1 position, Fig.10 for Figure 8 Cross-sectional view at CC1 position, Figure 8 The hard mask layer 206 and the barrier layer 205 are not shown. After the substrate 200 exposed by the gate trench 207 is doped to form an implanted doping region 209 under the gate trench 207, the substrate 200 between the gate trench 207 and the implanted doping region 209 is doped to form a transitional doping region 210 between the bottom of the gate trench 207 and the implanted doping region 209, wherein the transitional doping region 210 is electrically connected to the implanted doping region 209 and the position of the transitional doping region 210 corresponds to the position of the implanted doping region 209.
[0070] The position of the transitional doping region 210 corresponds to the position of the implanted doping region 209, that is, the projection of the implanted doping region 209 on the surface of the substrate 200 at least partially overlaps with the projection of the transitional doping region 210 on the surface of the substrate 200. Specifically, in some embodiments of the present invention, the projection of the implanted doping region 209 on the surface of the substrate 200 is within the projection range of the transitional doping region 210 on the surface of the substrate 200.
[0071] For details, please refer to Fig.10 In some embodiments of the present invention, the transitional doping region 210 further extends between the gate trench 207 and the drift region 203 . The transitional doping region 210 further extends between the gate trench 207 and the initial body doping region 204 .
[0072] Specifically, in some embodiments of the present invention, please refer to Fig.10 , the length of the gate trench 207 is greater than 10 μm. The length of the gate trench 207 is: the size of the gate trench 207 along the extension direction of the gate trench 207 .
[0073] In the process of doping the substrate 200 located between the gate trench 207 and the injection doping area 209 to form a transition doping area 210 located between the bottom of the gate trench 207 and the injection doping area 209, the hard mask layer 206 is used as a mask to dope the substrate 200 located between the gate trench 207 and the injection doping area 209.
[0074] The transition doping region 210 is located between the bottom of the gate trench 207 and the implantation doping region 209 , and the position of the transition doping region 210 corresponds to the position of the implantation doping region 209 . The formation of the transition doping region 210 does not require the introduction of a new mask, thereby reducing process costs.
[0075] The substrate 200 exposed by the gate trench 207 is doped to form an implanted doping region 209 located under the gate trench 207. The doping dose is less than the doping dose of the substrate 200 located between the gate trench 207 and the implanted doping region 209 to form a transitional doping region 210 located between the bottom of the gate trench 207 and the implanted doping region 209. The transitional doping region 210 is heavily doped, and the doping concentration of the transitional doping region 210 is greater than the doping concentration of the implanted doping region 209.
[0076] The transition doping region 210 is used to electrically connect the implantation doping region 209 , and the doping concentration of the transition doping region 210 is relatively high, so that the resistance of the semiconductor device is reduced and the response speed is increased.
[0077] The implantation dose range of the transition doping region 210 is: 1E14atom / cm 2 ~5E15atom / cm 2 The implantation energy range of the transition doping region 210 is 10KeV to 100KeV. Specifically, in some embodiments of the present invention, when the implanted ions of the transition doping region 210 are impurity boron (B), the implantation energy range is 2KeV to 25KeV, and the implantation dose range is 1E14atom / cm 2 ~5E15cmatom / cm 2 When the implanted ions in the transition doping region 210 are boron difluoride (BF2), the implantation energy range is 10KeV to 100KeV, and the implantation dose range is 1E14 atom / cm 2 ~5E15 atom / cm 2 .
[0078] Table 1 is a data graph showing the breakdown voltage of the device as a function of the doping dosage of the transition doping region 210 .
[0079]
[0080] Table 1
[0081] As the doping dose of the transition doping region 210 increases, the resistance of the transition doping region 210 decreases, and the response speed of the device increases. At the same time, it can be seen from Table 1 that as the doping dose of the transition doping region 210 increases, the breakdown voltage of the device decreases.
[0082] Therefore, it is necessary to control the doping dose of the transition doping region 210 to avoid the doping dose of the transition doping region 210 being too large, which causes the breakdown voltage of the device to be reduced; and to avoid the doping dose of the transition doping region 210 being too small, which causes the response speed of the device to be too slow.
