Semiconductor device, memory device, and method for manufacturing semiconductor device

By optimizing the insulating layer structure of the transistor and the orientation of the oxide layer, the problems of small on-state current and large parasitic capacitance in the existing semiconductor devices are solved, and semiconductor devices and display devices with high density and low power consumption are realized.

CN119031706APending Publication Date: 2024-11-26SEMICON ENERGY LAB CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410637530.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-01
Filing Date
2024-05-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In existing semiconductor devices, the transistor has a small on-state current and a large parasitic capacitance, making it difficult to achieve miniaturization or high integration, and has a high power consumption, which cannot meet the demands of electronic devices for high density and low power consumption.

Method used

A transistor structure including a first insulating layer and a second insulating layer is adopted, wherein the transistor has a first conductive layer, a second conductive layer, a semiconductor layer and a gate insulating layer, and the second insulating layer is located in the first conductive layer and the second conductive layer. Between, the second conductive layer is located on the second insulating layer, and by forming a plurality of crystallization portions to optimize the c-axis orientation and crystallization structure of the oxide layer, reduce contact resistance, improve channel length and on-state current.

Benefits of technology

It realizes transistors with good electrical characteristics, with large on-state current and small parasitic capacitance, and supports miniaturized or highly integrated semiconductor devices and display devices, reducing power consumption, improving reliability and working speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031706A_ABST
    Figure CN119031706A_ABST
Patent Text Reader

Abstract

Provided is a transistor having good electrical characteristics. Provided is a transistor having a large on-state current. Provided is a transistor having low parasitic capacitance. Provided are a transistor, a semiconductor device, or a memory device capable of achieving miniaturization or high integration. The transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer on the semiconductor layer, and a gate electrode on the gate insulating layer, the first insulating layer being located between the first conductive layer and the second conductive layer, the second conductive layer being located on the first insulating layer, the first insulating layer and the second conductive layer having an opening portion reaching the first conductive layer, the semiconductor layer is in contact with the side wall of the opening part and comprises a first oxide layer and a second oxide layer, the first oxide layer is provided with a first region and a second region, and the second oxide layer is located between the first region and the second region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device, a storage device, a display device, and an electronic device. Another embodiment of the present invention relates to a method for manufacturing a semiconductor device.

[0002] Note that one embodiment of the present invention is not limited to the above-mentioned technical field. As an example of the technical field of one embodiment of the present invention, a semiconductor device, a display device, a light-emitting device, a power storage device, a storage device, an electronic device, a lighting device, an input device (e.g., a touch sensor), an input-output device (e.g., a touch panel), and a driving method or a manufacturing method of the above-mentioned device can be cited.

[0003] In this specification, etc., a semiconductor device refers to a device that utilizes semiconductor characteristics, a circuit including a semiconductor element (transistor, diode, photodiode, etc.), and a device including the circuit. In addition, a semiconductor device refers to all devices that can function by utilizing semiconductor characteristics. For example, as examples of semiconductor devices, there are integrated circuits, chips with integrated circuits, and electronic components that contain chips in packages. In addition, storage devices, display devices, light-emitting devices, lighting devices, and electronic devices themselves are semiconductor devices, and sometimes all include semiconductor devices. Background Art

[0004] In recent years, semiconductor devices have been developed, and LSI, CPU, memory, etc. are mainly used for semiconductor devices. CPU is an aggregate of semiconductor elements including a semiconductor integrated circuit (including at least transistors and memory) processed into a chip by a semiconductor wafer and having electrodes formed as connection terminals.

[0005] Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as one of the components of various electronic devices.

[0006] In addition, the technology of forming a transistor using a semiconductor thin film formed on a substrate having an insulating surface has attracted attention. The transistor is widely used in electronic devices such as integrated circuits (ICs) and display devices. As a semiconductor thin film that can be applied to transistors, silicon-based semiconductor materials are widely known. As other materials, oxide semiconductors have attracted attention.

[0007] In addition, it is known that the leakage current of a transistor using an oxide semiconductor is extremely small in the off state. For example, Patent Document 1 has disclosed a low-power CPU that utilizes the small leakage current characteristic of a transistor using an oxide semiconductor. In addition, for example, Patent Document 2 discloses a storage device that utilizes the small leakage current characteristic of a transistor using an oxide semiconductor to achieve long-term retention of stored content.

[0008] In recent years, with the miniaturization and lightness of electronic devices, the demand for further high density of integrated circuits has increased. In addition, it is required to improve the productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technology in which a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film are stacked and a plurality of memory cells are arranged in an overlapping manner, thereby increasing the density of the integrated circuit. In addition, Patent Document 4 discloses a technology in which the channel of a transistor using an oxide semiconductor film is configured vertically to achieve high density of the integrated circuit.

[0009] [Patent Document 1] Japanese Patent Application Publication No. 2012-257187 [Patent Document 2] Japanese Patent Application Publication No. 2011-151383 [Patent Document 3] International Patent Application Publication No. 2021 / 053473 [Patent Document 4] Japanese Patent Application Publication No. 2013-211537 [Non-patent literature]

[0010] [Non-patent document 1] M. Oota et al., “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig., 2019, pp. 50-53 Summary of the invention

[0011] One of the purposes of one embodiment of the present invention is to provide a transistor with good electrical characteristics. In addition, one of the purposes of one embodiment of the present invention is to provide a transistor with large on-state current. In addition, one of the purposes of one embodiment of the present invention is to provide a transistor with small parasitic capacitance. In addition, one of the purposes of one embodiment of the present invention is to provide a transistor, semiconductor device or storage device that can achieve miniaturization or high integration. In addition, one of the purposes of one embodiment of the present invention is to provide a high-definition or high-aperture display device. In addition, one of the purposes of one embodiment of the present invention is to provide a transistor, semiconductor device, display device or storage device with high reliability. In addition, one of the purposes of one embodiment of the present invention is to provide a semiconductor device, display device or storage device with low power consumption. In addition, one of the purposes of one embodiment of the present invention is to provide a storage device with a fast operating speed. In addition, one of the purposes of one embodiment of the present invention is to provide a method for manufacturing the above-mentioned transistor, semiconductor device, display device or storage device.

[0012] Note that the description of these objectives does not prevent the existence of other objectives. One embodiment of the present invention does not need to achieve all of the above objectives. Objectives other than the above objectives can be extracted from the description of the specification, drawings, and claims.

[0013] One embodiment of the present invention is a semiconductor device, comprising: a transistor on a first insulating layer; and a second insulating layer, wherein the transistor comprises a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer and a gate electrode on the first insulating layer, the second insulating layer is located between the first conductive layer and the second conductive layer, the second conductive layer is located on the second insulating layer, the second insulating layer and the second conductive layer have an opening reaching the first conductive layer, the semiconductor layer is in contact with the side surface of the second insulating layer in the opening and the side surface of the second conductive layer in the opening, the gate insulating layer is located on the semiconductor layer, the gate electrode has a region overlapping with the semiconductor layer via the gate insulating layer in the opening, the semiconductor layer comprises a first oxide layer and a second oxide layer, the first oxide layer has a first region and a second region, the first region and the second region respectively have a plurality of crystal portions, and the second oxide layer is located between the first region and the second region.

[0014] In the above structure, the plurality of crystal parts preferably have c-axis orientation.

[0015] In the above structure, the second oxide layer preferably includes a crystal portion having the same crystal structure as the plurality of crystal portions.

[0016] In the above structure, the second oxide layer preferably includes a crystal portion connected to one of the plurality of crystal portions.

[0017] In the above structure, preferably, a boundary between the first oxide layer and the second oxide layer cannot be observed in a cross-sectional TEM image.

[0018] In the above structure, preferably, the first conductive layer has a recessed portion overlapping the opening, and the semiconductor layer has a region embedded in the recessed portion.

[0019] In the above structure, preferably, the opening portion has an eighth region whose side walls are conical in shape and a ninth region whose side walls are steeper than the eighth region, the eighth region has an upper end of the opening portion, the ninth region is located below the eighth region, the eighth region has a side surface of the second conductive layer, and the ninth region has a side surface of the second insulating layer.

[0020] In the above structure, preferably, the angle formed by the side wall of the eighth region and the top surface of the first insulating layer is greater than 20 degrees and less than 75 degrees, and the angle formed by the side wall of the ninth region and the top surface of the first insulating layer is greater than 75 degrees and less than 90 degrees.

[0021] One embodiment of the present invention is a method for manufacturing a semiconductor device, comprising the following steps: forming a first insulating layer on a first conductive layer; forming a second conductive layer on the first insulating layer; forming a first opening reaching the first conductive layer and exposing the top surface of the first conductive layer by removing a portion of the second conductive layer and a portion of the first insulating layer; and forming a semiconductor layer in contact with the top surface of the first conductive layer, the side surface of the first insulating layer in the first opening, the side surface of the second conductive layer in the first opening, and the top surface of the second conductive layer, wherein the semiconductor layer is formed by a first process of forming a first oxide layer, a second process of forming a second oxide layer, and a third process of performing a heat treatment, the first oxide layer is formed by sputtering, the second oxide layer is formed by atomic layer deposition, the second insulating layer is formed in contact with the top surface of the semiconductor layer and the top surface of the first insulating layer, and a third conductive layer is formed on the second insulating layer.

[0022] One embodiment of the present invention is a storage device, comprising: a first insulating layer; a capacitor; and a transistor on the capacitor, wherein the transistor comprises a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode, the capacitor comprises a third conductive layer, a second insulating layer on the third conductive layer, and a first conductive layer on the second insulating layer, the first insulating layer is located between the first conductive layer and the second conductive layer, the second conductive layer is located on the first insulating layer, the first insulating layer and the second conductive layer have an opening that reaches the first conductive layer, the semiconductor layer is in contact with a side surface of the first insulating layer in the opening and a side surface of the second conductive layer in the opening, the gate insulating layer is located on the semiconductor layer, the gate electrode has a region overlapping with the semiconductor layer via the gate insulating layer in the opening, the semiconductor layer comprises a metal oxide, in the transistor, an Id-Vgs characteristic of the transistor is measured at a drain-source voltage of 0.05 V or more and 1 V or less, Id is a drain current and Vgs is a gate-source voltage, and in the Id-Vgs characteristic, Id is 1×10 -12 Vgs at [A] is greater than 0V and less than 0.5V.

[0023] In the above method, preferably, the metal oxide is In-M-Zn oxide, and the element M is one or more selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium and antimony.

[0024] In the above aspect, the retention time of the storage device is preferably 0.64 seconds or longer.

[0025] In the above method, preferably, when the gate of the transistor is set to 0 V, the source of the transistor is set to 0 V, and a voltage of 0.05 V to 1 V is applied to the drain of the transistor, the accumulated amount of charge flowing through the transistor for 0.64 seconds is 3×10 -15 [F]×0.1[V] or less.

[0026] In the above aspect, the writing time of the storage device is preferably 15 ns or less.

[0027] In the above aspect, the read time of the storage device is preferably 15 ns or less.

[0028] In the above method, it is preferred that the write time is calculated using a circuit including a first load connected to the gate of the transistor and a second load connected to the drain of the transistor, the first load includes 256 first circuits, each of the multiple first circuits includes a first resistor and a second capacitor, the second load includes 32 second circuits, each of the multiple second circuits includes a second resistor and a third capacitor, the multiple first resistors included in the first circuits are connected in series, the multiple second resistors included in the second circuits are connected in series, the resistance value of the first resistor is greater than 1Ω and less than 100Ω, the resistance value of the second resistor is greater than 1Ω and less than 100Ω, the capacitance value of the second capacitor is greater than 1aF and less than 0.5fF, and the capacitance value of the third capacitor is greater than 1aF and less than 0.5fF.

[0029] In the above method, it is preferred that the read time is calculated using a circuit including a first load connected to the gate of the transistor and a second load connected to the drain of the transistor, the first load includes 256 first circuits, each of the plurality of first circuits includes a first resistor and a second capacitor, the second load includes 32 second circuits, each of the plurality of second circuits includes a second resistor and a third capacitor, the plurality of first resistors included in the first circuits are connected in series, the plurality of second resistors included in the second circuits are connected in series, the resistance value of the first resistor is greater than 1Ω and less than 100Ω, the resistance value of the second resistor is greater than 1Ω and less than 100Ω, the capacitance value of the second capacitor is greater than 1aF and less than 0.5fF, and the capacitance value of the third capacitor is greater than 1aF and less than 0.5fF.

[0030] According to one embodiment of the present invention, a transistor with good electrical characteristics can be provided. In addition, according to one embodiment of the present invention, a transistor with large on-state current can be provided. In addition, according to one embodiment of the present invention, a transistor with small parasitic capacitance can be provided. In addition, according to one embodiment of the present invention, a transistor, semiconductor device or storage device capable of miniaturization or high integration can be provided. In addition, according to one embodiment of the present invention, a display device with high definition or high aperture ratio can be provided. In addition, according to one embodiment of the present invention, a transistor, semiconductor device, display device or storage device with high reliability can be provided. In addition, according to one embodiment of the present invention, a semiconductor device, display device or storage device with low power consumption can be provided. In addition, according to one embodiment of the present invention, a storage device with fast operating speed can be provided. In addition, according to one embodiment of the present invention, a method for manufacturing the above-mentioned transistor, semiconductor device, display device or storage device can be provided.

[0031] Note that the description of these effects does not prevent the existence of other effects. One embodiment of the present invention does not necessarily have all of the above effects. Effects other than the above effects can be extracted from the description of the specification, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1A is a plan view showing an example of a semiconductor device, Figure 1B and Figure 1C is a cross-sectional view showing an example of a semiconductor device; Figure 2A is a plan view showing an example of a semiconductor device, Figure 2B and Figure 2C is a cross-sectional view showing an example of a semiconductor device; Figure 3A is a plan view showing an example of a semiconductor device, FIG. 3B to FIG. 3D is a cross-sectional view showing an example of a semiconductor device; Figure 4A is a plan view showing an example of a semiconductor device, Figure 4B and Figure 4C is a cross-sectional view showing an example of a semiconductor device; FIG. 5A to FIG. 5C is a cross-sectional view showing an example of a semiconductor device; FIG. 6A to FIG. 6D is a cross-sectional view showing an example of a semiconductor device; Fig. 7A and Figure 7B is a cross-sectional view showing an example of a semiconductor device; Fig. 8A and Figure 8B is a cross-sectional view showing an example of a semiconductor device; Fig.9A and Fig. 9B is a cross-sectional view showing an example of a semiconductor device; Fig. 10A and Fig. 10B is a cross-sectional view showing an example of a semiconductor device; FIG. 11A to FIG. 11D is a diagram illustrating a cross section of an oxide semiconductor; FIG. 12A to FIG. 12C is a cross-sectional view showing an example of a method for manufacturing a semiconductor device; Fig.13A is a plan view showing an example of a storage device, Fig. 13B and Fig. 13C is a cross-sectional view showing an example of a storage device; Fig.14A is a plan view showing an example of a storage device, Fig. 14B and Fig. 14C is a cross-sectional view showing an example of a storage device; Fig.15A is a plan view showing an example of a storage device, Fig. 15B is a cross-sectional view showing an example of a storage device; Fig.16 is a cross-sectional view showing an example of a storage device; Fig.17 is a cross-sectional view showing an example of a storage device; Fig.18 is a block diagram illustrating a structural example of a semiconductor device; FIG. 19A to FIG. 19H is a diagram illustrating an example of a circuit configuration of a memory cell; Fig. 20A and Fig. 20B is a perspective view illustrating a structural example of a semiconductor device; Fig.21 is a block diagram illustrating a CPU; Fig.22A and Fig. 22B is a three-dimensional diagram of a semiconductor device; Fig.23A and Fig. 23B is a three-dimensional diagram of a semiconductor device; Fig.24A and Fig. 24B is a diagram showing various storage devices in a hierarchical manner; Fig.25A and Fig.25B is a perspective view showing an example of a display device; Fig.26 is a cross-sectional view showing an example of a display device; Fig. 27is a cross-sectional view showing an example of a display device; FIG. 28A to FIG. 28C is a diagram showing a structural example of a display device; Fig.29A and Fig.29B is a diagram showing an example of an electronic component; FIG. 30A to FIG. 30C is a diagram showing an example of a large computer, Fig.30D is a diagram showing an example of a space device, Fig.30E is a diagram showing an example of a storage system that may be used in a data center; FIG. 31A to FIG. 31F is a diagram showing an example of an electronic device; FIG. 32A to FIG. 32G is a diagram showing an example of an electronic device; FIG. 33A to FIG. 33F is a diagram showing an example of an electronic device; Fig.34A and Fig.34B is a diagram showing Id-Vg characteristics; Fig.35A and Fig.35B is a diagram showing Id-Vd characteristics; Fig.36 It is a circuit diagram used for circuit simulation; Fig.37A and Fig.37B It is a timing diagram that illustrates the operation of the circuit; FIG. 38A to FIG. 38C is a cross-sectional TEM image according to Example 3; FIG. 39A to FIG. 39C is a diagram showing the crystal orientation according to Example 3; Fig.40 is a diagram showing Id-Vgs characteristics; FIG. 41A to FIG. 41C It is a timing diagram that illustrates the operation of the circuit; Fig.42A and Fig.42B is the result of circuit simulation; Fig.43 is a cross-sectional TEM image according to Example 5; Fig.44 is a cross-sectional TEM image according to Example 5; Fig.45 is a circuit diagram according to Embodiment 6; Fig.46 is a diagram showing the measurement results of the current of the transistor. DETAILED DESCRIPTION

[0033] The embodiments are described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the following description, and a person skilled in the art can easily understand that the mode and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the embodiments shown below.

[0034] Note that in the invention structure described below, the same symbol is shared in different drawings to show the same part or part with the same function, and repeated description is omitted. In addition, when representing a part with the same function, the same hatching is sometimes used without adding a special reference numeral.

[0035] For ease of understanding, the position, size, and range of each component shown in the drawings may not represent its actual position, size, and range. Therefore, the disclosed invention is not necessarily limited to the position, size, and range disclosed in the drawings.

[0036] Note that in this specification, etc., ordinal numbers such as "first" and "second" are added for convenience, but they do not limit the number of components or the order of components (for example, the order of processes or the order of stacking). In addition, the ordinal numbers added to components in one part of this specification may not be consistent with the ordinal numbers added to the components in other parts of this specification or claims.

[0037] A transistor is a type of semiconductor element and can realize a function of amplifying current or voltage and a switch operation of controlling conduction or non-conduction, etc. The transistor in this specification includes an IGFET (Insulated Gate Field Effect Transistor) and a thin film transistor (TFT: Thin Film Transistor).

[0038] In this specification, etc., a transistor using an oxide semiconductor or metal oxide for a semiconductor layer and a transistor including an oxide semiconductor or metal oxide in a channel formation region may be referred to as an OS transistor. Also, a transistor including silicon in a channel formation region may be referred to as a Si transistor.

[0039] In this specification, etc., a transistor refers to an element including at least three terminals: a gate, a drain, and a source. The transistor has a region (also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel formation region. Note that in this specification, etc., a channel formation region refers to a region where current mainly flows.

[0040] In addition, when transistors with different polarities are used or the direction of current changes during circuit operation, the functions of the source and the drain may be interchanged. Therefore, in this specification, the source and the drain may be interchanged.

[0041] Note that the impurities of a semiconductor refer to, for example, elements other than the main components that constitute the semiconductor. For example, an element with a concentration lower than 0.1 atomic% can be said to be an impurity. When impurities are contained, for example, the defect state density of the semiconductor may increase or the crystallinity may decrease. When the semiconductor is an oxide semiconductor, the impurities that change the properties of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specifically, for example, there are hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, nitrogen, etc. In addition, water sometimes acts as an impurity. In addition, for example, the mixing of impurities sometimes leads to oxygen vacancies (also recorded as V O )’s formation.

[0042] Note that in this specification and the like, an oxynitride refers to a material containing more oxygen than nitrogen in its composition, and an oxynitride refers to a material containing more nitrogen than oxygen in its composition.

[0043] For example, the content of hydrogen, oxygen, carbon, nitrogen and other elements in the film can be analyzed by secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS). XPS is suitable when the content of the target element is high (for example, 0.5 atomic% or more or 1 atomic%). On the other hand, SIMS is suitable when the content of the target element is low (for example, 0.5 atomic% or less or 1 atomic%). When comparing the content of elements, it is more preferable to use a composite analysis using both SIMS and XPS analysis techniques.

[0044] In addition, depending on the situation or state, the "film" and the "layer" may be interchanged. For example, the "conductive layer" may be replaced with the "conductive film". In addition, the "insulating film" may be replaced with the "insulating layer".

[0045] In this specification, etc., "parallel" refers to a state where the angle formed by two straight lines is greater than -10° and less than 10°. Therefore, a state where the angle is greater than -5° and less than 5° is also included. "Approximately parallel" refers to a state where the angle formed by two straight lines is greater than -30° and less than 30°. In addition, "perpendicular" refers to a state where the angle formed by two straight lines is greater than 80° and less than 100°. Therefore, a state where the angle is greater than 85° and less than 95° is also included. "Approximately perpendicular" refers to a state where the angle formed by two straight lines is greater than 60° and less than 120°.

[0046] In this specification, "electrical connection" includes connection through "an element having some kind of electrical function". Here, "an element having some kind of electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "an element having some kind of electrical function" includes switching elements such as transistors, resistors, coils, and other elements having various functions in addition to electrodes and wiring.

[0047] In addition, in this specification, etc., unless otherwise specified, off-state current refers to the leakage current between the source and the drain when the transistor is in the off state (also called non-conducting state or blocking state). In n-channel transistors, the off state refers to the voltage V between the gate and the source. gs Below the threshold voltage V th (In a p-channel transistor, V gs Higher than V th ) status.

[0048] In this specification, etc., the normally-on characteristic refers to a state in which a channel exists and current flows through a transistor even when no voltage is applied to the gate. In addition, the normally-off characteristic refers to a state in which current does not flow through a transistor when no voltage is applied to the gate or when a ground potential is supplied to the gate.

[0049] In this specification, the top surface shape of a component refers to the outline shape of the component when viewed in a plan view. In addition, the plan view refers to the situation when viewed from the normal direction of the surface on which the component is formed or the surface of the support (e.g., substrate) on which the component is formed.

[0050] In this specification, etc., "the top surface shapes are roughly consistent" means that at least a portion of the edges of each layer in the stack overlap. For example, it includes the case where the upper layer and the lower layer are processed by the same mask pattern or a portion of the same mask pattern. However, in reality, there are cases where the edges do not overlap, and sometimes the upper layer is located on the inner side of the lower layer or the upper layer is located on the outer side of the lower layer. In this case, it can also be said that "the top surface shapes are roughly consistent". When the top surface shapes are consistent or roughly consistent, it can also be said that the ends are aligned or roughly aligned, or the side ends are aligned or roughly consistent.

[0051] In this specification, etc., a tapered shape refers to a shape in which at least a portion of the side surface of a constituent element is inclined relative to a substrate surface or a formed surface. For example, it is preferred to have a region where the angle formed by the inclined side surface and the substrate surface or the formed surface (also referred to as a taper angle) is greater than 0 degrees and less than 90 degrees. Here, the side surface, substrate surface, and formed surface of a constituent element do not necessarily have to be completely flat, and may also be a substantially planar shape with a slight curvature or a substantially planar shape with fine concave-convex shapes.

[0052] In this specification and the like, when there is a description that "A is in contact with B", at least a portion of A is in contact with B. Therefore, for example, it can be alternatively stated that A includes a region in contact with B.

[0053] In this specification and the like, when there is a description that “A is located on B”, at least a portion of A is located on B. Therefore, for example, it can be alternatively stated that A includes a region located on B.

[0054] In this specification and the like, when there is a description that "A covers B", at least a portion of A covers B. Therefore, for example, it can be alternatively described that A includes a region covering B.

[0055] In this specification and the like, when there is a description that "A overlaps with B", at least a portion of A overlaps with B. Therefore, for example, it can be alternatively stated that A includes a region overlapping with B.

[0056] In this specification, etc., a device manufactured using a metal mask or FMM (Fine Metal Mask) is sometimes referred to as a device having an MM (Metal Mask) structure. In addition, in this specification, etc., a device manufactured without using a metal mask or FMM is sometimes referred to as a device having an MML (Metal Mask Less) structure.

[0057] In this specification, etc., a structure in which light-emitting layers are separately manufactured in light-emitting elements (also called light-emitting devices) with different emission wavelengths is sometimes referred to as an SBS (Side By Side) structure. Since the SBS structure can optimize the materials and structures of each light-emitting element, the freedom of choice of materials and structures is increased, and it is easy to achieve improved brightness and reliability.

[0058] In this specification, holes or electrons are sometimes referred to as "carriers". Specifically, a hole injection layer or an electron injection layer is sometimes referred to as a "carrier injection layer", a hole transport layer or an electron transport layer is sometimes referred to as a "carrier transport layer", and a hole blocking layer or an electron blocking layer is sometimes referred to as a "carrier blocking layer". Note that the above-mentioned carrier injection layer, carrier transport layer and carrier blocking layer are sometimes not clearly distinguishable. In addition, sometimes a layer has the functions of two or three of the carrier injection layer, the carrier transport layer and the carrier blocking layer.

[0059] In this specification, etc., a light-emitting element includes an EL layer between a pair of electrodes. The EL layer includes at least a light-emitting layer. Here, as the layer included in the EL layer (also referred to as a functional layer), a light-emitting layer, a carrier injection layer (hole injection layer and electron injection layer), a carrier transport layer (hole transport layer and electron transport layer) and a carrier blocking layer (hole blocking layer and electron blocking layer) can be cited. In this specification, etc., a light-receiving element (also referred to as a light-receiving device) includes at least an active layer used as a photoelectric conversion layer between a pair of electrodes. In this specification, etc., one of a pair of electrodes is sometimes referred to as a pixel electrode, and the other is referred to as a common electrode.

[0060] In this specification, etc., the sacrificial layer (also referred to as a mask layer) is located at least above the light-emitting layer (more specifically, a layer processed into an island shape among the layers constituting the EL layer) and has a function of protecting the light-emitting layer during the manufacturing process.

[0061] In this specification, etc., "island-shaped" means a state where two or more layers formed in the same process and using the same material are physically separated. For example, an island-shaped EL layer means a state where the EL layer is physically separated from an adjacent EL layer.

[0062] In this specification and the like, disconnection refers to a phenomenon in which a layer, a film, or an electrode is disconnected due to the shape of a formed surface (for example, a step, etc.).

[0063] Note that sometimes arrows indicating the X direction, Y direction, and Z direction are attached in the drawings of the present invention. Note that in this specification, "X direction" refers to the direction along the X axis, and sometimes the forward and reverse directions are not distinguished except for the cases clearly indicated. The same is true for "Y direction" and "Z direction". In addition, the X direction, Y direction, and Z direction are directions that intersect each other. For example, the X direction, Y direction, and Z direction are directions that are orthogonal to each other.

[0064] Implementation Method 1 In this embodiment, a semiconductor device which is one embodiment of the present invention is described.

[0065] A semiconductor device according to one embodiment of the present invention includes a first conductive layer, a second conductive layer, a third conductive layer, an oxide semiconductor layer, a first insulating layer, and a second insulating layer.

[0066] The first insulating layer is located on the first conductive layer, and the second conductive layer is located on the first insulating layer. The first insulating layer and the second conductive layer include an opening portion that reaches the first conductive layer. The oxide semiconductor layer is in contact with at least the top surface of the first conductive layer, the side surface of the first insulating layer, and the side surface of the second conductive layer in the opening portion. The second insulating layer is located on the oxide semiconductor layer in the opening portion. The third conductive layer overlaps the oxide semiconductor layer in the opening portion via the second insulating layer. Note that the opening portion is also referred to as an opening.

[0067] The first conductive layer is used as one of the source electrode and the drain electrode of the transistor. The second conductive layer is used as the other of the source electrode and the drain electrode of the transistor. The third conductive layer is used as the gate electrode of the transistor, and the second insulating layer is used as the gate insulating layer.

[0068] In this specification, the phrase "when viewed in section" may be used to describe the relationship between multiple components. For example, when describing the relationship between multiple components, the relationship when viewed in section from the same direction is described. In this case, the relationship between the multiple components can be described with reference to one cross-sectional view.

[0069] The source electrode and drain electrode of a transistor of one embodiment of the present invention are located at different heights, so the current flowing through the semiconductor layer flows in the height direction. In other words, it can be said that the channel length direction has a component in the height direction (vertical direction), so the transistor of one embodiment of the present invention can also be called VFET (Vertical Field Effect Transistor: vertical field effect transistor), vertical transistor, vertical channel transistor, etc.

[0070] Since the source electrode, the semiconductor layer, and the drain electrode can be overlapped, the occupied area of ​​the transistor of one embodiment of the present invention can be made much smaller than that of a so-called planar transistor in which the semiconductor layer is arranged in a planar shape.

[0071] Note that in this specification, "ends are consistent" refers to a situation where at least a portion of the contours of the stacked layers overlap when viewed from a plane. For example, this includes a situation where the upper layer and the lower layer are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, sometimes the contours do not overlap and the contour of the upper layer is located inside the contour of the lower layer or the contour of the upper layer is located outside the contour of the lower layer. These situations can also be said to be "ends consistent".

[0072] Note that, in general, it is sometimes difficult to clearly distinguish between “completely consistent” and “substantially consistent.” Therefore, in this specification, etc., “consistent” may include both completely consistent and substantially consistent.

[0073] <Structural Example 1 of Semiconductor Device> Reference FIG. 2A to FIG. 6D The structure of a semiconductor device according to one embodiment of the present invention will be described. Figure 2A is a plan view of a semiconductor device including the transistor 200 . Figure 2B It is along Figure 2A A cross-sectional view along the dashed line A1-A2 is shown. Figure 2C It is along Figure 2A A cross-sectional view along the dashed line A3-A4 is shown. Figure 3A is a cross-sectional view of the XY plane including the insulating layer 280. Note that Figure 2A In the plan view shown below, some components are omitted for clarity.

[0074] FIG. 2A to FIG. 2C and Figure 3A The semiconductor device shown includes an insulating layer 210 on a substrate (not shown), a transistor 200 on the insulating layer 210, and an insulating layer 280 on the insulating layer 210. The insulating layer 210 and the insulating layer 280 are used as interlayer films.

[0075] The transistor 200 includes a conductive layer 220, a conductive layer 240 on an insulating layer 280, an oxide semiconductor layer 230, an insulating layer 250 on the oxide semiconductor layer 230, and a conductive layer 260 on the insulating layer 250. The conductive layer 220 and the conductive layer 240 are located at different heights.

[0076] In transistor 200, oxide semiconductor layer 230 is used as a semiconductor layer, conductive layer 260 is used as a gate electrode, insulating layer 250 is used as a gate insulating layer, conductive layer 220 is used as one of a source electrode and a drain electrode, and conductive layer 240 is used as the other of the source electrode and the drain electrode.

[0077] A region of the oxide semiconductor layer 230 that is in contact with the conductive layer 220 and the conductive layer 240 is preferably used as a low-resistance region.

[0078] like Figure 2B and Figure 2C As shown in FIG. 2 , the insulating layer 280 and the conductive layer 240 are provided with an opening 290 that reaches the conductive layer 220. Fig.6D In the structure shown in FIG. 1 , the bottom of the opening 290 is, for example, the top surface of the conductive layer 220. Figure 2B and Figure 2CAs shown, when a recessed portion overlapping with the opening 290 is provided in the conductive layer 220, the opening 290 and the recessed portion of the conductive layer 220 sometimes constitute a continuous opening. In this case, for example, the region of the top surface of the conductive layer 220 overlapping with the opening 290 is a continuous bottom of the opening. The side walls of the opening 290 are the side surfaces of the insulating layer 280 and the side surfaces of the conductive layer 240. The opening 290 includes the opening of the insulating layer 280 and the opening of the conductive layer 240. In other words, the opening of the insulating layer 280 in the region overlapping with the conductive layer 220 is a part of the opening 290, and the opening of the conductive layer 240 in the region overlapping with the conductive layer 220 is another part of the opening 290. Note that among the openings 290, the opening 290 provided in the insulating layer 280 is referred to as the opening 290a, and the opening 290 provided in the conductive layer 240 is referred to as the opening 290b.

[0079] At least a portion of the components of the transistor 200 is disposed inside the opening 290. Specifically, at least a portion of each of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 is located inside the opening 290. The oxide semiconductor layer 230 is in contact with the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the side surface of the conductive layer 240 in the opening 290.

[0080] The insulating layer 280 includes an insulating layer 280a, an insulating layer 280b on the insulating layer 280a, and an insulating layer 280c on the insulating layer 280b. The insulating layer 280a has a region in contact with the top surface of the insulating layer 210, a region in contact with the side surface of the conductive layer 220, and a region in contact with the top surface of the conductive layer 220. The insulating layer 280c has a region in contact with the bottom surface of the conductive layer 240.

[0081] The oxide semiconductor layer 230 is provided inside the opening 290 of the insulating layer 280. In addition, since one of the source electrode and the drain electrode in the transistor 200 (here, the conductive layer 220) is located below and the other of the source electrode and the drain electrode (here, the conductive layer 240) is located above, the transistor 200 has a structure in which current flows in the vertical direction. That is, a channel is formed along the side wall of the opening 290a.

[0082] The oxide semiconductor layer 230 is in contact with the top surface of the conductive layer 220 and the side surface of the conductive layer 240 inside the opening 290. The oxide semiconductor layer 230 is also in contact with a portion of the top surface of the conductive layer 240. In this way, by making the oxide semiconductor layer 230 contact not only the side surface but also the top surface of the conductive layer 240, for example, compared with the case where the oxide semiconductor layer 230 is in contact with the side surface of the conductive layer 240 but not with the top surface, the area in which the oxide semiconductor layer 230 contacts the conductive layer 240 can be increased. Therefore, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced.

[0083] The conductive layer 240 has an opening 290b in a region overlapping with the conductive layer 220. In addition, the conductive layer 240 is preferably not provided inside the opening 290a provided in the insulating layer 280. That is, the conductive layer 240 preferably does not have a region in contact with the side surface of the insulating layer 280 in the opening 290a. By adopting such a structure, the opening 290b provided in the conductive layer 240 and the opening 290a provided in the insulating layer 280 can be formed together. In addition, by adopting a structure in which the side surface of the conductive layer 240 in the opening 290b is consistent or substantially consistent with the side surface of the insulating layer 280 in the opening 290a, the thickness distribution of the oxide semiconductor layer 230 provided inside the opening 290 can be made uniform. In addition, the oxide semiconductor layer 230 can be suppressed from being separated due to the step between the conductive layer 240 and the insulating layer 280.

[0084] The conductive layer 260 preferably has a stacked-layer structure of a conductive layer 260a and a conductive layer 260b on the conductive layer 260a. Alternatively, the conductive layer 260a and the conductive layer 260b may each have a stacked-layer structure.

[0085] The width of the opening 290 is the width D. The width D sometimes varies in the depth direction. For example, it may be the width of the upper end of the opening 290a of the insulating layer 280. Alternatively, it may be the width of the lower end. Alternatively, it may be the width of half the depth of the opening 290a in the insulating layer 280. Alternatively, the width of the opening 290b in the conductive layer 240 may be used.

[0086] The portions of the oxide semiconductor layer 230 and the insulating layer 250 disposed inside the opening 290 reflect the shape of the opening 290. Specifically, the oxide semiconductor layer 230 is disposed so as to cover the bottom and sidewalls of the opening 290, and the insulating layer 250 is disposed so as to cover the oxide semiconductor layer 230. The oxide semiconductor layer 230 is preferably disposed so as to be in contact with the sidewalls of the insulating layer 280 in the opening 290a. In addition, the insulating layer 250 is disposed so as to face the sidewalls of the insulating layer 280 in the opening 290a via the oxide semiconductor layer 230.

[0087] The conductive layer 260 is provided so as to fit into the recess of the insulating layer 250 reflecting the shape of the opening 290. By reducing the width D, the miniaturization of the transistor 200 can be achieved. However, when the width D is reduced, if the aspect ratio of the opening 290 is high, and if the value of the depth of the opening divided by the width of the opening is large, the coverage of the side wall of the opening 290 may be reduced depending on the formation method or thickness of the components arranged inside the opening 290. In addition, when the width D is reduced and the oxide semiconductor layer 230 is made thick, there is a concern that the coverage of the inside of the opening may be further reduced.

[0088] The opening 290 preferably has a tapered shape at the upper end of the opening. In addition, the opening 290 preferably has a region having a tapered shape at the upper end of the opening and a region located deeper than the region and having a side wall steeper than the upper end. Steep here means, for example, that the angle with respect to the side wall of the insulating layer 210 is vertical or nearly vertical.

[0089] By forming the opening 290 in the above-described shape, the size of the transistor 200 can be made finer, and even when the width of the opening is small and the aspect ratio is high, the conductive layer 260 can be formed to have an appropriate shape. Specifically, for example, the conductive layer 260 can be formed at the upper end of the opening 290 so that the conductive layer 260a has high coverage of the side wall of the opening 290 and the conductive layer 260b has a relatively large thickness.

[0090] The film provided inside the opening 290 can be formed by atomic layer deposition (ALD), sputtering, chemical vapor deposition (CVD), vacuum evaporation, pulsed laser deposition (PLD), or the like.

[0091] The upper end of the opening 290 preferably has a tapered shape. At least a portion of the side wall of the tapered region is preferably covered with the conductive layer 260 b.

[0092] The opening 290 preferably has a region where the side wall is steeper than the upper end in a region deeper than the region having the tapered shape. When the opening 290 has such a shape, for example, in the tapered region, the contact area with the conductive layer 240 increases, so the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced. In addition, when a portion of the insulating layer 280 has a tapered shape, for example, the region is sometimes used as a relaxation region of the electric field between the conductive layer 240 and the conductive layer 260.

[0093] exist Figure 2B and Figure 2CIn the transistor 200 shown, in the opening 290 , the sidewalls of the conductive layer 240 and the sidewalls of the insulating layer 280 c include tapered regions, and the sidewalls of the insulating layer 280 b and the sidewalls of the insulating layer 280 a include regions steeper than the sidewalls of the conductive layer 240 .

[0094] The insulating layer 250 preferably has a structure that can well cover the side wall of the opening 290 and suppress a short circuit between the conductive layer 240 and the conductive layer 260 .

[0095] The conductive layer 260 has a region located on the insulating layer 280. Figure 2B and Figure 2C In the embodiment, the conductive layer 260 has regions on the insulating layer 280 that respectively cover the conductive layer 240 , the oxide semiconductor layer 230 , and the insulating layer 250 .

[0096] The conductive layer 240 preferably has an area not covered by the conductive layer 260. In the area not overlapping with the conductive layer 260, the end of the conductive layer 240 is located outside the end of the conductive layer 260. In the area of ​​the conductive layer 240 not overlapping with the conductive layer 260, a conductive layer is provided on the upper layer, and the conductive layer and the conductive layer 240 can be electrically connected.

[0097] Figure 2B The structure is shown in which the end of the conductive layer 240 outside the opening 290 is located outside the end of the conductive layer 260. With this structure, a plug or the like can be provided on the area of ​​the conductive layer 240 extending outside the conductive layer 260, and electrically connected to the conductive layers such as wiring and electrodes located above the conductive layer 240 and the conductive layer 260.

[0098] The insulating layer 250 is provided in contact with the top surface of the oxide semiconductor layer 230. The insulating layer 250 preferably has a region in contact with the top surface of the conductive layer 240, a region in contact with the side surface of the conductive layer 240, and a region in contact with the top surface of the insulating layer 280.

[0099] like Figure 2B and Figure 2C As shown, a portion of the insulating layer 250 is located outside the opening 290, that is, located on the conductive layer 240 and the insulating layer 280. At this time, the insulating layer 250 preferably covers the end of the oxide semiconductor layer 230. Thus, the conductive layer 260 and the oxide semiconductor layer 230 can be prevented from being short-circuited. In addition, the insulating layer 250 preferably covers the end of the conductive layer 240. Thus, the conductive layer 260 and the conductive layer 240 can be prevented from being short-circuited.

[0100] The insulating layer 250 is used as a gate insulating layer of the transistor 200. By thinning the gate insulating layer, it is possible to reduce a gate potential applied when the transistor 200 operates. In addition, the transistor 200 can be operated at a high speed.

[0101] Here, Figure 2B and Figure 2C A structure is shown in which the end of the oxide semiconductor layer 230 is located inside the end of the conductive layer 240 outside the opening 290. Note that the present invention is not limited to this. For example, in the X direction, the end of the oxide semiconductor layer 230 is sometimes consistent with or approximately consistent with the end of the conductive layer 240. Alternatively, the end of the oxide semiconductor layer 230 is sometimes located outside the end of the conductive layer 240. By having the end of the oxide semiconductor layer 230 be located outside the end of the conductive layer 240 and the oxide semiconductor layer 230 covering the end of the conductive layer 240, it is sometimes possible to further improve the withstand voltage between the conductive layer 240 and the conductive layer 260, and further reduce the leakage current flowing through the insulating layer 250 located between the conductive layer 240 and the conductive layer 260.

[0102] By setting the angle formed by the top surface of the insulating layer 210 and the side wall of the opening 290 to be 60 degrees or less, more preferably 50 degrees or less, and further preferably 40 degrees or less, the side wall of the opening 290 can be made to have a tapered shape. In addition, when the angle formed by the top surface of the insulating layer 210 and the side wall of the opening 290 is set to be less than 20 degrees, the width D of the opening 290 increases, and it is sometimes difficult to achieve miniaturization of the transistor 200. Therefore, in the case where the side wall of the opening 290 has a tapered shape, for example, the angle formed by the top surface of the insulating layer 210 and the side wall of the opening 290 can be 20 degrees or more and 75 degrees or less, preferably 20 degrees or more and 70 degrees or less, more preferably 20 degrees or more and 60 degrees or less, and further preferably 20 degrees or more and 50 degrees or less.

[0103] By making the angle formed by the top surface of the insulating layer 210 and the side wall of the opening 290 greater than 60 degrees and less than 90 degrees, preferably greater than 70 degrees and less than 90 degrees, more preferably greater than 75 degrees and less than 90 degrees, and further preferably greater than 80 degrees and less than 90 degrees, the side wall of the opening 290 can have a steep shape, thereby realizing miniaturization or high integration of the semiconductor device.

[0104] Alternatively, for example, the sidewall of the opening 290 may have an inverse tapered shape. In other words, the angle formed by the side surface of the insulating layer 280 and the top surface of the insulating layer 210 in the opening 290 may be greater than 90 degrees.

[0105] For example, the side wall of the opening 290 is preferably provided perpendicular to the top surface of the insulating layer 210 . Figure 3BAngles θ1a, θ1b, θ1c, and θ2 are shown, which are formed by the side surfaces of the insulating layer 280a, the insulating layer 280b, the insulating layer 280c, and the conductive layer 240 in the opening 290 and the top surface of the insulating layer 210. The angles θ1a, θ1b, θ1c, and θ2 are, for example, greater than 20 degrees and less than 90 degrees.

[0106] Figure 3B An example in which the conductive layer 240 and the insulating layer 280c have a tapered shape is shown. Figure 3B The tapered portion is surrounded by a dotted line. Angle θ2 and angle θ1c are each preferably 20 degrees to 75 degrees, more preferably 20 degrees to 70 degrees, further preferably 20 degrees to 60 degrees, and further preferably 20 degrees to 50 degrees.

[0107] Each of the angle θ1b and the angle θ1a is preferably greater than 60 degrees and less than 90 degrees, more preferably greater than 70 degrees and less than 90 degrees, further preferably greater than 75 degrees and less than 90 degrees, and further preferably greater than 80 degrees and less than 90 degrees.

[0108] Here, each of the angle θ1 a , the angle θ1 b , the angle θ1 c , and the angle θ2 is an angle formed with the top surface of the insulating layer 210 , but may be an angle formed with the top surface of the conductive layer 220 .

[0109] In addition, by setting the thickness of the insulating layer 280c to, for example, less than 50 nm, less than 30 nm, preferably less than 20 nm, and more preferably less than 10 nm, even if the insulating layer 280c has a conical shape, the size of the opening 290 will not increase excessively, and the area occupied by the transistor can be reduced, which is preferred.

[0110] Figures 1A to 1C Shown in FIG. 2A to FIG. 2C This is an example in which the angle θ1a, the angle θ1b, the angle θ1c, and the angle θ2 are 90 degrees.

[0111] Figure 3C and Figure 3D Both Figure 3B Deformation example.

[0112] Figure 3C In addition to the conductive layer 240 and the insulating layer 280c, the side wall of the insulating layer 280a in the opening 290 also has a tapered shape. Figure 3C, the portion having a tapered shape is surrounded by a dotted line. The tapered sidewall of the insulating layer 280a in the opening 290 can improve the coverage of the bottom of the opening 290 and the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260a in the vicinity thereof. In addition, by sufficiently thinning the insulating layer 280a, the increase in the size of the transistor 200 can also be suppressed. The insulating layer 280a can be, for example, 50 nm or less, 30 nm or less, preferably 20 nm or less, and more preferably 10 nm or less.

[0113] Figure 3D The conductive layer 240 and the insulating layer 280c have regions with steep sidewalls, and the insulating layer 280b and the insulating layer 280a have tapered regions. In this way, by partially tapering the insulating layer 280, for example, coverage of the components of the transistor 200 can be improved in the opening 290.

[0114] Furthermore, by making the lower end of the side wall of the conductive layer 240 discontinuous with the upper end of the side wall of the insulating layer 280c, a region that is in contact with the top surface of the insulating layer 280 and is located within the opening 290 can be provided in the oxide semiconductor layer 230. This region is sometimes used as, for example, a region for relaxing the electric field between the conductive layer 240 and the conductive layer 260. In addition, for example, the coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250, the conductive layer 260, and the like thereon can be improved.

[0115] Figure 4A is a plan view of a semiconductor device including the transistor 200 . Figure 4B It is along Figure 4A A cross-sectional view along the dashed line A1-A2 is shown. Figure 4C It is along Figure 4A The cross-sectional view of the dotted line A3-A4 is shown. Figure 5A is a diagram illustrating angle θ1a, angle θ1b, angle θ1c, and angle θ2, corresponding to Figure 4B Cross section shown. FIG. 4A to FIG. 4C The semiconductor device shown is FIG. 2A to FIG. 2C The difference is that the lower end of the side wall of the conductive layer 240 is not continuous with the upper end of the side wall of the insulating layer 280c. Note that Figure 4B and Figure 4C The side wall ratios of the insulating layer 280c and the conductive layer 240 in the opening 290 are shown. Figure 2B and Figure 2C Steep examples, but each side wall may also have a tapered shape.

[0116] Figure 5A Show Figure 4BThe angles θ1a, θ1b, θ1c, and θ2 formed by the respective sides of the insulating layers 280a, 280b, 280c, and the conductive layer 240 in the opening 290 with the top surface of the insulating layer 210. In Figure 5A In the example shown, the position of the lower end of the side wall of the conductive layer 240 is shifted outward by a length d1 from the position of the upper end of the side wall of the insulating layer 280c.

[0117] In Figure 5A it is preferable that the angles θ1a, θ1b, θ1c, and θ2 are, for example, greater than 60 degrees and 90 degrees or less, more preferably greater than 70 degrees and 90 degrees or less, still more preferably greater than 75 degrees and 90 degrees or less, and even more preferably 80 degrees or more and 90 degrees or less.

[0118] Figure 5B And Figure 5C both show Figure 5A modified examples.

[0119] Figure 5B Differences from Figure 5A lie in the angles θ2 and θ1c. In Figure 5B a portion having a conical shape is surrounded by a dotted line. In Figure 5B it is preferable that the angles θ2 and θ1c are, for example, 20 degrees or more and 75 degrees or less, more preferably 20 degrees or more and 70 degrees or less, still more preferably 20 degrees or more and 60 degrees or less, and even more preferably 20 degrees or more and 50 degrees or less.

[0120] Figure 5C Differences from Figure 5A lie in the angles θ2, θ1c, and θ1a. In Figure 5C a portion having a conical shape is surrounded by a dotted line. In Figure 5C it is preferable that the angles θ2, θ1c, and θ1a are, for example, 20 degrees or more and 75 degrees or less, more preferably 20 degrees or more and 70 degrees or less, still more preferably 20 degrees or more and 60 degrees or less, and even more preferably 20 degrees or more and 50 degrees or less.

[0121] <OS transistor> In the transistor 200, the oxide semiconductor layer 230 including a channel formation region contains a metal oxide (also referred to as an oxide semiconductor) used as a semiconductor. That is, the transistor 200 can be said to be an OS transistor.

[0122] In an OS transistor, when there are oxygen vacancies (V O) and impurities, the electrical characteristics are easily changed and reliability may be reduced. In addition, hydrogen near the oxygen vacancy forms a defect in which hydrogen enters the oxygen vacancy (hereinafter sometimes referred to as V O H) and may generate electrons that become carriers. Therefore, when the channel formation region in the oxide semiconductor contains oxygen vacancies, the OS transistor tends to have a normally-on characteristic. Therefore, in the channel formation region in the oxide semiconductor, it is preferred to minimize oxygen vacancies and impurities. In other words, it is preferred that the carrier concentration in the channel formation region in the oxide semiconductor is reduced and is i-typed (intrinsic) or substantially i-typed.