[0083] In the process of performing doping treatment on the substrate 200 between the gate trench 207 and the implanted doping region 209 to form the transitional doping region 210 between the bottom of the gate trench 207 and the implanted doping region 209, the angle between the implantation direction of the doping treatment and the normal direction of the substrate 200 is in the range of 15° to 45°. By adopting the inclined implantation angle, the cross-sectional area of the transitional doping region 210 of the same type as the implanted doping region 209 formed by the sidewall of the gate trench 207 and the bottom of the gate trench 207 in the direction parallel to the substrate surface is larger, thereby increasing the contact area between the transitional doping region 210 and the initial body doping region 204 and strengthening the electrical connection between the transitional doping region 210 and the initial body doping region 204.
[0084] Please refer to Fig.11 , Fig.11 Perspective and Fig. 9 Similarly, after forming the transition doping region 210, the hard mask layer 206 (eg, Fig. 9 As shown) and the sacrificial protection layer 208 (as shown Fig. 9 shown).
[0085] Specifically, in some embodiments of the present invention, wet etching is used to remove the hard mask layer 206 and the sacrificial protection layer 208. The hard mask layer 206 and the sacrificial protection layer 208 are removed in one step, saving process costs.
[0086] Please refer to Fig.12 , a gate structure 211 is formed in the gate trench 207 .
[0087] The step of forming a gate structure 211 in the gate trench 207 includes: forming a gate dielectric layer 212 on the sidewalls of the gate trench 207 and the bottom of the gate trench 207 ; and forming a gate layer 213 in the gate trench 207 having the gate dielectric layer 212 .
[0088] Specifically, in some embodiments of the present invention, a first gate oxide layer is formed on the sidewalls of the gate trench 207 and the bottom of the gate trench 207 using a low-temperature thermal oxidation process; a second gate oxide layer is formed on the first gate oxide layer using a deposition process; and a gate layer 213 is formed in the gate trench 207 having the first gate oxide layer and the second gate oxide layer located on the first gate oxide layer to form the gate structure 211.
[0089] Specifically, in some embodiments of the present invention, the step of forming the second gate oxide layer includes: depositing a TEOS silicon oxide layer; and rapidly annealing the TEOS silicon oxide layer. The purpose of the rapid annealing is to densify the TEOS silicon oxide layer.
[0090] The gate layer 213 is made of polysilicon. The steps of forming the gate layer 213 include: forming an initial gate layer in the gate trench 207 having a first gate oxide layer and a second gate oxide layer on the first gate oxide layer; and planarizing the initial gate layer to form the gate layer 213 .
[0091] The planarization treatment method includes mechanical polishing, chemical polishing, fluid polishing, and chemical mechanical polishing. Specifically, in this embodiment, the first planarization treatment method is chemical mechanical polishing. Different from the traditional pure mechanical or pure chemical polishing method, the chemical mechanical polishing method avoids the surface damage caused by pure mechanical polishing and the shortcomings of slow polishing speed, poor surface flatness and polishing consistency caused by pure chemical polishing through the combined action of chemistry and mechanics. Chemical mechanical polishing is widely used for high planarization polishing of various materials at the nano level.
[0092] Specifically, in some embodiments of the present invention, the thickness of the first gate oxide layer ranges from 100 angstroms to 400 angstroms; the oxidation temperature range of the low-temperature thermal oxidation process is from 800°C to 930°C; and the time of the low-temperature thermal oxidation process is less than 30 minutes.
[0093] The first gate oxide layer and the second gate oxide layer are formed by combining low-temperature oxidation and deposition, thereby reducing the thermal process introduced by thermal growth and lowering the degree of lateral diffusion of the implanted doping region 209 .
[0094] The doping method adopted by the transition doping region 210 is heavy doping injection. After thermal diffusion, the diffusion speed of the transition doping region 210 in the direction parallel to the surface of the substrate 200 is greater than the diffusion speed of the injection doping region 209 in the direction parallel to the surface of the substrate 200.
[0095] Please refer to Fig.13 After forming the gate structure 211, the initial body doping regions 204 (such as Fig.12 As shown in the figure, a doping treatment is performed to form a first heavily doped layer 214 and a body doped region 217; an interlayer dielectric layer 215 is formed on the gate structure 211 and the first heavily doped layer 214; a through hole is formed that penetrates the first heavily doped layer 214 and the interlayer dielectric layer 215; and the body doped region exposed at the bottom of the through hole is doped to form a second heavily doped layer 216.
[0096] The first heavily doped layer 214 is a source end heavily doped layer. Specifically, in some embodiments of the present invention, the first heavily doped layer 214 is N-type heavily doped, and the second heavily doped layer 216 is P-type heavily doped. In other embodiments, the first heavily doped layer may also be P-type heavily doped, and the second heavily doped layer may also be N-type heavily doped.