[0123] On the other hand, the source region and drain region of the OS transistor are preferably the following regions: O In other words, the source and drain regions of the OS transistor are preferably n-type regions with higher carrier concentration and lower resistance than the channel formation region.

[0124] The region of the oxide semiconductor layer 230 in contact with the insulating layer 280 and its vicinity are used as a channel formation region of the transistor 200. One of the region of the oxide semiconductor layer 230 in contact with the conductive layer 220 and the region of the oxide semiconductor layer 230 in contact with the conductive layer 240 is used as a source region, and the other is used as a drain region. That is, the channel formation region is sandwiched between the source region and the drain region.

[0125] When the oxide semiconductor layer 230 is in contact with the conductive layer 220, a metal compound or oxygen vacancies are formed, and the region of the oxide semiconductor layer 230 in contact with the conductive layer 220 is reduced in resistance. Thus, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 can be reduced. Similarly, when the oxide semiconductor layer 230 is in contact with the conductive layer 240, the region of the oxide semiconductor layer 230 in contact with the conductive layer 240 is reduced in resistance. Thus, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced.

[0126] like Figure 3A As shown, the insulating layer 280 is in contact with the entire edge of the oxide semiconductor layer 230. Therefore, the channel formation region of the transistor 200 may be formed at the entire edge of the oxide semiconductor layer 230 in the opening 290 (the entire region in contact with the insulating layer 280). Figure 3A It can also be said that it is a cross-sectional view along the XY plane including the channel formation region of the oxide semiconductor layer 230 .

[0127] The channel length of the transistor 200 is the distance between the source region and the drain region. In other words, it can be said that the channel length of the transistor 200 is determined by the thickness of the insulating layer 280 on the conductive layer 220. Figure 2C , the dotted double arrow indicates the channel length L of the transistor 200. When viewed from the cross section, the channel length L is the distance between the end of the region where the oxide semiconductor layer 230 and the conductive layer 220 are in contact and the end of the region where the oxide semiconductor layer 230 and the conductive layer 240 are in contact. That is, the channel length L is equivalent to the length of the side surface of the opening 290 side of the insulating layer 280 when viewed from the cross section.

[0128] In a planar transistor, the channel length is limited by the exposure limit of photolithography, and it is difficult to further achieve miniaturization, but in a transistor included in a semiconductor device of one embodiment of the present invention, the channel length can be set according to the thickness of the insulating layer 280. Therefore, the channel length of the transistor 200 can be set to a very fine structure below the exposure limit of photolithography (for example, less than 60nm, less than 50nm, less than 40nm, less than 30nm, less than 20nm or less than 10nm, more than 0.1nm, more than 1nm or more than 5nm). Therefore, the on-state current of the transistor 200 becomes larger, thereby improving the frequency characteristics.

[0129] Since the channel length of the transistor included in the semiconductor device of one embodiment of the present invention depends on the thickness of the insulating layer 280 on the conductive layer 220, for example, when the channel length is set to be greater than 60nm, the area occupied by the transistor, specifically, the area of ​​the transistor when viewed from above, is also roughly determined by the width of the opening 290. As described later, the width D of the opening 290 is preferably greater than 5nm, greater than 10nm, or greater than 20nm and less than 100nm, less than 60nm, less than 50nm, less than 40nm, or less than 30nm. As an example, when the channel length is set to 150nm, the width of the opening 290 can also be less than 150nm. That is, a transistor whose width of the opening is narrower than the channel length can be formed, the area occupied by the transistor can be reduced, and high integration of the semiconductor device can be achieved.

[0130] In addition, by setting the channel length of the transistor to, for example, 1 μm or less, 500 nm or less, or 300 nm or less, productivity and yield can be improved in forming the insulating layer 280 and forming the opening 290 in the insulating layer 280 .

[0131] Therefore, the channel length of the transistor included in the semiconductor device of one embodiment of the present invention is preferably 0.1 nm or more, 1 nm or more, or 5 nm or more and 1 μm or less, 500 nm or less, or 300 nm or less.

[0132] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed in the opening 290. Therefore, compared with a lateral transistor such as a planar transistor in which a channel formation region, a source region, and a drain region are respectively provided on the XY plane, the occupied area of ​​the transistor 200 can be reduced. Thus, high integration of semiconductor devices can be achieved. In addition, when a semiconductor device of one embodiment of the present invention is used in a storage device, the storage capacity per unit area can be increased.

[0133] In addition, if Figure 3A As shown, the oxide semiconductor layer 230, the insulating layer 250 and the conductive layer 260 are arranged in a concentric circle shape. Therefore, the side surface of the conductive layer 260 arranged in the center is opposite to the side surface of the oxide semiconductor layer 230 via the insulating layer 250. In other words, the edge of the oxide semiconductor layer 230 as a whole becomes a channel formation region when viewed from above. At this time, for example, the channel width of the transistor 200 is determined by the length of the edge of the oxide semiconductor layer 230. In other words, the channel width of the transistor 200 is determined by the width of the opening 290 (the diameter when the shape of the opening 290 when viewed from above is circular). Figures 2C to 3A In FIG. 1 , a double-pointed dashed double arrow indicates the width D of the opening 290. Figure 3A In FIG. 1 , a double-pointed arrow indicates a channel width W of the transistor 200 . By increasing the width D of the opening 290 , the channel width per unit area can be increased, thereby increasing the on-state current.

[0134] When the opening 290 is formed by photolithography, the width D of the opening 290 is subject to the exposure limit of the photolithography. In addition, the width D of the opening 290 is set according to the thickness of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 provided in the opening 290. The width D of the opening 290 is preferably 5 nm or more, 10 nm or more, or 20 nm or more and 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. Note that when the opening 290 is circular in a plan view, the width D of the opening 290 is equivalent to the diameter of the opening 290, and the channel width W can be calculated as "D×π".

[0135] In addition, the channel length L of the transistor 200 is preferably at least smaller than the channel width W of the transistor 200. The channel length L of the transistor 200 is preferably greater than 0.1 times and less than 0.99 times, and more preferably greater than 0.5 times and less than 0.8 times, of the channel width W of the transistor 200. By adopting such a structure, a transistor with good electrical characteristics and high reliability can be realized.

[0136] In addition, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are arranged in concentric circles by forming the opening 290 in a circular shape in a plan view. As a result, the distance between the conductive layer 260 and the oxide semiconductor layer 230 is substantially uniform, so that a gate electric field can be applied to the oxide semiconductor layer 230 substantially uniformly.

[0137] Note that, although this embodiment shows an example in which the shape of the opening 290 when viewed from a plane is a circle, the present invention is not limited thereto. For example, the shape of the opening 290 when viewed from a plane may be a substantially circular shape such as an ellipse, a polygonal shape such as a quadrangle, or a shape in which the corners of a polygon such as a quadrangle are curved.

[0138] Fig. 6A enlarge Figure 2B The cross section shown is shown as a portion of the cross section shown. Fig. 6A As shown, a recessed portion overlapping the opening 290 is formed in the conductive layer 220, and at least a part of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 is formed so as to be embedded in the recessed portion. With such a structure, the gate electric field of the conductive layer 260 can be easily applied to the conductive layer 220 near the oxide semiconductor layer 230. The recessed portion of the conductive layer 220 is formed, for example, by overetching when the opening 290 is formed.

[0139] exist Fig. 6A In the embodiment, the opening 290 and the concave portion of the conductive layer 220 constitute a continuous opening. In this case, for example, the bottom of the continuous opening is the top surface of the conductive layer 220.

[0140] Figure 6B An example of a three-layer stacked structure in which the conductive layer 220 has a conductive layer 220a, a conductive layer 220b on the conductive layer 220a, and a conductive layer 220c on the conductive layer 220b is shown. The bottom surface of the recess included in the conductive layer 220 is equivalent to the top surface of the conductive layer 220b, and the side surface of the recess is equivalent to the side surface of the opening 290 of the conductive layer 220c. Here, the shortest distance Tc from the top surface of the insulating layer 210 to the top surface of the conductive layer 220c in contact with the insulating layer 280 is preferably longer than the shortest distance Ta from the top surface of the insulating layer 210 to the top surface of the insulating layer 250. As a result, the contact resistance between the side surface of the conductive layer 220c and the oxide semiconductor layer 230 can be reduced. Therefore, the decrease in the on-state current of the transistor 200 can be suppressed.

[0141] Figure 6C yes Figure 6B An example of a deformation of . Figure 6C In the embodiment, the bottom surface of the recessed portion included in the conductive layer 220 is located above the top surface of the conductive layer 220b. Figure 6CAs shown, the oxide semiconductor layer 230 does not necessarily need to be in contact with the conductive layer 220a or the conductive layer 220b.

[0142] Fig.6D The top surfaces of the oxide semiconductor layer 230 and the conductive layer 220 are shown ( Fig.6D According to the formation conditions of the opening 290, such as Fig.6D As shown, the conductive layer 220 is sometimes not provided with a recess.

[0143] exist Fig.6D In the embodiment, the bottom of the opening 290 is the top surface of the conductive layer 220 .

[0144] Since the conductive layer 220 is in contact with the side surface of the oxide semiconductor layer 230 , the contact area between the conductive layer 220 and the oxide semiconductor layer 230 can be increased, thereby reducing the contact resistance.

[0145] In addition, by having a region where the conductive layer 220 and the conductive layer 260 overlap each other, the electrical characteristics of the transistor can be improved, for example, because the gate electric field is easily applied to the channel formation region of the oxide semiconductor layer 230. Furthermore, the gate electric field is easily applied to the region of the oxide semiconductor layer 230 that is in contact with the conductive layer 220, so that, for example, the on-state current of the transistor can be increased.

[0146] <Semiconductor Device Structure Example 2> The conductive layer 240 may also have a stacked structure of two or more layers. Fig. 7A and Figure 2B The main difference is that the conductive layer 240 has a stacked structure of a conductive layer 240a and a conductive layer 240b on the conductive layer 240a.

[0147] Figure 7B is a diagram illustrating angle θ1a, angle θ1b, angle θ1c, angle θ2a, and angle θ2b, corresponding to Fig. 7A The cross section is shown. In addition, angle θ2a and angle θ2b are angles corresponding to the side walls of the conductive layer 240a and the conductive layer 240b, respectively.

[0148] Note that although Fig. 7A Although the example in which the conductive layer 240 is a stack of two layers is shown, the conductive layer 240 may be a stack of three or more layers. In addition, the conductive layer 260a and the conductive layer 260b may each have a stacked-layer structure.

[0149] exist Figure 7BIn the example shown, the angle θ2b is larger than the angle θ2a. The angle θ2b and the angle θ2a are each preferably greater than 20 degrees and less than 60 degrees, more preferably greater than 20 degrees and less than 50 degrees, and further preferably greater than 20 degrees and less than 40 degrees. By making the angle θ2b greater than the angle θ2a, the tapered shape of the upper end of the opening 290 can be a concave shape, for example, the coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250, the conductive layer 260, etc. thereon can be improved.

[0150] in addition, Fig. 8A and Figure 8B Shown separately Fig. 7A and Figure 7B Deformation example. Fig. 8A An example is shown in which the lower end of the side wall of the conductive layer 240 b is not continuous with the upper end of the side wall of the conductive layer 240 a . Figure 8B is a diagram illustrating angle θ1a, angle θ1b, angle θ1c, angle θ2a, and angle θ2b, corresponding to Fig. 8A The cross section shown. Figure 8B As shown, the position of the lower end of the side wall of the conductive layer 240b on the opening 290 side is moved outward by a length d2 from the position of the upper end of the side wall of the conductive layer 240a on the opening 290 side.

[0151] exist Fig. 8A In the embodiment, the oxide semiconductor layer 230 has a region in contact with the top surface of the conductive layer 240a. Thus, the contact area between the oxide semiconductor layer 230 and the conductive layer 240a can be increased, thereby reducing the contact resistance. Fig. 8A As shown, by forming a step shape at the upper end of the opening 290 by the conductive layer 240a and the conductive layer 240b, for example, the coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250 and the conductive layer 260 thereon can be improved.

[0152] <Semiconductor Device Structure Example 3> Fig.9A and Figure 4B The main difference is that the conductive layer 240 has a stacked structure of a conductive layer 240a and a conductive layer 240b on the conductive layer 240a. Fig.9A In the embodiment, the position of the end of the conductive layer 240b on the side of the opening 290 is moved outward from the position of the end of the conductive layer 240a on the side of the opening 290. Therefore, the conductive layers 240a and 240b have a stepped shape.

[0153] Fig. 9B is a diagram illustrating angle θ1a, angle θ1b, angle θ1c, angle θ2a, and angle θ2b, corresponding to Fig.9AThe cross section shown. In addition, angle θ2a and angle θ2b are angles corresponding to the side walls of conductive layer 240a and conductive layer 240b, respectively. The position of the lower end of the side wall of the opening 290 side of the conductive layer 240b is moved outward by a length d2 from the position of the upper end of the side wall of the opening 290 side of the conductive layer 240a.

[0154] Note that although Fig.9A Although the example in which the conductive layer 240 is a stack of two layers is shown, the conductive layer 240 may be a stack of three or more layers. Fig. 9B Although an example is shown in which the side walls of the insulating layer 280 a , the insulating layer 280 b , the insulating layer 280 c , the conductive layer 240 a , and the conductive layer 240 b are all steep side walls, each side wall may also have a tapered shape.

[0155] <Insulating Layer 283 and Insulating Layer 285> like Fig. 10A As shown in FIG. 2 , in the semiconductor device, an insulating layer 283 on the transistor 200 and an insulating layer 285 on the insulating layer 283 may be provided. Both the insulating layer 283 and the insulating layer 285 are used as interlayer films. The insulating layer 283 is provided so as to cover the conductive layer 260, the insulating layer 280, and the like. Fig. 10A In the illustrated structural example, for example, the insulating layer 283 can be formed using a deposition method that forms a film isotropically with high coverage, and the insulating layer 285 whose top surface is flattened can be formed on the insulating layer 283 .

[0156] <Variation Example of Semiconductor Device> Fig. 10B The semiconductor device shown includes an insulating layer 283 and an insulating layer 285 on the transistor 200, and a conductive layer 265 on the insulating layer 285. The height of the top surface of the conductive layer 260 is preferably the same or substantially the same as the height of the top surface of the insulating layer 285. The conductive layer 265 is disposed on the insulating layer 285, the insulating layer 283, and the conductive layer 260. The conductive layer 260 and the conductive layer 265 are electrically connected to each other. The conductive layer 265 is preferably in contact with the top surface of the conductive layer 260.

[0157] exist Fig. 10B In the semiconductor device shown, the area where conductive layer 260 on insulating layer 280 overlaps with conductive layer 240 is extremely small. In addition, since insulating layer 285 is provided between conductive layer 265 and conductive layer 240, the parasitic capacitance between conductive layer 265 and conductive layer 240 can be reduced by increasing the thickness of insulating layer 285.

[0158] <Structural Materials of Semiconductor Devices> Materials that can be used for the semiconductor device of this embodiment are described below. Note that a layer constituting the semiconductor device of this embodiment may have a single-layer structure or a stacked-layer structure.

[0159] [Insulation layer] As the insulating layer (insulating layer 210, insulating layer 250, insulating layer 280, insulating layer 283, insulating layer 285, etc.) included in the semiconductor device, an inorganic insulating film is preferably used. As the inorganic insulating film, for example, an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film can be cited. As the oxide insulating film, for example, a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, a yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminum oxide film can be cited. As the nitride insulating film, for example, a silicon nitride film and an aluminum nitride film can be cited. As the oxynitride insulating film, for example, an oxynitride silicon film, an oxynitride aluminum film, an oxynitride gallium film, an oxynitride yttrium film, and an oxynitride hafnium film can be cited. As the nitride oxide insulating film, for example, a silicon nitride oxide film and an aluminum nitride oxide film can be cited. Alternatively, an organic insulating film may be used as an insulating layer included in the semiconductor device.

[0160] In addition, by surrounding a transistor using a metal oxide with an insulating layer having a function of suppressing the transmission of impurities and oxygen, the electrical characteristics of the transistor can be stabilized. As an insulating layer having a function of suppressing the transmission of impurities and oxygen, for example, a single layer or a stack of insulating layers containing one or more selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium and tantalum can be used. Specifically, as a material for an insulating layer having a function of suppressing the transmission of impurities and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon oxynitride, and silicon nitride can be used.

[0161] Specifically, it is preferable to use an insulating layer that blocks impurities such as water and hydrogen, and oxygen.

[0162] In this specification, etc., a barrier insulating layer refers to an insulating layer having barrier properties. In addition, barrier properties refer to properties that a corresponding substance does not diffuse easily, properties that a corresponding substance does not permeate easily, properties that a corresponding substance has low permeability, functions to inhibit diffusion of a corresponding substance, or functions to inhibit permeation of a corresponding substance. In addition, hydrogen, which is recorded as a corresponding substance, refers to, for example, hydrogen atoms, hydrogen molecules, water molecules, and OH. - In addition, unless otherwise specified, impurities recorded as corresponding substances refer to impurities in the channel formation region or the semiconductor layer, such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N 2 O, NO, NO 2 In addition, oxygen described as a corresponding substance refers to at least one of an oxygen atom, an oxygen molecule, etc.

[0163] Specifically, as an insulating layer having a function of inhibiting the permeation of impurities such as water and hydrogen and oxygen, for example, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide can be cited. For example, an oxide containing aluminum and hafnium (hafnium aluminate) can be cited. For example, metal nitrides such as aluminum nitride, silicon oxynitride, and silicon nitride can be cited.

[0164] In addition, an insulating layer such as a gate insulating layer in contact with the oxide semiconductor layer or an insulating layer provided near the oxide semiconductor layer preferably has a region containing oxygen (hereinafter sometimes referred to as excess oxygen) released by heating. For example, by making the insulating layer having a region containing excess oxygen contact the oxide semiconductor layer or be located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. As an insulating layer that easily forms a region containing excess oxygen, silicon oxide, silicon oxynitride, or silicon oxide with vacancies can be cited.

[0165] For example, as the miniaturization and high integration of transistors progress, problems such as leakage current sometimes occur due to the thin filming of the gate insulating layer. By using a material with a high relative dielectric constant (high-k) for the gate insulating layer, it is possible to achieve low voltage when the transistor is operating while maintaining the physical thickness. In addition, the equivalent oxide thickness (EOT: Equivalent Oxide Thickness) of the gate insulating layer can be reduced. In addition, by using a material with a high relative dielectric constant for the dielectric layer of the capacitor, an element with a larger capacitance value can be achieved. On the other hand, by using a material with a low relative dielectric constant for an insulating layer used as an interlayer film, the parasitic capacitance generated between wirings can be reduced. Therefore, it is preferable to select the material according to the function of the insulating layer. In addition, a material with a low relative dielectric constant is also a material with a high dielectric strength.

[0166] Examples of materials having a high relative dielectric constant include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.

[0167] As materials with low relative dielectric constant, for example, resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate and acrylic resin can be cited. In addition, as inorganic insulating materials with low relative dielectric constant other than the above, for example, silicon oxide added with fluorine, silicon oxide added with carbon, and silicon oxide added with carbon and nitrogen can be cited. In addition, silicon oxide with holes can be cited. In addition, these silicon oxides can also contain nitrogen.

[0168] For example, inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide can be used for both layers such as gate insulating layers to which materials with high relative dielectric constants are applied and layers such as interlayer films to which materials with low relative dielectric constants are applied. These materials have relatively low relative dielectric constants compared to high-k materials such as hafnium oxide, and therefore are sometimes described as materials with low relative dielectric constants in this specification and the like.

[0169] In addition, a material having ferroelectricity may be used as an insulating layer included in a semiconductor device. Examples of the material having ferroelectricity include hafnium oxide, zirconium oxide, HfZrO X (X is a real number greater than 0) and other metal oxides. In addition, as a material that can have ferroelectricity, a material in which an element J1 (herein, the element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added to hafnium oxide can be cited. Here, the ratio of the number of atoms of hafnium to the number of atoms of element J1 can be appropriately set. For example, the ratio of the number of atoms of hafnium to the number of atoms of element J1 can be set to 1:1 or thereabouts. In addition, as a material that can have ferroelectricity, a material in which an element J2 (herein, the element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added to zirconium oxide can be cited. In addition, the ratio of the number of atoms of zirconium to the number of atoms of element J2 can be appropriately set. For example, the ratio of the number of atoms of zirconium to the number of atoms of element J2 can be set to 1:1 or thereabouts. In addition, as a material that can have ferroelectricity, lead titanate (PbTiO X ), barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), barium titanate and other piezoelectric ceramics with perovskite structure.

[0170] In addition, as a material that can have ferroelectricity, a metal nitride containing an element M1, an element M2 and nitrogen can be cited. Here, the element M1 is one or more selected from aluminum, gallium, indium, etc. In addition, the element M2 is one or more selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. In addition, the atomic number ratio of the element M1 to the element M2 can be appropriately set. In addition, a metal oxide containing the element M1 and nitrogen sometimes has ferroelectricity even if it does not contain the element M2. In addition, as a material that can have ferroelectricity, a material in which the element M3 is added to the above-mentioned metal nitride can be cited. Note that the element M3 is one or more selected from magnesium, calcium, strontium, zinc, cadmium, etc. In addition, the atomic number ratio of the element M1, the element M2 and the element M3 can be appropriately set.

[0171] In addition, as a material that can have ferroelectricity, SrTaO 2 N、BaTaO 2N and other perovskite-type oxynitrides, GaFeO 3 wait.

[0172] Note that the materials described above that can have ferroelectricity include metal oxides and metal nitrides, but are not limited thereto. For example, metal oxynitrides obtained by adding nitrogen to the above metal oxides or metal nitride oxides obtained by adding oxygen to the above metal nitrides may also be used.

[0173] In addition, as a material that can have ferroelectricity, for example, a mixture or compound composed of a plurality of materials selected from the above materials can be used. In addition, the insulating layer 130 can have a stacked structure composed of a plurality of materials selected from the above materials. Note that the crystal structure (properties) of the materials listed above may change not only depending on the deposition conditions but also depending on various processes, and thus in this specification, etc., a material that exhibits ferroelectricity is referred to not only as a ferroelectric but also as a material that can have ferroelectricity.

[0174] Even when the metal oxide containing one or both of hafnium and zirconium is processed into a thin film of several nm, it can have ferroelectricity. In addition, even when the area of ​​the metal oxide containing one or both of hafnium and zirconium is small, it can have ferroelectricity. Therefore, by using the metal oxide containing one or both of hafnium and zirconium, miniaturization of semiconductor devices can be achieved.

[0175] In this specification, etc., a material that can have ferroelectricity formed in a layer is sometimes referred to as a ferroelectric layer. In addition, in this specification, etc., a device including a ferroelectric layer, a metal oxide film, or a metal nitride film is sometimes referred to as a ferroelectric device.

[0176] In addition, ferroelectricity is considered to be exhibited because oxygen or nitrogen of the crystals contained in the ferroelectric layer is displaced by the action of an external electric field. In addition, the exhibiting of ferroelectricity is presumed to depend on the structure of the crystals contained in the ferroelectric layer. Therefore, in order for the insulating layer to exhibit ferroelectricity, the insulating layer 130 needs to contain crystals. In particular, the insulating layer preferably has crystals with an orthorhombic crystal structure, thereby exhibiting ferroelectricity. The crystal structure of the crystals contained in the insulating layer is any one or more selected from the group consisting of an isometric system, a tetragonal system, an orthorhombic system, a monoclinic system, and a hexagonal system. In addition, the insulating layer may also have an amorphous structure. At this time, the insulating layer may also have a composite structure of an amorphous structure and a crystal structure.

[0177] The insulating layer 250 is used as a gate insulating layer of the transistor 200. The insulating layer 250 is preferably made of a material having a high relative dielectric constant.

[0178] The insulating layer 250 preferably has a function of capturing and fixing hydrogen. Thus, the hydrogen concentration of the oxide semiconductor layer 230 (especially, the hydrogen concentration in the channel formation region of the transistor) can be reduced. Therefore, the V O H is used to make the channel formation region i-type or substantially i-type.

[0179] As the material of the insulating layer having the function of capturing or fixing hydrogen, metal oxides such as oxides containing hafnium, oxides containing magnesium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate) can be cited. In addition, these metal oxides can also contain zirconium, for example, oxides containing hafnium and zirconium can be cited. Here, in the metal oxide having an amorphous structure, since a part of the oxygen atoms have dangling bonds, the ability to capture or fix hydrogen is high. Therefore, these metal oxides preferably have an amorphous structure. For example, by making these oxides contain silicon, an amorphous structure can be achieved. For example, it is preferred to use an oxide containing hafnium and silicon (hafnium silicate). In addition, sometimes a part of the metal oxide has one or both of a crystalline region and a grain boundary.

[0180] In addition, the function of capturing or fixing the corresponding substance can also be said to have the property that the corresponding substance is not easy to diffuse. Therefore, the function of capturing or fixing the corresponding substance can also be replaced by barrier properties.

[0181] When the insulating layer 250 has a stacked structure, it is preferable to use a layer having a function of trapping and fixing hydrogen for any layer (hereinafter referred to as the first insulating layer of the insulating layer 250). In addition, when the insulating layer 250 has a stacked structure of two layers, a layer having a function of trapping and fixing hydrogen is used as a layer in contact with the oxide semiconductor layer 230, and when it has a stacked structure of three or more layers, a layer having a function of trapping and fixing hydrogen is used as a layer close to the oxide semiconductor layer 230, whereby hydrogen contained in the oxide semiconductor layer 230 can be more effectively captured or fixed. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced.

[0182] In addition to the first insulating layer, a hydrogen barrier insulating layer is preferably used as the second insulating layer for the insulating layer 250. Examples of the material of the hydrogen barrier insulating layer include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, silicon nitride, and silicon nitride oxide.

[0183] As the first insulating layer of the insulating layer 250, for example, hafnium silicate or the like is preferably used. In addition, the first insulating layer of the insulating layer 250 preferably has an amorphous structure. By adopting an amorphous structure for the first insulating layer of the insulating layer 250, the formation of grain boundaries can be suppressed. By suppressing the formation of grain boundaries, the flatness of the insulating layer can be improved. As a result, the thickness distribution of the insulating layer becomes uniform, and the extremely thin portion can be reduced, so that the withstand voltage of the insulating layer can be improved. In addition, the thickness distribution of the film provided on the insulating layer can be made uniform.

[0184] Furthermore, by suppressing the formation of grain boundaries in the insulating layer, leakage current caused by defect states at the grain boundaries can be reduced, thereby making it possible to use the insulating layer as an insulating film with less leakage current.

[0185] Since hafnium oxide is a material with a high relative dielectric constant, hafnium silicate becomes a material with a high relative dielectric constant according to the silicon content. Therefore, when hafnium silicate is used as a gate insulating layer, the gate potential applied when the transistor is operating can be reduced while maintaining the physical thickness of the gate insulating layer. In addition, the equivalent oxide thickness (EOT) of the gate insulating layer can be reduced.

[0186] Therefore, as the first insulating layer of the insulating layer 250, an oxide containing one or both of aluminum and hafnium is preferably used, an oxide having an amorphous structure and containing one or both of aluminum and hafnium is more preferably used, and aluminum oxide having an amorphous structure is further preferably used.

[0187] Furthermore, by using a hydrogen barrier insulating layer as the second insulating layer of the insulating layer 250, diffusion of impurities contained in the conductive layer 260 into the oxide semiconductor layer 230 can be suppressed. Silicon nitride has a high hydrogen barrier property and is therefore suitable for the insulating layer 250. Here, the second insulating layer is preferably an upper layer of the first insulating layer.

[0188] By adopting the above structure, a semiconductor device having good electrical characteristics can be provided. In addition, a semiconductor device having high reliability can be provided. In addition, a semiconductor device having small variations in the electrical characteristics of the transistor can be provided. In addition, a semiconductor device having large on-state current can be provided.

[0189] Furthermore, the insulating layer 250 may also include an insulating layer having a thermally stable structure such as silicon oxide or silicon oxynitride.

[0190] The insulating layer 250 preferably includes a layer capable of supplying oxygen to the oxide semiconductor layer 230. As the layer capable of supplying oxygen, an oxide can be used. When the insulating layer 250 includes silicon oxide or silicon oxynitride, oxygen can be appropriately supplied from the insulating layer 250 to the oxide semiconductor layer 230.

[0191] In addition, the insulating layer 250 may also include an insulating layer having a thermally stable structure between a pair of insulating layers having a function of capturing and fixing hydrogen.

[0192] Insulating layer 250 preferably includes an oxygen blocking insulating layer. This can suppress oxidation of conductive layer 240 and conductive layer 260. When insulating layer 250 has a stacked structure, the layer in contact with conductive layer 240 and the layer in contact with conductive layer 260 are preferably both oxygen blocking insulating layers.

[0193] The layer in contact with the conductive layer 240 in the insulating layer 250 is preferably less likely to allow oxygen to permeate than the insulating layer 280. When the layer has oxygen barrier properties, it is possible to suppress oxidation of the side surface of the conductive layer 240 and formation of an oxide film on the side surface. Therefore, it is possible to suppress a decrease in the on-state current of the transistor 200 or a decrease in the field effect mobility.

[0194] For example, by using a hydrogen and oxygen blocking insulating layer as the second insulating layer, oxidation of the conductive layer 260 can be suppressed. In addition, diffusion of oxygen included in the oxide semiconductor layer 230 into the conductive layer 260 to form oxygen vacancies in the oxide semiconductor layer 230 can be suppressed.

[0195] Examples of the oxygen blocking insulating layer include oxides containing hafnium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate), magnesium oxide, gallium oxide, gallium zinc oxide, silicon nitride, and silicon oxynitride. In addition, examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).

[0196] An oxide containing hafnium and silicon (hafnium silicate) is an excellent insulating layer that not only functions as an oxygen blocking insulating layer but also easily realizes an amorphous structure as described above and has a function of trapping or fixing hydrogen.

[0197] Silicon nitride is used as an oxygen blocking insulating layer and is also an excellent insulating layer having a high barrier property against hydrogen as described above.

[0198] The insulating layer 250 preferably has a two-layer structure in which a first insulating layer having a function of trapping or fixing hydrogen and a second insulating layer having a hydrogen and oxygen barrier property are stacked in this order from the oxide semiconductor layer 230 side.

[0199] As an example, an oxide containing one or both of aluminum and hafnium may be used as the first insulating layer, and silicon nitride may be used as the second insulating layer.

[0200] As the insulating layer 250, a three-layer structure is preferably adopted in which a third insulating layer containing a material with a relatively low relative dielectric constant, a first insulating layer having a function of capturing or fixing hydrogen, and a second insulating layer having hydrogen and oxygen barrier properties are stacked in sequence from the oxide semiconductor layer 230 side. The material with a relatively low relative dielectric constant contained in the third insulating layer refers to, for example, a material whose relative dielectric constant is lower than that of one or more of the other layers in the stacked structure. Here, silicon oxide or silicon oxynitride can be used as the third insulating layer. The third insulating layer is a layer in contact with the oxide semiconductor layer 230. By using an oxide for the third insulating layer, oxygen can be supplied to the oxide semiconductor layer 230. In addition, by providing a second insulating layer, diffusion of oxygen contained in the third insulating layer to the conductive layer 260 can be suppressed, thereby suppressing oxidation of the conductive layer 260. In addition, the amount of oxygen supplied from the third insulating layer to the oxide semiconductor layer 230 can be suppressed from being reduced.

[0201] As an example, silicon oxide or silicon oxynitride may be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium may be used as the first insulating layer, and silicon nitride may be used as the second insulating layer.

[0202] As the insulating layer 250, a four-layer structure is preferably used in which a fourth insulating layer having oxygen barrier properties, a third insulating layer containing a material with a relatively low relative dielectric constant, a first insulating layer having a function of capturing or fixing hydrogen, and a second insulating layer having hydrogen and oxygen barrier properties are stacked in sequence from the oxide semiconductor layer 230 side. The first insulating layer to the third insulating layer can adopt the same structure as the layers used for the above three-layer structure. The fourth insulating layer is a layer in contact with the oxide semiconductor layer 230. When the fourth insulating layer has oxygen barrier properties, oxygen can be suppressed from being released from the oxide semiconductor layer 230. As the fourth insulating layer, aluminum oxide is preferably used, for example. Since aluminum oxide has the function of capturing or fixing hydrogen, it is suitable for use as the fourth insulating layer in contact with the oxide semiconductor layer 230.

[0203] For example, aluminum oxide may be used as the fourth insulating layer, silicon oxide or silicon oxynitride may be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium may be used as the first insulating layer, and silicon nitride may be used as the second insulating layer.

[0204] In the insulating layer 250, the thickness of the region of the oxide semiconductor layer 230 overlapping with the channel formation region is particularly preferably greater than 0.1 nm and less than 30 nm, preferably greater than 0.1 nm and less than 20 nm, preferably greater than 0.1 nm and less than 10 nm, more preferably greater than 0.1 nm and less than 8.0 nm, and more preferably greater than 0.5 nm and less than 7.0 nm.

[0205] In order to achieve miniaturization of the transistor, the thickness of each layer constituting the insulating layer 250 is preferably thin. The thickness of each layer constituting the insulating layer 250 is, for example, 0.1 nm to 10 nm, 0.1 nm to 5 nm, 0.5 nm to 5 nm, 1 nm to less than 5 nm, or 1 nm to 3 nm. Note that at least a portion of each layer constituting the insulating layer 250 only needs to have a region of the above thickness.

[0206] Typically, the thicknesses of the fourth insulating layer, the third insulating layer, the first insulating layer, and the second insulating layer are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. By adopting such a structure, the transistor can have good electrical characteristics even when it is miniaturized or highly integrated.

[0207] Since the insulating layer 210 is used as an interlayer film, its relative dielectric constant is preferably low. By using a material with a low relative dielectric constant for the interlayer film, the parasitic capacitance generated between wirings can be reduced. Silicon oxide and silicon oxynitride are suitable for the insulating layer 210 because they have thermal stability.

[0208] In addition, the concentration of impurities such as water and hydrogen in the insulating layer 210 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor layer 230 .

[0209] A hydrogen barrier insulating layer is preferably used as the insulating layer 210. When the insulating layer 210 provided outside the oxide semiconductor layer 230 has a hydrogen barrier property, diffusion of hydrogen into the oxide semiconductor layer 230 can be suppressed.

[0210] In addition, examples of the material of the hydrogen barrier insulating layer include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, silicon nitride, and silicon nitride oxide.

[0211] For example, as the insulating layer 210 , a silicon nitride film is preferably used.

[0212] The insulating layer 210 may also have a two-layer stacked structure. For example, as the upper layer of the insulating layer 210, an insulating layer having a function of capturing or fixing hydrogen may be used. Thus, hydrogen in the oxide semiconductor layer 230 diffuses to the upper layer of the insulating layer 210 through the conductive layer 220, and the hydrogen may be captured or fixed. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 may be reduced.

[0213] For example, it is preferable that a silicon nitride film be used as the lower layer of the insulating layer 210 , and an oxide film (hafnium silicate film) containing hafnium and silicon be used as the upper layer.

[0214] A hydrogen barrier insulating layer is preferably used as one or more of the insulating layer 283 and the insulating layer 285. Thus, diffusion of hydrogen from above the insulating layer 283 to the oxide semiconductor layer 230 can be suppressed. Since both the silicon nitride film and the silicon oxynitride film have the characteristics of releasing few impurities (for example, water and hydrogen) from themselves and not easily permeating oxygen and hydrogen, they can be suitably used for the insulating layer 283.

[0215] It is particularly preferable to use silicon nitride deposited by sputtering as one or more of the insulating layer 283 and the insulating layer 285. Since the sputtering method does not require molecules containing hydrogen to be used for the deposition gas, the hydrogen concentration of the insulating layer 283 can be reduced. By depositing the insulating layer 283 by sputtering, high-density silicon nitride can be formed.

[0216] In addition, an insulating layer having a function of capturing or fixing hydrogen may be used as one or more of the insulating layer 283 and the insulating layer 285. By adopting such a structure, it is possible to suppress the diffusion of hydrogen from above the insulating layer 283 and the insulating layer 285 to the oxide semiconductor layer 230, and it is possible to capture or fix hydrogen contained in the oxide semiconductor layer 230. Therefore, the hydrogen concentration of the oxide semiconductor layer 230 can be reduced. As one or more of the insulating layer 283 and the insulating layer 285, hafnium silicate or the like may be used.

[0217] Alternatively, a stacked-layer structure of an insulating layer having a function of trapping or fixing hydrogen and a hydrogen barrier insulating layer may be used as the insulating layer 283. For example, a stacked-layer film of aluminum oxide and silicon nitride on the aluminum oxide may be used as the insulating layer 283.

[0218] In addition, the semiconductor device may not include either the insulating layer 283 or the insulating layer 285 .

[0219] In addition, for example, a material with a low relative dielectric constant can be used for the insulating layer 285. By using a material with a low relative dielectric constant for the interlayer film, parasitic capacitance generated between wirings can be reduced.

[0220] Note that the concentration of impurities such as water and hydrogen in the insulating layer 285 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor layer 230 .

[0221] The insulating layer 280 is preferably the above-mentioned hydrogen barrier insulating layer. The insulating layer 280 is provided so as to surround the oxide semiconductor layer 230. Since the insulating layer 280 provided outside the oxide semiconductor layer 230 has hydrogen barrier properties, it is possible to suppress the diffusion of hydrogen into the oxide semiconductor layer 230. For example, the insulating layer 280 preferably includes a silicon nitride film.

[0222] In addition, silicon nitride has an oxygen barrier property. Therefore, by using silicon nitride for the insulating layer 280 , it is possible to suppress the formation of excessive oxygen vacancies in the oxide semiconductor layer 230 due to oxygen desorption from the oxide semiconductor layer 230 .

[0223] In addition, by using silicon nitride for the insulating layer 280, it is possible to prevent excess oxygen from being supplied to the oxide semiconductor layer 230. Therefore, excess oxygen in the channel formation region of the oxide semiconductor layer 230 can be prevented, so that the reliability of the transistor 200 can be improved.

[0224] In addition, the insulating layer 280 preferably includes the above-mentioned oxide insulating film, oxynitride insulating film, or an insulating layer having a region containing excess oxygen.

[0225] For example, the insulating layer having a region containing excess oxygen can be formed by a sputtering method in an atmosphere containing oxygen. By using a sputtering method that does not require the use of molecules containing hydrogen as a deposition gas, the hydrogen concentration in the insulating layer 280 can be reduced. In this way, by depositing a layer constituting at least a portion of the insulating layer 280, oxygen can be supplied from the insulating layer 280 to the channel formation region of the oxide semiconductor layer 230, and oxygen vacancies and VoH can be reduced.

[0226] In addition, the concentration of impurities such as water and hydrogen in the insulating layer 280 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor layer 230 .

[0227] Note that the thickness of the insulating layer 280 over the conductive layer 220 corresponds to the channel length of the transistor 200 , and therefore the thickness of the insulating layer 280 is appropriately set according to the design value of the channel length of the transistor 200 .

[0228] The insulating layer 280 preferably has a stacked-layer structure including, for example, an insulating layer 280 a , an insulating layer 280 b on the insulating layer 280 a , and an insulating layer 280 c on the insulating layer 280 b .

[0229] The insulating layer 280b is in contact with the channel formation region of the oxide semiconductor layer 230. By using an insulating layer containing oxygen as the insulating layer 280b, oxygen can be supplied to the oxide semiconductor layer 230.

[0230] The insulating layer 280b preferably has a region containing more oxygen than at least one of the insulating layer 280a and the insulating layer 280c. In particular, the insulating layer 280b preferably has a region containing more oxygen than each of the insulating layer 280a and the insulating layer 280c. By increasing the oxygen content of the insulating layer 280b, it is easy to form an i-type region in the oxide semiconductor layer 230 near the insulating layer 280b.

[0231] As the insulating layer 280 b, a film that releases oxygen by heating is more preferably used. Since the insulating layer 280 b releases oxygen by heating during the manufacturing process of the transistor 200, oxygen can be supplied to the oxide semiconductor layer 230. By supplying oxygen from the insulating layer 280 b to the oxide semiconductor layer 230, especially to the channel formation region of the oxide semiconductor layer 230, oxygen vacancies in the oxide semiconductor layer 230 and V O H, a transistor with good electrical characteristics and high reliability can be realized.

[0232] In order to improve the electrical characteristics and reliability of the OS transistor, it is important to optimize the amount of oxygen supplied to the oxide semiconductor while the hydrogen concentration in the oxide semiconductor is sufficiently reduced.

[0233] As an example, the amount of oxygen molecules released from the insulating layer 280b is preferably 1.0×10 14 molecules / cm 2 More than and less than 1.0×10 15 molecules / cm 2 Note that the amount of oxygen molecules released can also be measured by thermal desorption spectroscopy.

[0234] In particular, when the channel length of the transistor 200 is short, oxygen vacancies in the channel formation region and V O H has a particularly large influence on electrical characteristics and reliability. Therefore, by optimizing the amount of oxygen supplied to the oxide semiconductor layer 230 while sufficiently reducing the hydrogen concentration in the oxide semiconductor layer 230, a short channel length transistor having good electrical characteristics and high reliability can be realized.

[0235] The insulating layer 280b is preferably formed by a deposition method such as a sputtering method or a PECVD method. In particular, when the sputtering method is used, hydrogen gas does not need to be used as a deposition gas, thereby achieving a film with a very low hydrogen content. Therefore, the supply of hydrogen to the oxide semiconductor layer 230 can be suppressed to achieve stabilization of the electrical characteristics of the transistor 200.

[0236] In the case of increasing the amount of oxygen supplied to the oxide semiconductor layer 230, for example, it is preferred to perform heat treatment in an oxygen-containing atmosphere or plasma treatment in an oxygen-containing atmosphere after forming the insulating layer 280b. In addition, an oxide film may be deposited on the top surface of the insulating layer 280b by sputtering in an oxygen atmosphere to supply oxygen. Then, the oxide film may also be removed. By performing such treatment, oxygen can be supplied to the insulating layer 280b to increase the amount of oxygen supplied to the oxide semiconductor layer 230.

[0237] In addition, in the oxide semiconductor layer 230, the amount of oxygen supplied to the region in contact with the insulating layer 280a and the region in contact with the insulating layer 280c is small compared to the region in contact with the insulating layer 280b. Therefore, the region in contact with the insulating layer 280a and the region in contact with the insulating layer 280c of the oxide semiconductor layer 230 are sometimes low-resistance. That is, by adjusting the thickness of the insulating layer 280a, the range of the region used as one of the source region and the drain region can be controlled. Similarly, by adjusting the thickness of the insulating layer 280c, the range of the region used as the other of the source region and the drain region can be controlled. In this way, the thickness of the insulating layer 280a and the insulating layer 280c can be appropriately set according to the characteristics required by the transistor.

[0238] In addition, as the insulating layer 280b, it is preferable to use a material with a low relative dielectric constant. This can reduce parasitic capacitance generated between wirings. As the insulating layer 280b, for example, silicon oxide or silicon oxynitride can be used.

[0239] As the insulating layer 280a and the insulating layer 280c, oxygen blocking insulating layers are preferably used. By providing the insulating layer 280a between the insulating layer 280b and the conductive layer 220, the resistance of the conductive layer 220 can be suppressed from increasing due to oxidation of the conductive layer 220. In addition, by providing the insulating layer 280c between the insulating layer 280b and the conductive layer 240, the resistance of the conductive layer 240 can be suppressed from increasing due to oxidation of the conductive layer 240.

[0240] In addition, as the insulating layer 280a, an insulating layer having a function of capturing or fixing hydrogen can also be used. By adopting such a structure, it is possible to suppress the diffusion of hydrogen from below the insulating layer 280a to the oxide semiconductor layer 230, and it is possible to capture or fix the hydrogen contained in the oxide semiconductor layer 230. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced. As the insulating layer 280a, magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon can be used. In addition, for example, as the insulating layer 280a, a stacked film of aluminum oxide and silicon nitride on the aluminum oxide can also be used. Similarly, as the insulating layer 280c, an insulating layer having a function of capturing or fixing hydrogen can also be used.

[0241] For example, silicon nitride may be used for the insulating layer 280a and the insulating layer 280c and silicon oxide may be used for the insulating layer 280b.

[0242] [Conductive layer] As the conductive layer (conductive layer 220, conductive layer 240, conductive layer 260, etc.) included in the semiconductor device, it is preferred to use a metal element selected from tungsten, copper, aluminum, chromium, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., an alloy with the above metal elements as a component, or an alloy combining the above metal elements, etc. As the alloy with the above metal elements as a component, a nitride of the alloy or an oxide of the alloy can also be used. For example, tantalum nitride, titanium nitride, ruthenium nitride, nitride containing molybdenum, nitride containing tungsten, titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. are preferably used. In addition, semiconductors with high conductivity represented by polycrystalline silicon containing impurity elements such as phosphorus and silicides such as nickel silicide can also be used.

[0243] In addition, a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing ruthenium, a nitride containing tantalum and aluminum, or a nitride containing titanium and aluminum, etc., a conductive material containing oxygen, such as ruthenium oxide, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel, and a material containing metal elements such as titanium, tantalum or ruthenium are conductive materials that are not easily oxidized, conductive materials that have the function of inhibiting oxygen diffusion, or materials that absorb oxygen and maintain conductivity, so they are preferred. As a conductive material containing oxygen, indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide added with silicon (also referred to as ITSO), indium zinc oxide (also referred to as IZO (registered trademark)), and indium zinc oxide containing tungsten oxide, etc. can be cited. In this specification, etc., a conductive film deposited using a conductive material containing oxygen is sometimes referred to as an oxide conductive film.

[0244] A conductive material mainly composed of tungsten, copper or aluminum is preferred because of its high conductivity.

[0245] In addition, a plurality of conductive layers formed of the above-mentioned materials may be stacked. For example, a laminated structure in which a material containing the above-mentioned metal element and a conductive material containing oxygen are combined may be used. In addition, a laminated structure in which a material containing the above-mentioned metal element and a conductive material containing nitrogen are combined may be used. In addition, a laminated structure in which a material containing the above-mentioned metal element, a conductive material containing oxygen, and a conductive material containing nitrogen are combined may be used.

[0246] In addition, when a metal oxide is used in the channel formation region of a transistor, a stacked structure of a material containing the above-mentioned metal element and a conductive material containing oxygen is preferably used as a conductive layer used as a gate electrode. In this case, the conductive material containing oxygen is preferably arranged on one side of the channel formation region. By arranging the conductive material containing oxygen on one side of the channel formation region, oxygen separated from the conductive material is easily supplied to the channel formation region.

[0247] As the conductive layer 260, the above-mentioned metal elements, alloys containing the above-mentioned metal elements as components, or alloys combining the above-mentioned metal elements can be used. For example, it is preferable to use a material with high conductivity such as tungsten. In addition, as the conductive layer 260, it is preferable to use a conductive material that is not easily oxidized or a conductive material having a function of inhibiting oxygen diffusion. As the conductive material, as described above, a conductive material containing nitrogen and a conductive material containing oxygen can be cited. Thus, the conductivity of the conductive layer 260 can be suppressed from decreasing.

[0248] The conductive layer 260 preferably uses a conductive material containing a metal element and oxygen contained in the metal oxide forming the channel. In addition, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide added with silicon may be used. In addition, indium gallium zinc oxide containing nitrogen may also be used. By using the above materials, hydrogen contained in the metal oxide forming the channel may be captured in some cases. Alternatively, hydrogen mixed from an external insulating layer or the like may be captured in some cases.

[0249] The thickness of the conductive layer 260 may be, for example, not less than 3 nm and not more than 500 nm. The thickness of the conductive layer 260 may be, for example, not less than the thickness of the insulating layer 250. By increasing the thickness of the conductive layer 260, the resistance of the conductive layer 260 may be reduced.

[0250] In addition, as the conductive layer 260, it is preferable to adopt a two-layer structure of a conductive layer 260a and a conductive layer 260b on the conductive layer 260a.

[0251] By using a conductive material having a function of suppressing diffusion of oxygen as the conductive layer 260 a , for example, release of oxygen from the oxide semiconductor layer 230 can be suppressed, thereby suppressing formation of oxygen vacancies in the oxide semiconductor layer 230 .

[0252] In addition, by using a conductive material that is not easily oxidized as the conductive layer 260 a , a decrease in conductivity due to oxidation of the conductive layer 260 a caused by, for example, release of oxygen from the oxide semiconductor layer 230 or release of oxygen from the insulating layer 250 can be suppressed.

[0253] The material used for the conductive layer 260b preferably has, for example, higher conductivity than the material used for the conductive layer 260a. In addition, by increasing the thickness of the conductive layer 260b, the current flowing through the conductive layer 260b can be further increased.

[0254] By using a deposition method with high coverage as the conductive layer 260 a , the conductive layer 260 a can be appropriately formed along the side wall of the opening 290 .

[0255] The conductive layer 260a can be made of, for example, a conductive material containing nitrogen, a conductive material containing oxygen, or the like. Alternatively, the conductive layer 260a can be made of, for example, a conductive material containing a metal element contained in a metal oxide forming a channel and oxygen.