[0097] Specifically, in some embodiments of the present invention, the transition doping region 210 further extends between the gate structure 211 and the body doping region 217 .
[0098] The step of forming a through hole penetrating the first heavily doped layer 214 and the interlayer dielectric layer 215 includes: forming a mask layer on the interlayer dielectric layer 215, wherein the mask layer exposes a portion of the interlayer dielectric layer 215; and etching the interlayer dielectric layer 215 using the mask layer as a mask to form a through hole penetrating the first heavily doped layer 214 and the interlayer dielectric layer 215. Specifically, in some embodiments of the present invention, after the through hole is formed, the mask layer is not removed.
[0099] The step of performing a doping treatment on the body doping region 217 exposed at the bottom of the through hole to form a second heavily doped layer 216 includes: using the mask layer as a mask, performing a doping treatment on the body doping region 217 exposed at the bottom of the through hole to form a second heavily doped layer 216. The doping type of the second heavily doped layer 216 is opposite to that of the first heavily doped layer 214. Specifically, in some embodiments of the present invention, the second heavily doped layer 216 is P-type heavily doped, and in other embodiments, the second heavily doped layer may also be N-type heavily doped.
[0100] After forming the second heavily doped layer 216 , the method further includes: forming a conductive plug 218 in the through hole.
[0101] Please refer to Figures 14 to 16 , Fig.14 yes Fig.15 and Fig.16 A top view of Fig.15 yes Fig.14 Cross-sectional view at BB1 position, Fig.16 yes Fig.14 A cross-sectional view at position CC1 is shown in FIG. 2 . A drain metal layer 219 is formed on the side of the substrate 201 away from the epitaxial layer 202 . A source metal layer 220 is formed on the conductive plug 218 , and a gate metal layer 221 is formed on the gate structure 211 .
[0102] Accordingly, the embodiment of the present invention further provides a semiconductor structure, please refer to Fig.15 , comprising: a substrate 200, the substrate 200 comprising a drift region 203; a gate structure 211 partially located in the drift region 203; an implanted doping region 209 having a doping type opposite to that of the drift region 203, the implanted doping region 209 being located under the gate structure 211, and the position of the implanted doping region 209 corresponding to the position of the gate structure 211.
[0103] The semiconductor structure includes a substrate 200 , and the substrate 200 includes a drift region 203 .
[0104] The base 200 includes a substrate 201 and an epitaxial layer 202 (eg, Figure 5 As shown), the drift region 203 is located in the epitaxial layer 202.
[0105] The material of the substrate 201 includes: silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium; the material of the epitaxial layer 202 includes: silicon, germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium. Specifically, in some embodiments of the present invention, the material of the substrate 201 is silicon, and the material of the epitaxial layer 202 is silicon.
[0106] Specifically, in some embodiments of the present invention, the substrate 201 is N-type doped, the epitaxial layer 202 is N-type doped, and the doping concentration of the epitaxial layer 202 is in the range of 5E15atom / cm 3 ~1E17atom / cm 3 .
[0107] The semiconductor structure includes: a body doping region 217 located on the drift region 203, and the doping type of the body doping region 217 is opposite to the doping type of the drift region 203. Specifically, in some embodiments of the present invention, the body doping region 217 is P-type doped. In other embodiments, the substrate further includes P-type doping, the epitaxial layer further includes P-type doping, and the body doping region 217 further includes N-type doping.
[0108] The semiconductor structure includes a gate structure 211 partially located in the drift region 203 .
[0109] The gate structure 211 includes a gate dielectric layer 212 and a gate layer 213 located on the gate dielectric layer 212; specifically, in some embodiments of the present invention, the gate structure 211 includes: a first gate oxide layer, a second gate oxide layer located on the first gate oxide layer, and a gate layer 213 located on the second gate oxide layer.
[0110] The material of the first gate oxide layer is silicon oxide; the material of the second gate oxide layer is silicon oxide; the material of the gate layer 213 is polysilicon. The thickness of the first gate oxide layer ranges from 100 angstroms to 400 angstroms.
[0111] The semiconductor structure includes: an implantation doping region 209 having a doping type opposite to that of the drift region 203 , the implantation doping region 209 being located under the gate structure 211 , and the position of the implantation doping region 209 corresponding to the position of the gate structure 211 .