[0256] As the conductive layer 260a, for example, a conductive material containing the above-mentioned metal element and nitrogen can be used, such as tantalum nitride, titanium nitride, ruthenium nitride, nitride containing molybdenum, nitride containing tungsten, titanium and aluminum, nitride containing tantalum and aluminum, etc.

[0257] In addition, as the conductive layer 260a, for example, a conductive material containing the above-mentioned metal element and oxygen can be used, for example, ruthenium oxide, an oxide containing strontium and ruthenium, an oxide containing lanthanum and nickel, or the like can be used.

[0258] In addition, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide added with silicon may also be used. In addition, indium gallium zinc oxide containing nitrogen may also be used.

[0259] As the conductive layer 260a, titanium, tantalum, ruthenium and a material containing one or more of these metal elements are preferred because they are conductive materials that are not easily oxidized, conductive materials that have the function of suppressing oxygen diffusion, or materials that can maintain conductivity even when absorbing oxygen.

[0260] As the conductive layer 260b, for example, the above-mentioned metal elements, alloys containing the above-mentioned metal elements as components, or alloys combining the above-mentioned metal elements can be used. For example, tungsten can be used.

[0261] In addition, the conductive layer 260a may also have a laminated structure. In addition, the conductive layer 260b may also have a laminated structure. In the case where the conductive layer 260a has a laminated structure, for example, multiple materials that can be used for the conductive layer 260a can be laminated. Alternatively, multiple materials selected from the materials of the conductive layer that can be used in one embodiment of the present invention can be laminated. In the case where the conductive layer 260b has a laminated structure, for example, multiple materials that can be used as the conductive layer 260b can be laminated. Alternatively, multiple materials selected from the materials of the conductive layer that can be used in one embodiment of the present invention can be laminated.

[0262] The conductive layer 220 and the conductive layer 240 are conductive layers in contact with the oxide semiconductor layer 230, so it is preferable to use a conductive material that is not easily oxidized, a conductive material that maintains low resistance even if oxidized, an oxide conductive material, or a conductive material having a function of inhibiting oxygen diffusion. Examples of the conductive material include a conductive material containing nitrogen and a conductive material containing oxygen. Thus, a decrease in the conductivity of the conductive layer 220 and the conductive layer 240 can be suppressed.

[0263] By using a conductive material containing oxygen as the conductive layer 220 or the conductive layer 240, conductivity can be maintained even if the conductive layer 220 or the conductive layer 240 absorbs oxygen. In addition, when an insulator containing oxygen such as hafnium oxide is used as the insulating layer 210, the conductive layer 220 can also maintain conductivity, which is preferred. As the conductive layer 220 and the conductive layer 240, for example, ITO, ITSO, IZO (registered trademark), etc. are preferably used.

[0264] In the case where the conductive layer 220 adopts a three-layer structure in which a first conductive layer (e.g., conductive layer 220a), a second conductive layer (e.g., conductive layer 220b), and a third conductive layer (e.g., conductive layer 220c) are sequentially stacked on the insulating layer 210, it is preferred, for example, to use a conductive material that is not oxidized or a conductive material having a function of inhibiting oxygen diffusion as the first conductive layer, a material with high conductivity as the second conductive layer, and a conductive material containing oxygen as the third conductive layer. Specifically, for example, it is preferred to use titanium nitride as the first conductive layer, tungsten as the second conductive layer, and ITO or ITSO as the third conductive layer. In this case, titanium nitride is in contact with the insulating layer 210, and ITO or ITSO is in contact with the oxide semiconductor layer 230. By adopting such a structure, conductivity can be maintained even if the conductive layer 220 is in contact with the oxide semiconductor layer 230. In addition, in the case where an oxide insulating layer is used as the insulating layer 210, excessive oxidation of the conductive layer 220 due to the insulating layer 210 can be suppressed. Furthermore, by using tungsten having high conductivity as the second conductive layer, the conductivity of the conductive layer 220 can be improved.

[0265] In addition, in the case where the conductive layer 240 has a two-layer stacked structure (for example, a conductive layer 240a and a conductive layer 240b), for example, it is preferred to use a material whose conductivity is higher than that of the upper layer as the lower layer, and to use a conductive material containing oxygen as the upper layer. Specifically, for example, it is preferred to use ruthenium, tungsten, titanium nitride, or tantalum nitride as the lower layer, and to use ITO or ITSO as the upper layer. In this case, ITO or ITSO is in contact with the oxide semiconductor layer 230. By adopting such a structure, conductivity can be maintained even if the conductive layer 240 is in contact with the oxide semiconductor layer 230. In addition, by using a material whose conductivity is higher than that of the upper layer as the lower layer, the conductivity of the conductive layer 240 can be improved.

[0266] In the case where the conductive layer 240 has a two-layer stacked structure, a material having high conductivity may be used as the upper layer (e.g., the conductive layer 240b), and a conductive material containing oxygen may be used as the lower layer (e.g., the conductive layer 240a). In this case, for example, by adopting a structure in which the top surfaces of the oxide semiconductor layer 230 and the conductive layer 240a are in contact, the contact resistance between the conductive layer 240 and the oxide semiconductor layer 230 can be reduced.

[0267] [Oxide semiconductor layer 230] As described above, the oxide semiconductor layer 230 has a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The oxide semiconductor layer 230 also has a source region and a drain region. The source region and the drain region are n-type regions (low resistance regions) having a higher carrier concentration than the channel formation region.

[0268] There is no particular limitation on the crystallinity of the semiconductor material used for the oxide semiconductor layer 230, and an amorphous semiconductor, a single crystal semiconductor, or a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part thereof) can be used. When a single crystal semiconductor or a crystalline semiconductor is used, it is preferred because it can suppress degradation of transistor characteristics.

[0269] The band gap of the metal oxide used as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide with a wider band gap, the off-state current of the transistor can be reduced. The off-state current of the OS transistor is small, so the power consumption of the semiconductor device can be fully reduced. In addition, the frequency characteristics of the OS transistor are high, so the semiconductor device can be operated at high speed.

[0270] The off-state current of the OS transistor can be less than 100zA per channel width of 1μm (z: flat, 10 -21 ), 50zA or less, 10zA or less, 1zA or less, 100yA or less (y: one, 10 -24) or 10yA or less. For example, the off-state current of the OS transistor used in the semiconductor device of one embodiment of the present invention is preferably 50zA or less, 10zA or less, 1zA or less, 100yA or less, or 10yA or less.

[0271] The temperature dependence of the off-state current can be obtained by measuring the off-state current at multiple temperatures and extrapolating it using the Arrhenius curve. The off-state current of the OS transistor used in the semiconductor device of one embodiment of the present invention is preferably 1aA (a: A, 10 -18 ) or less, more preferably 100zA or less, and further preferably 10zA or less. Furthermore, at 27°C, it is preferably 1zA or less, more preferably 100yA or less, and further preferably 10yA or less.

[0272] As metal oxides that can be used for the oxide semiconductor layer 230, for example, indium oxide, gallium oxide, and zinc oxide can be cited. The metal oxide preferably contains at least indium (In) or zinc (Zn). In addition, the metal oxide preferably contains two or three selected from indium, element M, and zinc. Note that element M is a metal element or a semi-metal element having a high bonding energy with oxygen, for example, a metal element or a semi-metal element having a higher bonding energy with oxygen than indium. Specifically, as element M, aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony can be cited. The element M contained in the metal oxide is preferably any one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and further preferably gallium. Note that in this specification, etc., metal elements and semi-metal elements are sometimes collectively referred to as "metal elements", and the "metal elements" recorded in this specification, etc. sometimes include semi-metal elements.

[0273] The oxide semiconductor layer 230 may be made of, for example, indium oxide (In oxide), indium zinc oxide (In-Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In-Sn oxide), indium titanium oxide (In-Ti oxide), indium gallium oxide (In-Ga oxide), indium gallium aluminum oxide (In-Ga-Al oxide), indium gallium tin oxide (In-Ga-Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga-Zn oxide, also referred to as GZO), aluminum zinc oxide (Al-Zn oxide, also referred to as Indium tin zinc oxide (In-Al-Zn oxide, also recorded as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also recorded as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also recorded as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also recorded as IGZTO), indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also recorded as IGAZO, IGZAO or IAGZO), etc. Alternatively, indium tin oxide, gallium tin oxide (Ga-Sn oxide), aluminum tin oxide (Al-Sn oxide) and the like containing silicon can be used. Alternatively, the above-mentioned oxides having an amorphous structure can be used. For example, indium oxide having an amorphous structure or indium tin oxide having an amorphous structure can be used.

[0274] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements in the metal oxide, the field effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.

[0275] Note that the metal oxide may also replace indium or contain one or more metal elements with a large periodic number in the periodic table in addition to indium. There is a tendency that the greater the orbital overlap of the metal element, the greater the carrier conduction in the metal oxide. Therefore, by including a metal element with a large periodic number in the periodic table, the field effect mobility of the transistor can sometimes be improved. As metal elements with a large periodic number in the periodic table, metal elements belonging to the 5th period and metal elements belonging to the 6th period can be cited. As the metal element, specifically, yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium and europium can be cited. Note that lanthanum, cerium, praseodymium, neodymium, promethium, samarium and europium are called light rare earth elements.

[0276] The metal oxide may also contain one or more non-metallic elements. When the metal oxide contains non-metallic elements, the field effect mobility of the transistor may be improved by increasing the carrier concentration or narrowing the band gap. Examples of non-metallic elements include carbon, nitrogen, phosphine, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.

[0277] In addition, by increasing the ratio of the number of zinc atoms to the total number of atoms of all metal elements in the metal oxide, the crystallinity of the metal oxide is improved, thereby suppressing the diffusion of impurities in the metal oxide. Therefore, the variation of the electrical characteristics of the transistor is suppressed, thereby improving the reliability.

[0278] In addition, by increasing the ratio of the number of atoms of the element M to the sum of the number of atoms of all metal elements in the metal oxide, a metal oxide with a wider band gap can be obtained. In addition, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, the generation of carriers caused by oxygen vacancies is suppressed, and a transistor with a small off-state current can be realized. In addition, the drift of the threshold voltage of the transistor can be suppressed. In addition, the variation of the electrical characteristics of the transistor is suppressed, so that the reliability can be improved.

[0279] The electrical characteristics and reliability of the transistor vary depending on the composition of the metal oxide used for the oxide semiconductor layer 230. Therefore, by varying the composition of the metal oxide according to the electrical characteristics and reliability required for the transistor, a semiconductor device having both excellent electrical characteristics and high reliability can be realized.

[0280] When the metal oxide is an In-M-Zn oxide, the atomic number ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic number ratio of M. As examples of the atomic number ratio of metal elements in such In-M-Zn oxides, In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5 and compositions nearby. In addition, the composition in the vicinity includes a range of ±30% of the desired atomic number ratio. By increasing the atomic number ratio of indium in the metal oxide, the on-state current and field effect mobility of the transistor can be improved.

[0281] By using a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition thereof as a metal oxide, the transistor can also be made into a normally-off transistor. In addition, when the metal oxide is deposited by sputtering, zinc is sometimes reduced in the deposited metal oxide. Therefore, for example, the composition of the target material is preferably In:M:Zn=1:1:1.2 [atomic ratio] or a composition thereof. On the other hand, when deposition is performed by the ALD method, In is sometimes reduced in the deposited metal oxide.

[0282] The atomic number ratio of In in the In-M-Zn oxide may be smaller than the atomic number ratio of M. Examples of atomic number ratios of metal elements in such an In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions near these. By increasing the atomic number ratio of M in the metal oxide, the generation of oxygen vacancies can be suppressed.

[0283] Note that when a plurality of metal elements are included as the element M, the total of the ratios of the number of atoms of the metal elements may be the ratio of the number of atoms of the element M.

[0284] In this specification, etc., the ratio of the number of indium atoms to the total number of atoms of all metal elements contained may be described as the indium content. The same applies to other metal elements.

[0285] In addition, when the metal oxide is an In-Zn oxide, examples of the atomic number ratio of the metal element of the In-Zn oxide include In:Zn=1:1, In:Zn=2:1, In:Zn=4:1, and compositions near these. In-Zn oxide may also contain a trace amount of element M. For example, when Sn is included as the element M, examples of the atomic number ratio of the metal element of the metal oxide include In:Sn:Zn=2:0.1:1, In:Sn:Zn=4:0.1:1, and compositions near these.

[0286] As an analysis of the composition of the metal oxide used for the oxide semiconductor layer 230, for example, energy dispersive X-ray analysis (EDX: Energy Dispersive X-ray Spectrometry), X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectrometry), inductively coupled plasma mass spectrometry (ICP-MS: Inductively Coupled Plasma-Mass Spectrometry) or inductively coupled plasma atomic emission spectrometry (ICP-AES: Inductively Coupled Plasma-Atomic Emission Spectrometry) can be used. Alternatively, a plurality of the above methods can be combined for analysis. Note that elements with low contents are sometimes affected by the accuracy of analysis, and the actual contents are different from the contents obtained by analysis. For example, when the content of element M is low, the content of element M obtained by analysis is sometimes lower than the actual content. In addition, it is sometimes difficult to quantify element M or element M cannot be detected.

[0287] The metal oxide can be formed by sputtering or ALD as appropriate. Note that when the metal oxide is formed by sputtering, the composition of the deposited metal oxide is sometimes different from the composition of the target. In particular, the zinc content in the deposited metal oxide is sometimes reduced to about 50% of the zinc content in the target. In addition, when depositing the metal oxide, chemical vapor deposition (CVD: Chemical Vapor Deposition) method, molecular beam epitaxy (MBE) method, pulsed laser deposition (PLD: Pulsed Laser Deposition) method, etc. can also be used.

[0288] The oxide semiconductor layer 230 may also have a stacked structure including two or more metal oxide layers. The compositions of the two or more metal oxide layers included in the oxide semiconductor layer 230 may also be the same or substantially the same as each other. By adopting a stacked structure of metal oxide layers with the same composition, for example, the same sputtering target can be used to form the structure, thereby reducing manufacturing costs.

[0289] The compositions of the two or more metal oxide layers included in the oxide semiconductor layer 230 may be different from each other.

[0290] The oxide semiconductor layer 230 may have a two-layer structure, for example. Hereinafter, the first layer is referred to as an oxide layer 230a, and the second layer is referred to as an oxide layer 230b. Note that the oxide layer 230a and the oxide layer 230b are not shown here. In addition, the oxide layer 230a is, for example, a layer close to the side wall of the conductive layer 220 and the opening 290, and the oxide layer 230b is, for example, a layer close to the side of the insulating layer 250. Alternatively, the configuration of the oxide layer 230a and the oxide layer 230b is not limited thereto.

[0291] For example, the oxide layer 230a preferably uses a material having a higher conductivity than the oxide layer 230b. By using a material having a higher conductivity for the oxide layer 230a in contact with the source electrode and the drain electrode (the conductive layer 220 and the conductive layer 240), the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, thereby realizing a transistor having a large on-state current.

[0292] Here, when a material with high conductivity is used for the oxide layer 230b provided on one side of the conductive layer 260 used as the gate electrode, the threshold voltage of the transistor 200 is sometimes caused to drift, so that the drain current (hereinafter also recorded as the cut-off current) flowing when the gate voltage is 0V becomes larger. Specifically, when the transistor 200 is an n-channel transistor, the threshold voltage is sometimes reduced. Therefore, the oxide layer 230b preferably uses a material with low conductivity compared to the oxide layer 230a. Thus, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and a transistor with a small cut-off current can be realized. Note that sometimes the state with a small cut-off current is recorded as normally closed.

[0293] By making the oxide semiconductor layer 230 have a stacked structure and using a material having a higher conductivity than the oxide layer 230b for the oxide layer 230a, a normally-off transistor with a large on-state current can be realized. Thus, a semiconductor device having both low power consumption and high performance can be realized.

[0294] In addition, the carrier concentration of the oxide layer 230a is preferably higher than the carrier concentration of the oxide layer 230b. By increasing the carrier concentration of the oxide layer 230a, the conductivity becomes higher, and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, thereby realizing a transistor with a large on-state current. In addition, by reducing the carrier concentration of the oxide layer 230b, the conductivity becomes lower, thereby realizing a normally-off transistor.

[0295] Note that the oxide semiconductor layer 230 is not limited to the above structure, and the oxide layer 230a may be made of a material having lower conductivity than the oxide layer 230b. In addition, the carrier concentration of the oxide layer 230a may be lower than that of the oxide layer 230b.

[0296] In addition, the band gap of the first metal oxide used in the oxide layer 230a is preferably different from the band gap of the second metal oxide used in the oxide layer 230b. For example, the difference between the band gap of the first metal oxide and the band gap of the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and further preferably 0.3 eV or more.

[0297] The band gap of the first metal oxide used for the oxide layer 230a is preferably smaller than the band gap of the second metal oxide used for the oxide layer 230b. Thus, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, thereby realizing a transistor with a large on-state current. In addition, in the case where the transistor 200 is an n-channel transistor, the threshold voltage can be increased, thereby realizing a normally closed transistor. In addition, since the band gap of the second metal oxide is large, it is possible to suppress the generation and induction of carriers in the oxide layer 230b and at the interface between the oxide layer 230b and the insulating layer 250. Thus, the reliability of the transistor can be improved.

[0298] For example, the content of the element M of the first metal oxide is preferably lower than the content of the element M of the second metal oxide. More specifically, for example, it is preferred that a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto is used as the oxide layer 230a, and a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition close thereto is used as the oxide layer 230b. In this case, it is particularly preferred to use one or more of gallium, aluminum, and tin as the element M.

[0299] Note that the oxide semiconductor layer 230 is not limited to the above structure, and the band gap of the first metal oxide may be larger than the band gap of the second metal oxide.

[0300] In addition, the content of the element M of the first metal oxide is preferably lower than the content of the element M of the second metal oxide. The first metal oxide may also contain a trace amount of the element M or no element M. For example, the first metal oxide used for the oxide layer 230a is preferably In-Zn oxide, and the second metal oxide used for the oxide layer 230b is preferably In-M-Zn oxide. Specifically, the first metal oxide may be In-Zn oxide, and the second metal oxide may be In-Ga-Zn oxide.

[0301] For example, as the oxide layer 230a, it is preferable to use a metal oxide having a composition of In:Zn=1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=2:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=2:0.1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=4:1 [atomic ratio] or a composition close thereto, a metal oxide or indium oxide having a composition close thereto. In addition, as the oxide layer 230b, it is preferable to use a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Ga:Zn=1:3:2 [atomic ratio] or a metal oxide having a composition close thereto, or a metal oxide having a composition close thereto of In:Ga:Zn=1:3:4 [atomic ratio] or a composition close thereto. Thus, the on-state current of the transistor 200 can be increased, and thus a transistor structure with less unevenness and high reliability can be realized.

[0302] The oxide semiconductor layer 230 is not limited to the above structure, and the content of the element M in the first metal oxide may be higher than the content of the element M in the second metal oxide.

[0303] Alternatively, by using metal oxides having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto as the oxide layers 230 a and 230 b , the transistor can be made a normally-off transistor.

[0304] There is no particular limitation on the crystallinity of the semiconductor material used for the oxide semiconductor layer 230, and an amorphous semiconductor (a semiconductor having an amorphous structure), a single crystal semiconductor (a semiconductor having a single crystal structure), or a semiconductor having crystallinity other than a single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part thereof) can be used. When a single crystal semiconductor or a crystalline semiconductor is used, it is preferred because degradation of transistor characteristics can be suppressed.

[0305] The oxide semiconductor layer 230 preferably includes a crystalline metal oxide layer. As the structure of the crystalline metal oxide, for example, a CAAC (c-axis aligned crystal) structure, a polycrystalline (Poly-crystal) structure, and a microcrystalline (nc: nano-crystal) structure can be cited. By using a crystalline metal oxide layer for the oxide semiconductor layer 230, the defect state density in the oxide semiconductor layer 230 can be reduced, thereby realizing a semiconductor device with high reliability. Note that the CAAC structure is a crystal structure in which a plurality of microcrystals (typically, a plurality of microcrystals of IGZO) have a c-axis orientation and are connected on the ab plane in a manner in which the plurality of microcrystals are not oriented. In addition, by observing the cross-section of the OS film having the CAAC structure using a high-resolution TEM image, it can be confirmed that the metal atoms are arranged in layers in the crystal part. Therefore, the OS film having the CAAC structure can also be said to have a structure having a layered crystal part.

[0306] The polycrystalline structure has grain boundaries. In addition, when heat treatment is performed after the oxide semiconductor layer having a polycrystalline structure is formed, a tiny gap (also called nanocrack or microcrack) or a tiny space (also called nanospace or microspace) may be formed between the crystalline parts. When a tiny gap or a tiny space is formed in the oxide semiconductor layer, the resistance of the oxide semiconductor layer becomes higher. This is because the resistance of the tiny gap or the tiny space is very high, for example, infinite. When an oxide semiconductor layer having a tiny gap or a tiny space is used in the channel formation region of a transistor, the contact resistance between the oxide semiconductor layer and one or both of the source electrode and the drain electrode becomes higher. Therefore, this will have an adverse effect on the initial characteristics or reliability of the transistor. The CAAC structure has fewer grain boundaries on the ab plane than the polycrystalline structure, so a semiconductor device with high reliability can be achieved.

[0307] The higher the crystallinity of the metal oxide layer used for the oxide semiconductor layer 230, the lower the defect state density in the oxide semiconductor layer 230. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.

[0308] The higher the substrate temperature (stage temperature) when forming the metal oxide layer, the more crystalline the metal oxide layer can be formed. In addition, the higher the flow rate ratio of the oxygen gas relative to the entire deposition gas used during formation (hereinafter also referred to as the oxygen flow rate ratio) is, the more crystalline the metal oxide layer can be formed.

[0309] The crystallinity of the oxide semiconductor layer 230 can be analyzed, for example, by X-ray diffraction (XRD), transmission electron microscope (TEM), or electron diffraction (ED), or a combination of a plurality of the above methods.

[0310] The oxide semiconductor layer 230 may have a stacked structure of two or more metal oxide layers having different crystallinity. In this case, the compositions of the two or more metal oxide layers may also be different, the same, or substantially the same. For example, a stacked structure may be provided with a first metal oxide layer and a second metal oxide layer disposed on the first metal oxide layer, and the second metal oxide layer may have a region having a higher crystallinity than the first metal oxide layer. Alternatively, the second metal oxide layer may have a region having a lower crystallinity than the first metal oxide layer. In addition, when the second metal oxide layer has a region having a lower crystallinity than the first metal oxide layer, a heat treatment (also referred to as a crystallization treatment) may be performed after the second metal oxide layer is formed to improve the crystallinity of the second metal oxide layer.

[0311] For example, as the oxide layer 230a, a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition thereof, or a metal oxide having a composition of In:M:Zn=1:3:4 [atomic ratio] or a composition thereof is preferably used, and as the oxide layer 230b, a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition thereof is preferably used. By using a metal oxide having a large ratio of Zn to In as the oxide layer 230a, the crystallinity of the oxide layer 230a can be improved. Furthermore, by forming the oxide layer 230b on the oxide layer 230a having high crystallinity, it is easy to improve the crystallinity of the oxide layer 230b. Thus, the crystallinity of the entire oxide semiconductor layer 230 can be improved, so it is preferred. At this time, gallium, aluminum, or tin is particularly preferably used as the element M. For example, two IGZOs having different compositions can also be stacked. For example, a stacked-layer structure of any one selected from indium oxide, indium gallium oxide, and IGZO and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.

[0312] Alternatively, the oxide semiconductor layer 230 may have a stacked structure of three or more layers. For example, the oxide semiconductor layer 230 may have a three-layer structure including an oxide layer, an oxide layer 230 a on the oxide layer, and an oxide layer 230 b on the oxide layer 230 a.

[0313] The oxide layer 230a and the oxide layer 230b may have the above-mentioned structure. The oxide layer under the oxide layer 230a may have the same structure as that of the oxide layer 230b. The following description will be made as a pair of oxide layers sandwiching the oxide layer 230a.

[0314] For example, as the oxide layer 230a, it is preferable to use a metal oxide having a composition of In:Zn=1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=2:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=2:0.1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=4:1 [atomic ratio] or a composition close thereto, a metal oxide or indium oxide having a composition close thereto. In addition, as a pair of oxide layers sandwiching the oxide layer 230a, it is preferable to use a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Ga:Zn=1:3:2 [atomic ratio] or a metal oxide having a composition close thereto, or a metal oxide having a composition of In:Ga:Zn=1:3:4 [atomic ratio] or a composition close thereto.