[0112] The projection of the implanted doped region 209 on the surface of the substrate 200 at least partially overlaps with the projection of the gate structure 211 on the surface of the substrate 200. Specifically, in some embodiments of the present invention, the projection of the gate structure 211 on the surface of the substrate 200 is within the range of the projection of the implanted doped region 209 on the surface of the substrate 200.
[0113] The semiconductor structure includes: a transition doping region 210 with the same doping type located between the gate structure 211 and the implanted doping region 209 , the transition doping region 210 is in electrical contact with the implanted doping region 209 and the position of the transition doping region 210 corresponds to that of the implanted doping region 209 .
[0114] The doping concentration of the transition doping region 210 is greater than the doping concentration of the implantation doping region 209 .
[0115] The projection of the implanted doping region 209 on the surface of the substrate 200 at least partially overlaps with the projection of the transitional doping region 210 on the surface of the substrate 200 .
[0116] The projection of the implanted doping region 209 on the surface of the substrate 200 is located within the projection range of the transitional doping region 210 on the surface of the substrate 200 .
[0117] The transition doping region 210 further extends between the gate structure 211 and the drift region 203 .
[0118] The gate structure 211 penetrates the body doping region along a direction vertical to the surface of the substrate 200 , and the body doping region 217 is electrically connected to the transition doping region 210 .
[0119] The transition doping region 210 further extends between the gate structure 211 and the body doping region 217 .
[0120] The semiconductor structure includes: a first heavily doped layer 214 located on the body doped region 217 , wherein the doping type of the first heavily doped layer 214 is opposite to the doping type of the body doped region 217 .
[0121] The gate structure 211 penetrates the first heavily doped layer 214 along a direction perpendicular to the surface of the substrate 200 .
[0122] The semiconductor structure includes: a conductive plug 218 penetrating the first heavily doped layer 214, the conductive plug 218 being electrically connected to the body doped region; a second heavily doped layer 216 located at the bottom of the conductive plug 218, the second heavily doped layer 216 being electrically connected to the conductive plug 218, the doping type of the second heavily doped layer 216 being the same as the doping type of the body doped region, and the doping concentration of the second heavily doped layer 216 being greater than the doping concentration of the body doped region.
[0123] The semiconductor structure includes: a drain metal layer 219 located on a side of the substrate 201 away from the epitaxial layer 202 .
[0124] The semiconductor structure includes: a source metal layer 220 located on the conductive plug 218 and a gate metal layer 221 located on the gate structure 211 .
[0125] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A semiconductor structure, characterized in that include: a substrate comprising a drift region; a gate structure partially located within the drift region; An implantation doping region having a doping type opposite to that of the drift region, wherein the implantation doping region is located under the gate structure, and a position of the implantation doping region corresponds to a position of the gate structure.
2. The semiconductor structure according to claim 1, wherein The projection of the implanted doped region on the substrate surface at least partially overlaps with the projection of the gate structure on the substrate surface.
3. The semiconductor structure according to claim 1, wherein: The projection of the gate structure on the substrate surface is located within the range of the projection of the implanted doping region on the substrate surface.
4. The semiconductor structure according to claim 1, wherein: Also includes: A transition doping region with the same doping type as that of the implanted doping region is located between the gate structure and the implanted doping region, the transition doping region is in electrical contact with the implanted doping region and the position of the transition doping region corresponds to that of the implanted doping region.
5. The semiconductor structure according to claim 4, wherein: The doping concentration of the transition doping region is greater than the doping concentration of the implantation doping region.
6. The semiconductor structure according to claim 4, wherein: The projection of the implanted doping region on the substrate surface at least partially overlaps with the projection of the transitional doping region on the substrate surface.
7. The semiconductor structure according to claim 4, wherein: The projection of the implanted doping region on the substrate surface is located within the projection range of the transitional doping region on the substrate surface.
8. The semiconductor structure according to claim 4, wherein: The transition doping region further extends between the gate structure and the drift region.
9. The semiconductor structure according to claim 4, wherein: Also includes: a body-doped region located on the drift region, wherein a doping type of the body-doped region is opposite to a doping type of the drift region; The gate structure penetrates the body doping region in a direction perpendicular to the substrate surface, and the body doping region is electrically connected to the transition doping region.
10. The semiconductor structure according to claim 9, wherein: The transition doped region further extends between the gate structure and the body doped region.
11. The semiconductor structure according to claim 9, wherein: The invention further comprises: a first heavily doped layer located on the body doped region, wherein the doping type of the first heavily doped layer is opposite to the doping type of the body doped region; The gate structure penetrates the first heavily doped layer in a direction perpendicular to the surface of the substrate.
12. The semiconductor structure according to claim 11, wherein Also includes: a conductive plug penetrating the first heavily doped layer, the conductive plug being electrically connected to the body-doped region; and a second heavily doped layer located at the bottom of the conductive plug, the second heavily doped layer being electrically connected to the conductive plug, the doping type of the second heavily doped layer being the same as the doping type of the body-doped region, and the doping concentration of the second heavily doped layer being greater than the doping concentration of the body-doped region.
13. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, the substrate comprising a substrate and an epitaxial layer located on the substrate; Etching the substrate to form a gate trench in the epitaxial layer; Performing a doping treatment on the substrate exposed by the gate trench to form an implanted doping region located under the gate trench, wherein the position of the implanted doping region corresponds to the position of the gate trench; A gate structure is formed in the gate trench.
14. The method for forming a semiconductor structure according to claim 13, wherein: The step of etching the substrate to form a gate trench in the epitaxial layer includes: forming a hard mask layer having an opening on the substrate; The substrate is etched using the hard mask layer as a mask to form a gate trench in the epitaxial layer.
15. The method for forming a semiconductor structure according to claim 14, wherein: In the process of performing doping treatment on the substrate exposed by the gate trench to form an implanted doping region located under the gate trench, the substrate exposed by the gate trench is doped using the hard mask layer as a mask.
16. The method for forming a semiconductor structure according to claim 14, wherein: After the substrate exposed by the gate trench is doped to form an injection doping region located under the gate trench, and before the gate structure is formed in the gate trench, the method further includes: doping the substrate located between the gate trench and the injection doping region to form a transition doping region located between the bottom of the gate trench and the injection doping region, wherein the transition doping region is electrically connected to the injection doping region and the position of the transition doping region corresponds to the position of the injection doping region.
17. The method for forming a semiconductor structure according to claim 16, wherein: In the process of doping the substrate between the gate trench and the implanted doping region to form a transitional doping region between the bottom of the gate trench and the implanted doping region, the substrate between the gate trench and the implanted doping region is doped using the hard mask layer as a mask.
18. The method for forming a semiconductor structure according to claim 17, wherein: The substrate exposed by the gate trench is doped to form an implanted doping region located below the gate trench, and the doping dose of the doping treatment is less than the doping dose of the substrate located between the gate trench and the implanted doping region to form a transitional doping region located between the bottom of the gate trench and the implanted doping region.
19. The method for forming a semiconductor structure according to claim 16, wherein: In the process of performing doping treatment on the substrate located between the gate trench and the implanted doping region to form a transitional doping region located between the bottom of the gate trench and the implanted doping region, the angle between the implantation direction of the doping treatment and the normal direction of the substrate is in the range of 15° to 45°.
20. The method for forming a semiconductor structure according to claim 13, wherein: Also includes: After etching the substrate to form a gate trench in the epitaxial layer, and before doping the substrate exposed by the gate trench to form an implanted doping region under the gate trench, performing an oxidation repair treatment on the gate trench to form a sacrificial protection layer on the surface of the gate trench; In the step of doping the substrate exposed by the gate trench to form an implanted doping region under the gate trench, the substrate exposed by the gate trench having a sacrificial protective layer on the trench surface is doped to form an implanted doping region under the gate trench.
21. The method for forming a semiconductor structure according to claim 13, wherein: The step of forming a gate structure in the gate trench comprises: forming a first gate oxide layer on the sidewalls of the gate trench and the bottom of the gate trench by a low temperature thermal oxidation process; forming a second gate oxide layer on the first gate oxide layer by a deposition process; A gate layer is formed in a gate trench having a first gate oxide layer and a second gate oxide layer located on the first gate oxide layer to form the gate structure.
22. The method for forming a semiconductor structure according to claim 13, wherein: Before etching the substrate to form a gate trench in the epitaxial layer, the method further includes: performing doping treatment on the epitaxial layer to form a drift region and an initial body doping region on the drift region.
23. The method for forming a semiconductor structure according to claim 22, wherein: Also includes: After forming the gate structure, the initial body doping regions located on both sides of the gate structure are doped to form a first heavily doped layer.
Citation Information
Cited By