[0315] The band gap of a pair of oxide layers that clamp the oxide layer 230a is preferably greater than the band gap of the oxide layer 230a. Thus, the oxide layer 230a is clamped by the pair of oxide layers with a large band gap, and the oxide layer 230a is mainly used as a current path (channel). By using the pair of oxide layers to clamp the oxide layer 230a, the trap energy level at the interface of the oxide layer 230a and its vicinity can be reduced. Thus, an embedded channel transistor with a channel away from the insulating layer interface can be realized, thereby improving the field effect mobility. In addition, the influence of the interface state that can be formed on the back channel side can be reduced to suppress the light degradation of the transistor (for example, light negative bias degradation), thereby improving the reliability of the transistor.

[0316] The thickness of the oxide semiconductor layer 230 is preferably 3 nm or more and 200 nm or less, preferably 3 nm or more and 100 nm or less, more preferably 5 nm or more and 100 nm or less, more preferably 10 nm or more and 100 nm or less, more preferably 10 nm or more and 70 nm or less, more preferably 15 nm or more and 70 nm or less, more preferably 15 nm or more and 50 nm or less, more preferably 20 nm or more and 50 nm or less. In addition, in a transistor used for a more miniaturized semiconductor device, the thickness of the oxide semiconductor layer 230 is preferably 1 nm or more, 3 nm or more, or 5 nm or more and 20 nm or less, 15 nm or less, 12 nm or less, or 10 nm or less.

[0317] In addition, when depositing an oxide semiconductor layer, it is preferred to use two deposition methods of sputtering and ALD. For example, after forming a first oxide semiconductor layer of a CAAC structure by sputtering, when forming a second oxide semiconductor layer whose crystallinity is lower than that of the CAAC structure by ALD, it is expected that the atomic layer of the second oxide semiconductor layer fills or repairs the voids in the atomic-level crystalline part of the CAAC structure of the first oxide semiconductor layer. In addition, it is preferred to perform heat treatment (for example, above 100°C and below 500°C, preferably above 200°C and below 450°C, more preferably above 300°C and below 400°C) after forming the second oxide semiconductor layer by ALD. Through this heat treatment, it can be expected that the second oxide semiconductor layer (in other words, each crystalline molecule formed by the ALD method) repairs the voids in the atomic-level crystalline part of the CAAC structure of the first oxide semiconductor layer. In addition, the oxide semiconductor layer formed by the above two deposition methods can also be referred to as Hybrid OS.

[0318] Here, refer to Fig.11A , Fig. 11B , Fig. 11C and Fig.11D The concept of heat treatment for improving the crystallinity of the oxide semiconductor layer will be described. Fig.11A , Fig. 11B , Fig. 11C and Fig.11D Schematic diagrams illustrating a cross section of an oxide semiconductor layer having a CAAC structure. In each figure, the c-axis is indicated by an arrow.

[0319] Fig.11A The oxide semiconductor layer 370a shown includes a region 372a and a region 372b located between the regions 372a. The region 372a corresponds to a region of the CAAC structure (i.e., a structure having a layered crystal portion), and the region 372b corresponds to a region between the CAAC structures. The CAAC structure has fewer grain boundaries on the ab plane than the polycrystalline structure. Thus, in the oxide semiconductor layer 370a having the CAAC structure, there are sometimes small gaps or small spaces between the crystal portions ( Fig.11A area 372b).

[0320] Therefore, in order to improve the crystallinity of the oxide semiconductor layer, in other words, to reduce Fig.11A In the region 372b shown, an oxide semiconductor layer having a CAAC structure is formed as a first oxide semiconductor layer by a sputtering method, and then an oxide semiconductor layer having a microcrystalline structure or an amorphous structure whose crystallinity is lower than that of the CAAC structure is formed as a second oxide semiconductor layer by an ALD method.

[0321] More specifically, if Fig. 11BAs shown, as the first oxide semiconductor layer, an oxide semiconductor layer including the region 372a is formed by a sputtering method, and then as the second oxide semiconductor layer, an oxide semiconductor layer including the region 372c having lower crystallinity than the CAAC structure is formed by an ALD method. Fig. 11B In FIG. 3 , the oxide semiconductor layer 370 b includes a region 372 a and a region 372 c. Since the ALD method can deposit atoms of each layer, the second oxide semiconductor layer can be formed in a manner that fills the region 372 b.

[0322] Then, by performing a heat treatment, the crystallinity of the region 372c included in the second oxide semiconductor layer is improved using the region 372a included in the first oxide semiconductor layer as a seed. In other words, the region 372c included in the second oxide semiconductor layer can be crystal-grown using the region 372a included in the first oxide semiconductor layer as a seed. Alternatively, the region 372c included in the second oxide semiconductor layer having an amorphous structure can be crystal-grown using the region 372a of the first oxide semiconductor layer having a CAAC structure as a core. This crystal growth model can be considered to be equivalent to the concept of heteroepitaxial growth. Fig. 11C In FIG. 3 , the oxide semiconductor layer 370 c includes a region 372 a and a region 372 c. Fig. 11C The area 372a shown is Fig. 11B The region 372a shown in FIG. 372a is a region with higher crystallinity and density of crystal parts than the region 372a shown in FIG. By performing heat treatment, the crystallinity of either or both of the region 372a and the region 372c can be improved. In addition, the region 372c, for example, includes a crystal part having the same crystal structure as the crystal part included in the region 372a. Alternatively, the region 372c, for example, includes a crystal part connected to the crystal part included in the region 372a.

[0323] In addition, Fig.11D In the embodiment, the oxide semiconductor layer 370d includes a region 372a. The region 372a is Fig. 11B and Fig. 11C The crystallinity of the region 372a shown in the figure is further improved and the boundary between the region 372a and the region 372c disappears or the boundary between the region 372a and the region 372c cannot be confirmed. Therefore, the oxide semiconductor layer 370d has a CAAC structure as a whole. Fig.11D As shown, by making the entire oxide semiconductor layer 370d have a CAAC structure, a semiconductor device with high reliability can be realized. For example, the presence or absence of a boundary between the region 372a and the region 372c can be confirmed using cross-sectional TEM, cross-sectional STEM, or the like.

[0324] Even in the case where the first oxide semiconductor layer has a tiny gap or a tiny space, the tiny gap or the tiny space of the first oxide semiconductor layer can be filled by depositing the second oxide semiconductor layer on the first oxide semiconductor layer or depositing the second oxide semiconductor layer on the first oxide semiconductor layer and performing heat treatment. In this way, by using an oxide semiconductor layer with a CAAC structure as the first oxide semiconductor layer and using an oxide semiconductor layer with a microcrystalline structure or an amorphous structure as the second oxide semiconductor layer, a dense oxide semiconductor layer with improved crystallinity can be formed. By using the dense oxide semiconductor layer with improved crystallinity in the channel formation region of the transistor, the increase in the resistance of the oxide semiconductor layer can be suppressed or the initial characteristics of the transistor (especially the on-state current) can be improved, thereby expecting to realize a transistor suitable for high-speed driving.

[0325] In the case where an oxide semiconductor layer is formed by both a sputtering method and an ALD method, when the thickness of the oxide semiconductor layer formed by the ALD method is thin, it can be considered that the oxide semiconductor layer does not have a stacked structure of an oxide semiconductor layer formed by a sputtering method and an oxide semiconductor layer formed by an ALD method, but has a single-layer structure. For example, when the thickness of the oxide semiconductor layer formed by the ALD method exceeds 0 nm and is less than 3 nm, preferably exceeds 0 nm and is less than 2 nm, and more preferably exceeds 0 nm and is less than 1 nm, the oxide semiconductor layer formed by the two deposition methods of the sputtering method and the ALD method can be regarded as a single-layer structure. In this case, for example, in a cross-sectional TEM image, a cross-sectional STEM image, etc., the boundary between the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method cannot be observed. On the other hand, when the thickness of the oxide semiconductor layer formed by the ALD method exceeds 3 nm, it can sometimes be considered to have a stacked structure, a multilayer structure, or a multiple structure of an oxide semiconductor layer formed by a sputtering method and an oxide semiconductor layer formed by an ALD method.

[0326] In addition, when the oxide semiconductor layer is formed by both the sputtering method and the ALD method, it is preferable that each has a different composition. Typically, a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a vicinity thereof can be deposited by the sputtering method, and then a metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or a vicinity thereof can be deposited by the ALD method. By adopting the oxide semiconductor layer of the above composition, the following structure can be achieved: since the metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a vicinity thereof has higher reliability, and since the metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or a vicinity thereof has a high on-state current or high field effect mobility. In addition, a metal oxide having a high ratio of In:Ga:Zn=1:0:0 [atomic ratio], that is, a metal oxide having a high ratio of indium oxide or In, can be used instead of a metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or a vicinity thereof.

[0327] The oxide semiconductor layer formed by the above two deposition methods can be considered as a structure in which the gaps between the crystal parts in the CAAC structure are filled with atomic layers formed by the ALD method. In addition, the structure can be analyzed by cross-sectional SEM, STEM, cross-sectional TEM, SIMS, EDX and other analysis methods.

[0328] In addition, compared with an oxide semiconductor layer with a CAAC structure formed using one deposition method, any one or more of the relative dielectric constant, film density, and film hardness of the oxide semiconductor layer with a CAAC structure formed using the above two deposition methods is sometimes higher. In this way, by using an oxide semiconductor layer with a CAAC structure formed using two deposition methods for a channel formation region of a transistor, a transistor with good characteristics (for example, a transistor with a large on-state current, a transistor with a high field effect mobility, a transistor with a small S value, a transistor with a high frequency characteristic (also called f characteristic), a transistor with high reliability, etc.) can be realized.

[0329] In some cases, hydrogen contained in the oxide semiconductor reacts with oxygen bonded to a metal atom to generate water, thereby forming oxygen vacancies (V O In addition, sometimes hydrogen enters the defect in the oxygen vacancy (hereinafter referred to as V O H) is used as a donor to generate electrons as carriers. In addition, sometimes electrons as carriers are generated because part of the hydrogen is bonded to the oxygen bonded to the metal atom. Therefore, transistors using oxide semiconductors containing a large amount of hydrogen tend to have a normally-on characteristic (i.e., the threshold voltage is negative). In addition, because the hydrogen in the oxide semiconductor is easily moved due to heat, electric field, etc., the reliability of the transistor may be reduced when the oxide semiconductor contains a large amount of hydrogen.

[0330] That is, it is preferable to minimize the V O H so that the oxide semiconductor layer 230 becomes high-purity intrinsic or substantially high-purity intrinsic. O For an oxide semiconductor with sufficiently reduced H, it is important to: remove impurities such as water and hydrogen in the oxide semiconductor (sometimes referred to as dehydration or dehydrogenation treatment); and supply oxygen to the oxide semiconductor to repair oxygen vacancies. O An oxide semiconductor in which impurities such as H are sufficiently reduced is used for a channel formation region of a transistor to impart stable electrical characteristics. Note that a process of supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as an oxidation treatment.

[0331] The carrier concentration of the oxide semiconductor in the region serving as the channel formation region is preferably 1×10 18 cm -3 Below, more preferably below 1×10 17 cm -3 , more preferably less than 1×10 16 cm -3 , and more preferably less than 1×10 13 cm -3 , more preferably less than 1×10 12 cm -3 Note that the lower limit of the carrier concentration of the oxide semiconductor in the region serving as the channel formation region is not particularly limited, and can be set to 1×10 -9 cm -3 .

[0332] Here, the influence of each impurity in the metal oxide (oxide semiconductor) is described.

[0333] When the oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, a defect state is formed in the oxide semiconductor. Thus, the carbon concentration in the channel formation region of the oxide semiconductor measured by SIMS is set to 1×10 20 atoms / cm 3 Below, preferably 5×10 19 atoms / cm 3 Below, more preferably 3×10 19 atoms / cm 3 Below, more preferably 1×10 19 atoms / cm 3 Below, more preferably 3×10 18 atoms / cm 3 Below, more preferably 1×10 18atoms / cm 3 In addition, the silicon concentration in the channel formation region of the oxide semiconductor measured by SIMS was set to 1×10 20 atoms / cm 3 Below, preferably 5×10 19 atoms / cm 3 Below, more preferably 3×10 19 atoms / cm 3 Below, more preferably 1×10 19 atoms / cm 3 Below, more preferably 3×10 18 atoms / cm 3 Below, more preferably 1×10 18 atoms / cm 3 the following.

[0334] In addition, when the oxide semiconductor contains nitrogen, electrons as carriers are generated, which increases the carrier concentration and is easily converted to n-type. As a result, transistors using oxide semiconductors containing nitrogen as semiconductors tend to have normally-on characteristics. Alternatively, when the oxide semiconductor contains nitrogen, trap states are sometimes formed. As a result, the electrical characteristics of the transistor are sometimes unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor measured by SIMS is set to 1×10 20 atoms / cm 3 Below, preferably 5×10 19 atoms / cm 3 Below, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 Below, more preferably 1×10 18 atoms / cm 3 Below, more preferably 5×10 17 atoms / cm 3 the following.

[0335] In addition, hydrogen contained in the oxide semiconductor reacts with oxygen bonded to metal atoms to generate water, so oxygen vacancies are sometimes formed. When hydrogen enters the oxygen vacancy, electrons as carriers are sometimes generated. In addition, sometimes electrons as carriers are generated because part of the hydrogen is bonded to oxygen bonded to metal atoms. Therefore, transistors using oxide semiconductors containing hydrogen tend to have normally-on characteristics. Therefore, it is preferred to reduce the hydrogen in the channel formation region of the oxide semiconductor as much as possible. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor measured by SIMS is set to less than 1×1020 atoms / cm 3 , preferably less than 5×10 19 atoms / cm 3 , more preferably less than 1×10 19 atoms / cm 3 , more preferably less than 5×10 18 atoms / cm 3 , and more preferably less than 1×10 18 atoms / cm 3 .

[0336] In addition, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, a defect state is sometimes formed to generate carriers. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal tends to have a normally-on characteristic. Thus, the concentration of the alkali metal or alkaline earth metal in the channel formation region of the oxide semiconductor measured by SIMS is set to 1×10 18 atoms / cm 3 Below, preferably 2×10 16 atoms / cm 3 the following.

[0337] By using an oxide semiconductor in which impurities are sufficiently reduced for a channel formation region of a transistor, the transistor can have stable electrical characteristics.

[0338] In addition, transistors using other semiconductor materials in the channel formation region may also be used in the semiconductor device of this embodiment. As the other semiconductor material, for example, a semiconductor composed of a single element or a compound semiconductor may be cited. As a semiconductor composed of a single element, for example, silicon or germanium may be cited. As a compound semiconductor, for example, gallium arsenide and silicon germanium may be cited. In addition, as a compound semiconductor, for example, an organic semiconductor and a nitride semiconductor may be cited. The above-mentioned oxide semiconductor is also a type of compound semiconductor. These semiconductor materials may also contain impurities as dopants.

[0339] Examples of silicon that can be used as a semiconductor material for transistors include single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. Examples of polycrystalline silicon include low temperature polycrystalline silicon (LTPS: Low Temperature Poly Silicon).

[0340] In addition, the semiconductor layer of the transistor may also include a layered material used as a semiconductor. Layered material is a general term for a group of materials having a layered crystal structure. The layered crystal structure is a structure in which layers formed by covalent bonds or ionic bonds are stacked by bonds such as van der Waals bonding forces that are weaker than covalent bonds and ionic bonds. The layered material has high conductivity in a unit layer, that is, has high two-dimensional conductivity. By using a material used as a semiconductor and having high two-dimensional conductivity in a channel formation region, a transistor with a large on-state current can be provided.

[0341] Examples of the layered material include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing oxygen group elements (elements belonging to Group 16). In addition, examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides. Transistors include transition metal chalcogenides that can be used as semiconductor layers, specifically molybdenum sulfide (typically MoS 2 ), Molybdenum selenide (typically MoSe 2 ), molybdenum telluride (typically MoTe 2 ), tungsten sulfide (typically WS 2 ), tungsten selenide (typically WSe 2 ), tungsten telluride (typically WTe 2 ), hafnium sulfide (typically HfS 2 ), hafnium selenide (typically HfSe 2 ), zirconium sulfide (typically ZrS 2 ), zirconium selenide (typically ZrSe 2 )wait.

[0342] [Substrate] As a substrate for forming a transistor, for example, an insulator substrate, a semiconductor substrate or a conductor substrate can be used. As an insulator substrate, for example, a glass substrate, a quartz substrate, a sapphire substrate, a stabilized zirconia substrate (yttria stabilized zirconia substrate, etc.), a resin substrate, etc. can be cited. In addition, as a semiconductor substrate, for example, a semiconductor substrate made of silicon or germanium, or a compound semiconductor substrate composed of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, gallium oxide, etc. can be cited. In addition, a semiconductor substrate having an insulator region inside the above-mentioned semiconductor substrate, such as an SOI (Silicon On Insulator) substrate, etc. can also be cited. As a conductor substrate, a graphite substrate, a metal substrate, an alloy substrate, a conductive resin substrate, etc. can be cited. Alternatively, a substrate containing a metal nitride, a substrate containing a metal oxide, etc. can be cited. In addition, an insulator substrate provided with a conductor or a semiconductor, a semiconductor substrate provided with a conductor or an insulator, a conductor substrate provided with a semiconductor or an insulator, etc. can also be cited. Alternatively, a substrate having elements provided on these substrates can also be used. Examples of the element provided over the substrate include a capacitor, a resistor, a switching element, a light emitting element, and a memory element.

[0343] <Example 1 of Method for Manufacturing Semiconductor Device> Reference FIG. 12A to FIG. 12C A method for manufacturing a semiconductor device is described. Fig. 7A Note that regarding the materials and formation methods of the components, the same parts as those already described may be omitted.

[0344] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting semiconductor devices can be formed by sputtering, CVD, vacuum deposition, PLD, ALD, or the like.

[0345] As a sputtering method, there can be cited an RF sputtering method in which a high-frequency power supply is used as a power supply for sputtering, a DC sputtering method in which a direct current power supply is used, and a pulsed DC sputtering method in which the voltage applied to the electrode is changed in a pulsed manner. In addition, there is an RF superposition DC sputtering method in which RF and DC are superimposed. In the deposition using an insulating target material, the RF sputtering method is preferably used. The DC sputtering method is mainly used when a conductive target material is used for deposition. In addition, in the DC sputtering method, in addition to forming a conductive film, an insulating film can also be formed by performing reactive sputtering. In addition, the pulsed DC sputtering method is mainly used when compounds such as oxides, nitrides, and carbides are deposited using a reactive sputtering method. The RF superposition DC sputtering method can control the ion energy during deposition and the potential on one side of the target material. Therefore, compared with the RF sputtering method, the damage caused by deposition can be reduced. In addition, a film of good quality can be obtained.

[0346] As the sputtering method, for example, an ionized sputtering method, a long-throw sputtering method, etc. can be used. The ionized sputtering method is a method in which sputtered particles generated from a target material are ionized by RF or the like, and deposition is performed anisotropically by self-bias or the like. In addition, in the long-throw sputtering method, anisotropic deposition can be performed by increasing the distance between the sputtering target material and the substrate.

[0347] Note that the CVD method can be divided into PECVD method, thermal CVD (TCVD: Thermal CVD) method using heat, photo CVD (Photo CVD) method using light, etc. Furthermore, it can be divided into metal CVD (MCVD: Metal CVD) method and metal organic CVD (MOCVD: Metal Organic CVD) method according to the source gas used.

[0348] By utilizing the PECVD method, a high-quality film can be obtained at a lower temperature. In addition, since plasma is not used, the thermal CVD method is a deposition method that can reduce plasma damage to the object being processed. For example, the wiring, electrodes, components (transistors, capacitors, etc.) included in the semiconductor device sometimes generate charge accumulation due to receiving charges from plasma. At this time, the wiring, electrodes, components, etc. included in the semiconductor device are sometimes damaged due to the accumulated charges. On the other hand, since the above-mentioned plasma damage does not occur in the case of the thermal CVD method without using plasma, the yield of the semiconductor device can be improved. In addition, in the thermal CVD method, plasma damage during deposition is not generated, so a film with fewer defects can be obtained.

[0349] As the ALD method, a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, a PEALD (Plasma Enhanced ALD) method using a reactant excited by plasma, and the like are used.

[0350] The ALD method can deposit atoms in each layer, thereby achieving the effects of being able to deposit extremely thin films, being able to deposit structures with high aspect ratios, being able to deposit with fewer defects such as pinholes, being able to deposit with excellent coverage, and being able to deposit at low temperatures. In the PEALD (Plasma Enhanced ALD) method, by utilizing plasma, film formation can be performed at lower temperatures, so it is sometimes preferred. The precursors used in the ALD method sometimes contain impurities such as carbon. Therefore, films formed using the ALD method sometimes contain more impurities such as carbon than films formed using other deposition methods. In addition, the quantification of impurities can be measured using X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy).

[0351] Unlike a deposition method in which particles released from a target material are deposited, the CVD method and the ALD method are deposition methods in which a film is formed due to a reaction on the surface of the object to be processed. Therefore, the CVD method and the ALD method are deposition methods that are not easily affected by the shape of the object to be processed and have high step coverage. In particular, the ALD method has good step coverage and thickness uniformity, so the ALD method is suitable for forming a film covering the surface of an opening with a high aspect ratio. However, the deposition rate of the ALD method is relatively slow, so it is sometimes preferred to use it in combination with other deposition methods such as the CVD method with a fast deposition rate.

[0352] The CVD method or the ALD method can control the composition of the obtained film by adjusting the flow ratio of the source gas. For example, when the CVD method and the ALD method are used, a film of any composition can be deposited according to the flow ratio of the source gas. In addition, for example, when the CVD method or the ALD method is used, a film whose composition continuously changes can be formed by changing the flow ratio of the source gas while performing deposition. When deposition is performed while changing the flow ratio of the source gas, since the time required for conveying and adjusting the pressure is not required, the deposition time can be shortened compared to the case where deposition is performed using multiple deposition chambers. Therefore, the productivity of the semiconductor device can sometimes be improved.

[0353] In addition, when the CVD method is used, a film of any composition can be deposited according to the flow ratio of the source gas. For example, when the CVD method is used, a film whose composition continuously changes can be deposited by changing the flow ratio of the source gas while performing deposition. When deposition is performed while changing the flow ratio of the source gas, since the time required for conveying or adjusting the pressure is not required, the deposition time can be shortened compared to the case where deposition is performed using multiple deposition chambers. Therefore, the productivity of the semiconductor device can sometimes be improved.

[0354] When the ALD method is used, a film of any composition can be deposited by introducing different precursors at the same time. Alternatively, when introducing different precursors, a film of any composition can be deposited by controlling the number of cycles of each precursor.

[0355] Thin films (insulating films, semiconductor films, conductive films, etc.) that constitute semiconductor devices can be formed using wet deposition methods such as spin coating, dipping, spraying, inkjet, dispenser, screen printing, offset printing, doctor knife, slit coating, roll coating, curtain coating, or doctor knife coating.

[0356] In addition, when processing a thin film constituting a semiconductor device, photolithography or the like can be used. Alternatively, the thin film can be processed by nanoimprinting, sandblasting, lift-off, etc. In addition, an island-shaped thin film can be directly formed by a deposition method using a shielding mask such as a metal mask.

[0357] There are two typical methods of photolithography. One is to form a resist mask on the thin film to be processed, process the thin film by etching, etc., and remove the resist mask. The other is to deposit a photosensitive thin film, then expose and develop it, and process the thin film into a desired shape.

[0358] In the photolithography method, as the light used for exposure, for example, i-line (wavelength 365nm), g-line (wavelength 436nm), h-line (wavelength 405nm) or light mixed with these rays can be used. In addition, ultraviolet light, KrF laser or ArF laser, etc. can also be used. In addition, liquid immersion exposure technology can also be used for exposure. In addition, as the light used for exposure, extreme ultraviolet (EUV: Extreme Ultra-violet) light or X-rays can also be used. In addition, instead of the light used for exposure, an electron beam can also be used. When extreme ultraviolet light, X-rays or electron beams are used, extremely fine processing can be performed, so it is preferred. Note that when exposure is performed by scanning with a light beam such as an electron beam, a photomask is not required.

[0359] As a method for etching the thin film, dry etching, wet etching, sand blasting, or the like can be used.

[0360] First, conductive layer 220 is formed on insulating layer 210, insulating layer 280 is formed on conductive layer 220, and conductive layer 240 is formed on insulating layer 280. Here, insulating layer 280 has a three-layer stacked structure of insulating layer 280a, insulating layer 280b, and insulating layer 280c.

[0361] Note that it is preferable to perform a planarization process (also referred to as a CMP process) by a chemical mechanical polishing (CMP) method after depositing the insulating layer 280 to planarize the top surface of the insulating layer 280. By performing the planarization process of the insulating layer 280, the surface on which the conductive layer 240 is formed as wiring can be flattened, thereby suppressing disconnection of the conductive layer 240. Alternatively, the planarization process may not be performed, in which case the manufacturing cost can be reduced.

[0362] Next, an opening 290 ( Fig. 12A At this time, a recessed portion is formed in the conductive layer 220 at a position overlapping with the opening 290 .

[0363] Since the aspect ratio of the opening 290 is high, it is preferable to use anisotropic etching to process a portion of the conductive layer 240 and a portion of the insulating layer 280. In particular, processing using a dry etching method is suitable for micro-processing and is therefore preferred. In addition, the processing can also be performed under different conditions depending on the layer.

[0364] Here, it is preferable to adopt processing conditions that make the side walls of the conductive layer 240 and the insulating layer 280c have a tapered shape. In addition, it is preferable to adopt processing conditions that make the side walls of the insulating layer 280b have a steep shape.

[0365] The insulating layer 280a may be formed using processing conditions in which the sidewall has a tapered shape or may be formed using processing conditions in which the sidewall has a steep shape.

[0366] Here, by appropriately selecting and changing the material of the insulating layer 280 c and the material of the insulating layer 280 b , the insulating layer 280 c can have a tapered shape and the insulating layer 280 b can have a steep shape using the same dry etching conditions.

[0367] Next, a heat treatment may be performed. The heat treatment may be performed, for example, at 250° C. to 650° C., preferably 300° C. to 500° C., and more preferably 320° C. to 450° C.

[0368] In addition, heat treatment is performed in an atmosphere of nitrogen gas or an inert gas or an atmosphere containing an oxidizing gas of more than 10 ppm, more than 1%, or more than 10%. For example, when heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the ratio of oxygen gas is preferably set to about 20%. The heat treatment can also be performed under reduced pressure. Alternatively, the heat treatment can also be performed in an atmosphere of nitrogen gas or an inert gas, and then heat treatment is performed in an atmosphere containing an oxidizing gas of more than 10 ppm, more than 1%, or more than 10% to compensate for the oxygen that has been separated. By performing the above-mentioned heat treatment, impurities such as water contained in the insulating layer 280, etc. can be reduced before the deposition of the oxide semiconductor layer 230 to be described later.

[0369] In addition, the gas used in the above-mentioned heat treatment is preferably highly purified. For example, the amount of water contained in the gas used in the above-mentioned heat treatment is preferably 1 ppb or less, more preferably 0.1 ppb or less, and further preferably 0.05 ppb or less. By using a highly purified gas for heat treatment, it is possible to prevent moisture and the like from being absorbed by the insulating layer 280 and the like as much as possible.

[0370] The openings in the conductive layer 240 and the insulating layer 280 may be formed using the same mask or different masks.

[0371] Next, the oxide semiconductor layer 230 is formed to cover the opening 290. The oxide semiconductor layer 230 is formed to be in contact with the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the top surface and side surface of the conductive layer 240.

[0372] The oxide semiconductor layer 230 can be deposited by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method.

[0373] The oxide semiconductor layer 230 is preferably formed as a film having a thickness as uniform as possible along the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the side surface of the conductive layer 240 in the opening 290. By depositing using the ALD method, a thinner film can be deposited with high controllability. Therefore, the oxide semiconductor layer 230 is preferably deposited using the ALD method.

[0374] In addition, when the crystallinity of the oxide semiconductor layer 230 is high, diffusion of impurities in the oxide semiconductor layer 230 is suppressed, so that the electrical characteristics of the transistor are less likely to change, thereby improving reliability. Sputtering is preferred because it is easier to form a layer with high crystallinity than using the ALD method.

[0375] For example, when the oxide semiconductor layer 230 is formed by sputtering, oxygen or a mixed gas of oxygen and a rare gas is used as the sputtering gas. By increasing the ratio of oxygen contained in the sputtering gas, the excess oxygen in the deposited oxide film can be increased. In addition, when the above-mentioned oxide film is deposited by sputtering, an In-M-Zn oxide target or the like can be used.

[0376] In the case of forming the oxide semiconductor layer 230 using a sputtering method, when deposition is performed under the condition that the ratio of oxygen contained in the sputtering gas is greater than 30% and less than 100%, preferably greater than 70% and less than 100%, an oxygen-excess oxide semiconductor is formed. A transistor using an oxygen-excess oxide semiconductor in a channel formation region can obtain relatively high reliability. Note that one embodiment of the present invention is not limited to this. At this time, when the ratio of oxygen contained in the sputtering gas is set to greater than 1% and less than 30%, preferably greater than 5% and less than 20%, an oxygen-deficient oxide semiconductor is formed. A transistor using an oxygen-deficient oxide semiconductor in a channel formation region can have a higher field effect mobility. In addition, by performing deposition while heating the substrate, the crystallinity of the oxide semiconductor layer can be improved.

[0377] Next, the conductive layer 240 and the oxide semiconductor layer 230 are processed into island shapes ( Fig. 12B Here, the conductive layer 240 and the oxide semiconductor layer 230 can be processed together using the same mask.

[0378] In addition, the process of processing the conductive layer 240 into an island shape and the process of processing the oxide semiconductor layer 230 into an island shape may be performed separately and independently. In this case, for example, the process of processing the conductive layer 240 into an island shape and the process of providing the opening 290 in the conductive layer 240 may be performed separately and independently, and the order of the processes is not limited. In addition, etching may be performed after performing exposure using a mask for processing into a square island shape and exposure using a mask for providing a circular opening, thereby performing island processing and opening formation at one time. In addition, exposure using a multi-level grayscale mask (typically a halftone mask or a gray tone mask) may also be used.

[0379] Next, the insulating layer 250 is formed over the oxide semiconductor layer 230 and the insulating layer 280 . The insulating layer 250 is formed in contact with the oxide semiconductor layer 230 .

[0380] Next, heat treatment is preferably performed. The heat treatment is preferably performed within a temperature range in which the oxide semiconductor layer 230 is not polycrystallized. The temperature of the heat treatment is preferably 100° C. to 650° C., more preferably 250° C. to 600° C., and further preferably 350° C. to 550° C. The details of the heat treatment can be referred to the above description.

[0381] In addition, the gas used in the above-mentioned heat treatment is preferably highly purified. By performing the heat treatment using a highly purified gas, it is possible to prevent moisture and the like from being absorbed by the oxide semiconductor layer 230 and the like as much as possible.

[0382] In this embodiment, as a heat treatment, a treatment is performed for 1 hour under the conditions of a flow ratio of nitrogen gas to oxygen gas of 4:1 and a temperature of 450°C. Such a heat treatment containing oxygen gas can reduce impurities such as carbon, water, and hydrogen in the oxide semiconductor layer 230. In this way, by reducing impurities in the film and improving the crystallinity of the oxide semiconductor layer 230, a denser structure with a higher density can be obtained. Therefore, the crystallized area in the oxide film oxide semiconductor layer 230 can be increased, and the in-plane unevenness of the crystallized area in the oxide semiconductor layer 230 can be reduced. Therefore, the in-plane unevenness of the electrical characteristics of the transistor can be reduced.

[0383] In addition, when the insulating layer 280 contains oxygen, it is preferable to supply oxygen from the insulating layer 280 to the channel formation region of the oxide semiconductor layer 230 by heat treatment. In this way, oxygen vacancies and V O H.

[0384] Next, a conductive layer to be the conductive layer 260a is formed on the insulating layer 250. The conductive layer to be the conductive layer 260a is formed so as to sandwich the oxide semiconductor layer 230 and the insulating layer 250 and cover the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the top surface and side surface of the conductive layer 240. Next, a conductive layer to be the conductive layer 260b is formed.

[0385] Conductive layer 260a and conductive layer 260b are formed in contact with insulating layer 250 provided in opening portion 290 having a high aspect ratio. Therefore, the conductive layer to be conductive layer 260a and the conductive layer to be conductive layer 260b are preferably deposited using a deposition method with good coverage, and more preferably using an ALD method, a metal CVD method, or the like.

[0386] Next, a portion of the conductive layer to be the conductive layer 260b and a portion of the conductive layer to be the conductive layer 260a are removed using a mask to form the conductive layer 260b and the conductive layer 260a ( Fig. 12C ).

[0387] Through the above steps, the semiconductor device according to one embodiment of the present invention can be manufactured.

[0388] <Example 2 of Method for Manufacturing Semiconductor Device> The following instructions Fig. 10B An example of a method for manufacturing a semiconductor device is shown.

[0389] First, manufacture Fig. 12B Next, a dummy structure is formed in the region where the insulating layer 250 and the conductive layer 260 are provided. Then, an insulating layer 283 and an insulating layer 285 are formed outside the dummy structure.

[0390] Next, the dummy structure is removed, and the insulating layer 250 and the conductive layer 260 are formed.

[0391] Next, a conductive layer 265 is formed over the conductive layer 260 and the insulating layer 285 .

[0392] Through the above steps, we can produce Fig. 10B The semiconductor device shown. Note that Fig. 10B The manufacturing method of the semiconductor device shown is not limited thereto.

[0393] This embodiment mode can be appropriately combined with other embodiment modes. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be appropriately combined.

[0394] Implementation Method 2 In this embodiment, refer to FIG. 14A to FIG. 17A memory device according to one embodiment of the present invention is described. A memory device according to one embodiment of the present invention includes a memory cell. The memory cell includes a transistor and a capacitor.

[0395] <Configuration Example 1 of Storage Device> Reference FIG. 14A to FIG. 14C The structure of a memory device including a transistor and a capacitor is described. Fig.14A is a plan view of a memory device including a transistor 200 and a capacitor 100 . Fig. 14B It is along Fig.14A A cross-sectional view along the dashed line A1-A2 is shown. Fig. 14C It is along Fig.14A A cross-sectional view along the dashed line A3-A4 is shown.

[0396] FIG. 14A to FIG. 14C The memory device shown includes an insulating layer 140 on a substrate (not shown), a conductive layer 110 on the insulating layer 140, a memory cell 150 on the conductive layer 110, an insulating layer 180 on the conductive layer 110, an insulating layer 280, and an insulating layer 283 on the memory cell 150. The insulating layer 140, the insulating layer 180, the insulating layer 280, and the insulating layer 283 are used as interlayer films. The conductive layer 110 is used as wiring.

[0397] The memory cell 150 includes a capacitor 100 on a conductive layer 110 and a transistor 200 on the capacitor 100 .

[0398] The capacitor 100 includes a conductive layer 115 on the conductive layer 110, an insulating layer 130 on the conductive layer 115, and a conductive layer 120 on the insulating layer 130. The conductive layer 120 is used as one of a pair of electrodes (sometimes referred to as an upper electrode), the conductive layer 115 is used as the other of the pair of electrodes (sometimes referred to as a lower electrode), and the insulating layer 130 is used as a dielectric. That is, the capacitor 100 constitutes a MIM (Metal-Insulator-Metal) capacitor.

[0399] like Fig. 14B and Fig. 14C As shown, an opening 190 that reaches the conductive layer 110 is provided in the insulating layer 180. At least a portion of the conductive layer 115 is disposed in the opening 190. Note that the conductive layer 115 has a region in contact with the top surface of the conductive layer 110 at the opening 190, a region in contact with the side surface of the insulating layer 180 at the opening 190, and a region in contact with at least a portion of the top surface of the insulating layer 180. The insulating layer 130 is disposed so that at least a portion thereof is located in the opening 190. The conductive layer 120 is disposed so that at least a portion thereof is located in the opening 190. In addition, as shown in FIG. Fig. 14B and Fig. 14CAs shown, the conductive layer 120 is preferably provided in a manner embedded in the opening 190. In addition, the film provided inside the opening 190 is preferably formed by a method with high coverage such as the ALD method. Thus, the film has good coverage. For example, the conductive layer 115, the insulating layer 130, and the conductive layer 120 are preferably formed by the ALD method, the metal CVD method, or the like.

[0400] The capacitor 100 has a structure in which the upper electrode and the lower electrode are opposed to each other through a dielectric body in the opening 190 not only on the bottom surface but also on the side surface, so that the electrostatic capacitance per unit area can be increased. Thus, the deeper the depth of the opening 190, the greater the electrostatic capacitance of the capacitor 100 can be. In this way, by increasing the electrostatic capacitance per unit area of ​​the capacitor 100, the read operation of the storage device can be stabilized. In addition, the miniaturization or high integration of the storage device can be promoted.

[0401] Fig. 14B and Fig. 14C The example in which the side wall of the opening 190 is perpendicular to the top surface of the conductive layer 110 is shown. In this case, the opening 190 has a cylindrical shape. By adopting such a structure, miniaturization or high integration of the storage device can be achieved.

[0402] Conductive layer 115 and insulating layer 130 are stacked along the sidewalls of opening 190 and the top surface of conductive layer 110. Conductive layer 120 is provided on insulating layer 130 so as to be embedded in opening 190. Capacitor 100 having such a structure may be referred to as a trench capacitor or trench capacitor.

[0403] The insulating layer 280 is disposed on the capacitor 100 . That is, the insulating layer 280 is disposed on the conductive layer 115 , the insulating layer 130 , and the conductive layer 120 . In other words, the conductive layer 120 is disposed under the insulating layer 280 .

[0404] The transistor 200 includes a conductive layer 120 (corresponding to Figure 2B The conductive layer 220 is formed on the insulating layer 280, the conductive layer 240 is formed on the insulating layer 280, the oxide semiconductor layer 230, the insulating layer 250 is formed on the oxide semiconductor layer 230, and the conductive layer 260 is formed on the insulating layer 250. The oxide semiconductor layer 230 is used as a semiconductor layer, the conductive layer 260 is used as a gate electrode, the insulating layer 250 is used as a gate insulating layer, the conductive layer 120 is used as one of a source electrode and a drain electrode, and the conductive layer 240 is used as the other of the source electrode and the drain electrode.

[0405] Regarding the transistor 200, reference can be made to Embodiment 1 ( FIG. 2A to FIG. 2C and FIG. 3A to FIG. 3D In addition, the transistors included in the memory cell 150 are not limited to FIG. 2A to FIG. 2C and FIG. 3A to FIG. 3D The transistor 200 , etc., can also be applied to each transistor illustrated in Embodiment 1.

[0406] like FIG. 14A to FIG. 14C As shown, the transistor 200 overlaps with the capacitor 100. In addition, the opening 290 in which a part of the structure of the transistor 200 is provided has an area overlapping with the opening 190 in which a part of the structure of the capacitor 100 is provided. In particular, the conductive layer 120 is used as one of the source electrode and the drain electrode of the transistor 200 and is used as the upper electrode of the capacitor 100, so the transistor 200 and the capacitor 100 share part of the structure. By adopting this structure, the transistor 200 and the capacitor 100 can be arranged in a manner that does not significantly increase the occupied area when viewed from above. As a result, the occupied area of ​​the memory cell 150 can be reduced, so the memory cell 150 can be arranged at a high density to increase the storage capacity of the storage device. In other words, high integration of the storage device can be achieved.

[0407] Furthermore, by placing the transistor 200 above the capacitor 100, the transistor 200 is not affected by the heat treatment during the manufacture of the capacitor 100. Therefore, the degradation of the electrical characteristics of the transistor 200, such as the variation in threshold voltage and the increase in parasitic resistance, and the increase in the unevenness of the electrical characteristics caused by the degradation of the electrical characteristics can be suppressed.

[0408] Fig.19A 2 is a circuit diagram of a storage device shown in this embodiment. Fig.19A As shown, FIG. 14A to FIG. 14C The structure shown is used as a memory cell. The memory cell 951 includes a transistor M1 and a capacitor CA. Here, the transistor M1 corresponds to the transistor 200, and the capacitor CA corresponds to the capacitor 100.

[0409] One of the source and drain of the transistor M1 is connected to one of the pair of electrodes of the capacitor CA. The other of the source and drain of the transistor M1 is connected to the wiring BIL. The gate of the transistor M1 is connected to the wiring WOL. The other of the pair of electrodes of the capacitor CA is connected to the wiring CAL.

[0410] Here, the wiring BIL corresponds to the conductive layer 240, the wiring WOL corresponds to the conductive layer 260, and the wiring CAL corresponds to the conductive layer 110. FIG. 14A to FIG. 14C As shown, it is preferred that the conductive layer 260 extends in the X direction and the conductive layer 240 extends in the Y direction. By adopting this structure, the wiring BIL and the wiring WOL intersect each other. Fig.14A The wiring CAL (conductive layer 110) is provided in a planar shape, but the present invention is not limited thereto. For example, the wiring CAL may be parallel to the wiring WOL (conductive layer 260) or the wiring BIL (conductive layer 240).

[0411] Note that the storage unit will be described in detail in a later embodiment.

[0412] FIG. 13A to FIG. 13C Shown in FIG. 14A to FIG. 14C The structure used as transistor 200 Figures 1A to 1C An example of the structure is shown.

[0413] [Capacitor 100] The capacitor 100 includes a conductive layer 115, an insulating layer 130, and a conductive layer 120. In addition, a conductive layer 110 is disposed below the conductive layer 115. The conductive layer 115 has a region in contact with the conductive layer 110.

[0414] The conductive layer 110 is provided on the insulating layer 140. The conductive layer 110 is used as a wiring CAL and can be provided in a planar shape, for example. As the conductive layer 110, a single layer or a stack of conductive materials described in [Conductor] of Embodiment 1 can be used. As the conductive layer 110, for example, a conductive material with high conductivity such as tungsten can be used. By using a conductive material with high conductivity in this way, the conductivity of the conductive layer 110 can be improved, so that the conductive layer 110 can fully function as a wiring CAL.

[0415] In addition, as the conductive layer 115, it is preferred to use a conductive material that is not easily oxidized or a conductive material that has a function of inhibiting oxygen diffusion in a single layer or a stacked layer. For example, titanium nitride or indium tin oxide with silicon added thereto may be used. Alternatively, for example, a structure may be provided in which tantalum nitride is stacked on tungsten. Alternatively, for example, a structure may be provided in which a first titanium nitride, tungsten, and a second titanium nitride are stacked in sequence. By adopting such a structure, when an oxide is used as the insulating layer 130, oxidation of the conductive layer 110 due to the insulating layer 130 can be suppressed. Furthermore, when an oxide is used as the insulating layer 180, oxidation of the conductive layer 110 due to the insulating layer 180 can be suppressed.

[0416] The insulating layer 130 is provided on the conductive layer 115. The insulating layer 130 is provided in contact with the top surface and the side surface of the conductive layer 115. That is, the insulating layer 130 preferably covers the side end of the conductive layer 110. Thus, the conductive layer 115 and the conductive layer 120 can be prevented from being short-circuited.

[0417] Alternatively, a structure may be employed in which the side ends of the insulating layer 130 are aligned with the side ends of the conductive layer 115. With such a structure, the insulating layer 130 and the conductive layer 115 can be formed using the same mask, thereby simplifying the manufacturing process of the memory device.

[0418] A material with a high relative dielectric constant (high-k) is preferably used as insulating layer 130. By using a high-k material for insulating layer 130, the thickness of insulating layer 130 can be increased to a level capable of suppressing leakage current and the electrostatic capacitance of capacitor 100 can be sufficiently ensured.

[0419] In addition, as the insulating layer 130, it is preferred to stack an insulator composed of a high-k material, and it is preferred to use a stacked structure of a material with a high relative dielectric constant (high-k) and a material with a dielectric strength greater than that of the high-k material. For example, as the insulating layer 130, an insulating film in which zirconium oxide, aluminum oxide, and zirconium oxide are stacked in sequence can be used. In addition, for example, an insulating film in which zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide are stacked in sequence can be used. In addition, for example, an insulating film in which hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide are stacked in sequence can be used. By stacking an insulating layer with a larger dielectric strength such as aluminum oxide, the dielectric strength can be increased and the electrostatic destruction of the capacitor 100 can be suppressed.

[0420] Alternatively, a material having ferroelectricity may be used as the insulating layer 130. For details of the material having ferroelectricity, the description of Embodiment Mode 1 can be referred to.

[0421] The metal oxide containing one or both of hafnium and zirconium can have ferroelectricity even in a thin film of a few nm, so it is preferably used for the insulating layer 130. The thickness of the insulating layer 130 can be 100nm or less, more preferably 50nm or less, further preferably 20nm or less, and further preferably 10nm or less (typically, 2nm or more and 9nm or less). In addition, for example, the thickness is preferably 8nm or more and 12nm or less. By using a ferroelectric layer that can be thinned, the capacitor 100 can be combined with a semiconductor element such as a miniaturized transistor to form a semiconductor device.

[0422] In addition, a metal oxide containing one or both of hafnium and zirconium can have ferroelectricity even when its area is small, and therefore it is preferably used for the insulating layer 130. For example, even if the area (occupied area) of the ferroelectric layer in plan view is 100 μm 2 Below, 10μm 2 Below, 1μm 2 Below or 0.1μm 2 The following may also have ferroelectric properties. In addition, sometimes the ferroelectric layer has an area (occupied area) of 10000nm when viewed from above. 2 Below or 1000nm 2 The area occupied by the capacitor 100 can be reduced by reducing the area of ​​the ferroelectric layer.

[0423] Ferroelectrics are insulators that are polarized internally when exposed to an external electric field and that maintain polarization even when the electric field is zero. Therefore, a nonvolatile memory element can be formed by using a capacitor (hereinafter sometimes referred to as a ferroelectric capacitor) that uses the material as a dielectric. Nonvolatile memory elements using ferroelectric capacitors are sometimes referred to as FeRAM (Ferroelectric Random Access Memory), ferroelectric memories, and the like. For example, a ferroelectric memory includes a transistor and a ferroelectric capacitor, and one of the source and drain of the transistor is electrically connected to a terminal of the ferroelectric capacitor. Thus, in the case where a ferroelectric capacitor is used as the capacitor 100, the storage device shown in this embodiment is used as a ferroelectric memory.

[0424] The conductive layer 120 is provided in contact with a portion of the top surface of the insulating layer 130. In addition, the side end portion of the conductive layer 120 is preferably located inside the side end portion of the conductive layer 115 in both the X direction and the Y direction. Note that in a structure in which the insulating layer 130 covers the side end portion of the conductive layer 115, the side end portion of the conductive layer 120 may be located outside the side end portion of the conductive layer 115.

[0425] The conductive layer 120 can be formed in a single layer or a stacked layer using the conductive material described in the item [Conductive layer] of Embodiment 1. As the conductive layer 120, it is preferable to use a conductive material that is not easily oxidized or a conductive material that has a function of inhibiting oxygen diffusion. For example, titanium nitride or tantalum nitride can be used. In addition, for example, it is also possible to have a structure in which tantalum nitride is stacked on titanium nitride. In this case, titanium nitride is in contact with the insulating layer 130, and tantalum nitride is in contact with the oxide semiconductor layer 230. By adopting this structure, excessive oxidation of the conductive layer 120 caused by the oxide semiconductor layer 230 can be suppressed. In addition, when an oxide is used for the insulating layer 130, excessive oxidation of the conductive layer 120 caused by the insulating layer 130 can be suppressed. Alternatively, the conductive layer 120 may also have a structure in which tungsten is stacked on titanium nitride, for example.

[0426] Since the conductive layer 120 has a region in contact with the oxide semiconductor layer 230, it is preferable to use a conductive material containing oxygen. By using a conductive material containing oxygen as the conductive layer 120, conductivity can be maintained even if the conductive layer 120 absorbs oxygen. In addition, when an insulating layer containing oxygen such as zirconium oxide is used as the insulating layer 130, conductivity can be maintained in the conductive layer 120, so it is preferable. As the conductive layer 120, for example, a single layer or a stacked layer of ITO, ITSO, IZO (registered trademark), etc. can be used.

[0427] Since the insulating layer 180 is used as an interlayer film, its relative dielectric constant is preferably low. By using a material with a low relative dielectric constant for the interlayer film, the parasitic capacitance generated between the wirings can be reduced. As the insulating layer 180, a single layer or a stack of insulating layers containing a material with a low relative dielectric constant can be used. Silicon oxide and silicon oxynitride are preferred because they have thermal stability.

[0428] Note that Fig. 14B and Fig. 14C The insulating layer 180 is shown as a single-layer structure, but the present invention is not limited thereto. The insulating layer 180 may also have a two-layer structure, or a stacked structure of three or more layers.

[0429] <Configuration Example 2 of Storage Device> The memory cell 150 of the transistor 200 and the capacitor 100 shown in this embodiment can be used as a memory cell of a memory device. The transistor 200 is a transistor whose channel is formed in a semiconductor layer including an oxide semiconductor. Since the off-state current of the transistor 200 is small, the storage content can be maintained for a long time by using it in a memory device. In other words, since no refresh operation is required or the frequency of the refresh operation is extremely low, the power consumption of the memory device can be substantially reduced. In addition, since the frequency characteristics of the transistor 200 are high, high-speed reading and writing of the memory device can be performed.

[0430] By arranging the memory cells 150 three-dimensionally and in a matrix, a memory cell array can be constructed.

[0431] Fig.15A is a plan view of a storage device. Fig.15A An example is shown in which 2×2 memory cells (memory cells 150 a to 150 d ) are arranged in the X direction and the Y direction.

[0432] Fig. 15B It is along Fig.15A The cross-sectional view along the dotted line A3-A4 is shown. Fig.15A and Fig. 15B In the two storage units (in Fig. 15B In the embodiment, the memory cell 150a and the memory cell 150b) are connected to a common wiring (conductive layer 246).

[0433] Here, Fig.15A and Fig. 15B The memory cell 150a and the memory cell 150b shown have the same structure as the memory cell 150. The memory cell 150a includes a capacitor 100a and a transistor 200a, and the memory cell 150b includes a capacitor 100b and a transistor 200b. Fig.15AThe storage unit 150c and the storage unit 150d shown in FIG. 1 also have the same structure as the storage unit 150. Fig.15A and Fig. 15B In the storage device shown, the FIG. 14A to FIG. 14C Components having the same functions as the components of the storage device shown are denoted by the same reference numerals. For details of the storage cells 150a to 150d, reference can be made to the description of the storage cell 150 in <Configuration example 1 of storage device>.

[0434] like Fig.15A and Fig. 15B As shown in FIG. 1 , the conductive layer 260 used as the wiring WOL is respectively provided in the memory cell 150a and the memory cell 150b. Fig.15A As shown, one conductive layer 260 is provided in a manner shared between the memory cell 150a and the memory cell 150c, and another conductive layer 260 is provided in a manner shared between the memory cell 150b and the memory cell 150d. In addition, one conductive layer 240 serving as a part of the wiring BIL is provided in a manner shared between the memory cell 150a and the memory cell 150b. In other words, the conductive layer 240 is in contact with the oxide semiconductor layer 230 of the memory cell 150a and the oxide semiconductor layer 230 of the memory cell 150b. In addition, another conductive layer 240 is provided in a manner shared between the memory cell 150c and the memory cell 150d.

[0435] Here, Fig.15A and Fig. 15B The memory device shown includes a conductive layer 245 and a conductive layer 246 which are electrically connected to the memory cells 150a and 150b and serve as plugs (which may also be referred to as connection electrodes). The conductive layer 245 is disposed in openings formed in the insulating layers 140, 180, 130, and 280 and is in contact with the bottom surface of the conductive layer 240. In addition, the conductive layer 246 is disposed in openings formed in the insulating layers 285, 283, and 250 and is in contact with the top surface of the conductive layer 240. As the conductive layer 245 and the conductive layer 246, a conductive material that can be used for the conductive layer 240 can be used.

[0436] The conductive layers 245 and 246 are used as plugs or wirings for electrically connecting circuit elements, wirings, electrodes or terminals such as switches, transistors, capacitors, inductors, resistors and diodes with the memory cells 150a and 150b. For example, the following structure can be adopted: the conductive layer 245 and the conductive layer 246 are provided at Fig. 15B The sense amplifier (not shown) under the storage device shown is electrically connected, and the conductive layer 246 is connected to the Fig. 15BThe same memory device (not shown) as shown in the memory device is electrically connected. In this case, the conductive layer 245 and the conductive layer 246 are used as part of the wiring BIL. Fig. 15B By arranging a storage device above or below the storage device shown, the storage capacity per unit area can be increased.

[0437] In addition, the memory cell 150a and the memory cell 150b are linearly symmetrical with the perpendicular bisector of the dot-dash line A3-A4 as the axis of symmetry. Therefore, the transistor 200a and the transistor 200b are also arranged linearly symmetrically with the conductive layer 245 and the conductive layer 246 sandwiched therebetween. Here, the conductive layer 240 also serves as the other of the source electrode and the drain electrode of the transistor 200a and the other of the source electrode and the drain electrode of the transistor 200b. In addition, the transistor 200a and the transistor 200b share the conductive layer 245 and the conductive layer 246 used as the plug. In this way, by adopting the above structure as the connection relationship between the two transistors and the plug, a storage device that can achieve miniaturization or high integration can be provided.

[0438] In addition, the conductive layer 110 used as the wiring CAL may be provided in each of the memory cells 150a and 150b, or may be provided in both the memory cells 150a and 150b. Fig. 15B As shown, the conductive layer 110 is disposed in a manner separated from the conductive layer 245 to prevent the conductive layer 110 and the conductive layer 245 from being short-circuited.

[0439] also, Fig.16 In the Z direction, n layers (n is an integer greater than or equal to 3) are stacked. Fig.15A An example of four memory cells is shown. Fig.16 It is along Fig.15A A cross-sectional view along the dashed line A3-A4 is shown.

[0440] Fig.16 The storage device shown includes n-layer storage layers 160. Specifically, a storage layer 160[2] is disposed on the storage layer 160[1]. A (n-2)-layer storage layer is further disposed on the storage layer 160[2]. A storage layer 160[n] is disposed as the top layer. There is no particular limitation on the number of storage cells included in one storage layer 160, and more than two storage cells may be included. The storage cells included in the n-layer storage layer 160 are electrically connected to a sense amplifier (not shown) disposed under the n-layer storage layer 160 through conductive layers 245, 246, 247, 248, etc.

[0441] like Fig.16As shown, by stacking a plurality of memory cells, the cells can be integrated without increasing the occupied area of ​​the memory cell array. That is, a 3D memory cell array can be constructed.

[0442] Fig.17 An example of a cross-sectional structure of a memory device in which a layer including memory cells is stacked on a layer including a driver circuit including a sense amplifier.

[0443] exist Fig.17 In the embodiment, the memory cell 150 (the transistor 200 and the capacitor 100 ) is disposed above the transistor 300 .

[0444] The transistor 300 is one of the transistors included in the sense amplifier.

[0445] Fig.17 For the storage unit 150 shown, reference can be made to the description of the storage unit 150 in <Configuration example 1 of storage device>. Fig.17 The example in which the capacitor 100 includes a conductive layer 120a and a conductive layer 120b on the conductive layer 120a instead of the conductive layer 120 is shown. Here, as the conductive layer 120b, for example, a material that can be used for the conductive layer 220c can be used. Also, as the conductive layer 120a, for example, a material that can be used for the conductive layer 220a and the conductive layer 220b can be used. Fig.17 Although the example in which the oxide semiconductor layer 230 is in contact with the top surface of the conductive layer 120 a is shown, the oxide semiconductor layer 230 may not be in contact with the top surface of the conductive layer 120 a .

[0446] like Fig.17 As shown in FIG. 1 , the bit line can be shortened by adopting a structure in which the sense amplifier is provided so as to overlap the memory cell 150. As a result, the bit line capacitance is reduced, and high-speed driving of the memory device can be realized.

[0447] Fig.17 The memory device shown can correspond to the semiconductor device 900 described in Embodiment 3. Specifically, the transistor 300 corresponds to the transistor included in the sense amplifier 927 in the semiconductor device 900. In addition, the memory cell 150 corresponds to the memory cell 950.

[0448] The transistor 300 is provided on a substrate 311 and includes a conductive layer 316 used as a gate, an insulating layer 315 used as a gate insulator, a semiconductor region 313 formed by a portion of the substrate 311, and a low resistance region 314a and a low resistance region 314b used as a source region or a drain region. The transistor 300 may be a p-channel type or an n-channel type.

[0449] Here, in Fig.17In the transistor 300 shown, the semiconductor region 313 (a part of the substrate 311) forming the channel has a convex shape. In addition, a conductive layer 316 is provided in a manner that covers the side and top surfaces of the semiconductor region 313 via an insulating layer 315. In addition, a material that adjusts the work function can also be used for the conductive layer 316. Because the convex portion of the semiconductor substrate is utilized, this transistor 300 is also referred to as a FIN-type transistor. In addition, an insulating layer having a mask for forming a convex portion in a manner that contacts the upper surface of the convex portion can also be provided. In addition, although a portion of the semiconductor substrate is processed to form a convex portion is shown here, an SOI substrate can also be processed to form a semiconductor film having a convex portion.

[0450] Notice, Fig.17 The structure of the transistor 300 shown is just an example and is not limited to the above structure, and an appropriate transistor can be used according to the circuit structure or driving method.

[0451] A wiring layer including an interlayer film, wiring, and plugs may also be provided between each structure. In addition, the wiring layer may be provided in multiple layers according to the design. Here, in a conductive layer having the function of a plug or wiring, the same symbol is sometimes used to represent multiple structures. In addition, in this specification, wiring and a plug electrically connected to the wiring may also be a constituent element. That is, a part of the conductive layer is sometimes used as wiring, and a part of the conductive layer is sometimes used as a plug.

[0452] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are sequentially stacked as interlayer films over the transistor 300. Furthermore, a conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. Furthermore, the conductive layer 328 and the conductive layer 330 are used as plugs or wirings.

[0453] In addition, the insulating layer used as an interlayer film can be used as a planarization film to cover the concavo-convex shape thereunder. For example, in order to improve the flatness of the top surface of the insulating layer 322, the top surface can also be planarized by a planarization process using a CMP method or the like.

[0454] Alternatively, a wiring layer may be formed over the insulating layer 326 and the conductive layer 330. Fig.17 In the embodiment, an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. Furthermore, a conductive layer 356 is formed in the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 is used as a plug or a wiring.

[0455] As the insulating layer 352 and the insulating layer 354 which function as an interlayer film, the above-described insulating layers which can be used in a semiconductor device or a memory device can be used.

[0456] As the conductive layer used as a plug or wiring, for example, the conductive layer 328, the conductive layer 330, and the conductive layer 356, the conductive material that can be used for the conductive layer 240 can be used. It is preferable to use a high melting point material such as tungsten or molybdenum that has both heat resistance and conductivity, and tungsten is preferably used. Alternatively, it is preferable to form it using a low-resistance conductive material such as aluminum or copper. By using a low-resistance conductive material, the wiring resistance can be reduced.

[0457] The conductive layer 240 included in the transistor 200 is electrically connected to the low resistance region 314 b serving as a source region or a drain region of the transistor 300 through the conductive layers 643 , 642 , 644 , 645 , 646 , 356 , 330 , and 328 .

[0458] The conductive layer 643 is embedded in the insulating layer 280. The conductive layer 642 is provided on the insulating layer 130 and embedded in the insulating layer 641. The conductive layer 642 can be manufactured using the same material and process as the conductive layer 120a. The conductive layer 644 is embedded in the insulating layer 180 and the insulating layer 130. The conductive layer 645 is embedded in the insulating layer 647. The conductive layer 645 can be manufactured using the same material and process as the conductive layer 110. The conductive layer 646 is embedded in the insulating layer 648. The transistor 300 is electrically insulated from the conductive layer 110 by the insulating layer 648.

[0459] As described above, the memory device of this embodiment includes a transistor with reduced parasitic capacitance, so the operating speed can be increased. In addition, since the memory device of this embodiment has capacitors and transistors stacked, the area occupied by the memory cell when viewed from above can be reduced, thereby realizing a highly integrated memory device.

[0460] This embodiment mode can be combined with other embodiment modes as appropriate.

[0461] Implementation 3 In this embodiment, a semiconductor device 900 which is one embodiment of the present invention is described. The semiconductor device 900 can be used as a memory device.

[0462] Fig.18 is a block diagram showing a structural example of a semiconductor device 900 . Fig.18 The semiconductor device 900 shown includes a driving circuit 910 and a memory cell array 920. The memory cell array 920 includes one or more memory cells 950. Fig.18 An example is shown in which the memory cell array 920 includes a plurality of memory cells 950 arranged in a matrix.

[0463] As the storage unit 950 , the storage device described in Embodiment 2 (such as the storage unit 150 ) can be used.

[0464] The driving circuit 910 includes a PSW 931 (power switch), a PSW 932 , and a peripheral circuit 915 . The peripheral circuit 915 includes a peripheral circuit 911 , a control circuit 912 , and a voltage generating circuit 928 .

[0465] In the semiconductor device 900, the above-mentioned circuits, signals and voltages can be appropriately selected as needed. Alternatively, other circuits or other signals can be added. Signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1 and PON2 are signals input from the outside, and signal RDA is a signal output to the outside. Signal CLK is a clock signal.

[0466] In addition, the signal BW, the signal CE, and the signal GW are control signals. The signal CE is a chip enable signal, the signal GW is a global write enable signal, and the signal BW is a byte write enable signal. The signal ADDR is an address signal. The signal WDA is write data, and the signal RDA is read data. The signals PON1 and PON2 are power gating control signals. In addition, the signals PON1 and PON2 can also be generated in the control circuit 912.

[0467] The control circuit 912 is a logic circuit that has the function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logic operation on the signal CE, the signal GW, and the signal BW to determine the operation mode (for example, writing operation, reading operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 to execute the above operation mode.

[0468] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H level signal is applied to the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.

[0469] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cell 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.

[0470] The row decoder 941 and the column decoder 942 have the function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has the function of selecting a row to be connected to the row specified by the row decoder 941. The column driver 924 has the following functions: a function of writing data to the memory cell 950; a function of reading data from the memory cell 950; a function of holding the read data, etc.

[0471] The input circuit 925 has a function of holding a signal WDA. The data held in the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is the data (Din) written to the memory cell 950. The data (Dout) read out from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data signal output from the output circuit 926 is a signal RDA.

[0472] PSW931 has the function of controlling the supply of V to the peripheral circuit 915 DD PSW932 has the function of controlling the supply of V to the row driver 923. HM Here, the high power supply voltage of the semiconductor device 900 is V DD , the low power supply voltage is GND (ground potential). In addition, V HM It is a high power supply voltage used to make the word line high, which is higher than V DD The on / off of PSW931 is controlled by signal PON1, and the on / off of PSW932 is controlled by signal PON2. Fig.18 In the peripheral circuit 915, V DD The number of power domains is 1, but may be multiple. In this case, a power switch may be provided for each power domain.

[0473] Reference FIG. 19A to FIG. 19H An example of the structure of a memory cell which can be used for the memory cell 950 is described.

[0474] In the following, when two components are recorded as being connected, this includes the case where they are electrically connected through circuit elements (transistors, switches, diodes, resistors, etc.). Electrical connection refers to a state where it is possible for current to flow between two components. In addition, when two components are connected through a switch or transistor, it is also possible that current flows when the switch or transistor is in the on state, so it is included in the category of electrical connection.

[0475] [DOSRAM] Fig.19AAn example of a circuit structure of a DRAM type memory cell is shown. In this specification and the like, a DRAM using an OS transistor is referred to as a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 951 includes a transistor M1 and a capacitor CA.

[0476] The transistor M1 may include a front gate (sometimes simply referred to as a gate) and a back gate. In this case, the back gate may be connected to a wiring to which a constant potential or a signal is supplied, and the front gate and the back gate may be connected.

[0477] The first terminal of the transistor M1 is connected to the first terminal of the capacitor CA, the second terminal of the transistor M1 is connected to the wiring BIL, the gate of the transistor M1 is connected to the wiring WOL, and the second terminal of the capacitor CA is connected to the wiring CAL.

[0478] The wiring BIL is used as a bit line, and the wiring WOL is used as a word line. The wiring CAL is used as a wiring for applying a specified potential to the second terminal of the capacitor CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.

[0479] Data writing and reading are performed by applying a high-level potential to the wiring WOL to turn on the transistor M1 and thereby bring the wiring BIL and the first terminal of the capacitor CA into a conductive state (allowing current to flow).

[0480] In addition, the memory cell that can be used as the memory cell 950 is not limited to the memory cell 951, and the circuit structure can also be changed. Fig.19B The memory cell 952 is shown. The memory cell 952 is an example of a case where the capacitor CA and the wiring CAL are not included. The first terminal of the transistor M1 is in an electrically floating state.

[0481] In the memory cell 952, the potential written by the transistor M1 is held in the capacitance (also referred to as parasitic capacitance) between the first terminal and the gate indicated by the dotted line. By adopting this structure, the structure of the memory cell can be greatly simplified.

[0482] As transistor M1, it is preferred to use an OS transistor. OS transistors have the characteristic of extremely small off-state current. By using an OS transistor as transistor M1, the leakage current of transistor M1 can be made very low. In other words, transistor M1 can be used to maintain written data for a long time, thereby reducing the refresh frequency of the memory cell. In addition, the refresh operation of the memory cell can be omitted. In addition, since the leakage current is very low, multi-value data or analog data can be maintained in the memory cell 951 and the memory cell 952.

[0483] [NOSRAM] Fig.19C An example of a circuit structure of a gain unit type memory cell including two transistors and one capacitor is shown. The memory cell 953 includes a transistor M2, a transistor M3, and a capacitor CB. In this specification, etc., a memory device including a gain unit type memory cell using an OS transistor for the transistor M2 is sometimes referred to as a NOSRAM (Nonvolatile Oxide Semiconductor RAM: oxide semiconductor nonvolatile random access memory).

[0484] The first terminal of the transistor M2 is connected to the first terminal of the capacitor CB, the second terminal of the transistor M2 is connected to the wiring WBL, and the gate of the transistor M2 is connected to the wiring WOL. The second terminal of the capacitor CB is connected to the wiring CAL. The first terminal of the transistor M3 is connected to the wiring RBL, the second terminal of the transistor M3 is connected to the wiring SL, and the gate of the transistor M3 is connected to the first terminal of the capacitor CB.

[0485] The wiring WBL is used as a write bit line, the wiring RBL is used as a read bit line, and the wiring WOL is used as a word line. The wiring CAL is used as a wiring for applying a predetermined potential to the second terminal of the capacitor CB. When writing data, when holding data, and when reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.

[0486] Data is written by applying a high-level potential to the wiring WOL to turn on the transistor M2 and to turn on the wiring WBL and the first terminal of the capacitor CB. Specifically, when the transistor M2 is in the on state, a potential corresponding to the information to be recorded is applied to the wiring WBL to write the potential to the first terminal of the capacitor CB and the gate of the transistor M3. Then, a low-level potential is applied to the wiring WOL to turn off the transistor M2, thereby maintaining the potential of the first terminal of the capacitor CB and the potential of the gate of the transistor M3.

[0487] Data is read by applying a predetermined potential to the wiring SL. Since the current flowing between the source and drain of the transistor M3 and the potential of the first terminal of the transistor M3 are determined by the potential of the gate of the transistor M3 and the potential of the second terminal of the transistor M3, the potential held by the first terminal of the capacitor CB (or the gate of the transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of the transistor M3. In other words, the information written in the storage unit can be read from the potential held by the first terminal of the capacitor CB (or the gate of the transistor M3).

[0488] For example, a structure in which the wiring WBL and the wiring RBL are combined into one wiring BIL may be employed. Fig.19D An example of the circuit structure of the memory cell in this case is shown. In the memory cell 954, the wiring WBL and the wiring RBL of the memory cell 953 are combined into one wiring BIL, and the second terminal of the transistor M2 and the first terminal of the transistor M3 are connected to the wiring BIL. In other words, the memory cell 954 operates by combining the write bit line and the read bit line into one wiring BIL.

[0489] Fig.19E The memory cell 955 shown is an example of a case where the capacitor CB and the wiring CAL in the memory cell 953 are omitted. Fig.19F The memory cell 956 shown is an example in which the capacitor CB and the wiring CAL in the memory cell 954 are omitted. By adopting such a structure, the integration degree of the memory cell can be increased.

[0490] Note that it is preferable to use an OS transistor as at least the transistor M2. In particular, it is preferable to use an OS transistor as the transistor M2 and the transistor M3.

[0491] Since the OS transistor has a very small off-state current, the transistor M2 can be used to maintain the written data for a long time, thereby reducing the refresh frequency of the memory cell. In addition, the refresh operation of the memory cell can be omitted. In addition, since the leakage current is very low, multi-value data or analog data can be maintained in the memory cells 953, 954, 955, and 956.

[0492] The memory cells 953 , 954 , 955 , and 956 using OS transistors as the transistors M2 are one embodiment of NOSRAM.

[0493] A Si transistor may be used as the transistor M3. A Si transistor can improve field effect mobility and can be a p-channel transistor, so the degree of freedom in circuit design can be increased.

[0494] Furthermore, when an OS transistor is used as the transistor M3, the memory cell can be formed of a unipolar circuit.

[0495] also, Figure 19G A gain unit type memory cell 957 of 3 transistors and 1 capacitor is shown. The memory cell 957 includes transistors M4 to M6 and a capacitor CC.

[0496] The first terminal of transistor M4 is connected to the first terminal of capacitor CC, the second terminal of transistor M4 is connected to wiring BIL, and the gate of transistor M4 is connected to wiring WOL. The second terminal of capacitor CC is connected to the first terminal of transistor M5 and wiring GNDL. The second terminal of transistor M5 is connected to the first terminal of transistor M6, and the gate of transistor M5 is connected to the first terminal of capacitor CC. The second terminal of transistor M6 is connected to wiring BIL, and the gate of transistor M6 is connected to wiring RWL.

[0497] The wiring BIL is used as a bit line, the wiring WOL is used as a write word line, and the wiring RWL is used as a read word line. The wiring GNDL is a wiring for supplying a low-level potential.

[0498] Data is written by applying a high-level potential to the wiring WOL to turn on the transistor M4 and to turn on the wiring BIL and the first terminal of the capacitor CC. Specifically, when the transistor M4 is in the on state, a potential corresponding to the information to be recorded is applied to the wiring BIL to write the potential to the first terminal of the capacitor CC and the gate of the transistor M5. Then, a low-level potential is applied to the wiring WOL to turn off the transistor M4, thereby maintaining the potential of the first terminal of the capacitor CC and the potential of the gate of the transistor M5.

[0499] The data is read out by precharging the wiring BIL to a predetermined potential, then making the wiring BIL electrically floating and applying a high level potential to the wiring RWL. By making the wiring RWL a high level potential, the transistor M6 is turned on, and the wiring BIL and the second terminal of the transistor M5 are turned on. At this time, the potential of the wiring BIL is applied to the second terminal of the transistor M5, but the potential of the second terminal of the transistor M5 and the potential of the wiring BIL will change in accordance with the potential maintained by the first terminal of the capacitor CC (or the gate of the transistor M5). Here, the potential maintained by the first terminal of the capacitor CC (or the gate of the transistor M5) can be read out by reading out the potential of the wiring BIL. In other words, the information written into the storage cell can be read out from the potential maintained by the first terminal of the capacitor CC (or the gate of the transistor M5).

[0500] Note that an OS transistor is preferably used as at least the transistor M4.

[0501] Si transistors may be used as the transistors M5 and M6. As described above, the field effect mobility of the Si transistor may be higher than that of the OS transistor depending on the crystal state of silicon used for the semiconductor layer and the like.

[0502] Furthermore, when OS transistors are used as the transistors M5 and M6, the memory cell can be formed of a unipolar circuit.

[0503] [OS-SRAM] Fig.19H An example of an SRAM (Static Random Access Memory) using an OS transistor is shown. In this specification, etc., an SRAM using an OS transistor is referred to as an OS-SRAM (Oxide Semiconductor-SRAM). Fig.19H The memory cell 958 shown is a SRAM type memory cell capable of backup.

[0504] The memory cell 958 includes transistors M7 to M10, transistors MS1 to MS4, capacitors CD1 and CD2. The transistors MS1 and MS2 are p-channel transistors, and the transistors MS3 and MS4 are n-channel transistors.

[0505] The first terminal of the transistor M7 is connected to the wiring BIL, and the second terminal of the transistor M7 is connected to the first terminal of the transistor MS1, the first terminal of the transistor MS3, the gate of the transistor MS2, the gate of the transistor MS4, and the first terminal of the transistor M10. The gate of the transistor M7 is connected to the wiring WOL. The first terminal of the transistor M8 is connected to the wiring BILB, and the second terminal of the transistor M8 is connected to the first terminal of the transistor MS2, the first terminal of the transistor MS4, the gate of the transistor MS1, the gate of the transistor MS3, and the first terminal of the transistor M9. The gate of the transistor M8 is connected to the wiring WOL.

[0506] The second terminal of the transistor MS1 is connected to the wiring VDL. The second terminal of the transistor MS2 is connected to the wiring VDL. The second terminal of the transistor MS3 is connected to the wiring GNDL. The second terminal of the transistor MS4 is connected to the wiring GNDL.

[0507] The second terminal of the transistor M9 is connected to the first terminal of the capacitor CD1, and the gate of the transistor M9 is connected to the wiring BRL. The second terminal of the transistor M10 is connected to the first terminal of the capacitor CD2, and the gate of the transistor M10 is connected to the wiring BRL.

[0508] A second terminal of the capacitor CD1 is connected to the wiring GNDL, and a second terminal of the capacitor CD2 is connected to the wiring GNDL.

[0509] The wiring BIL and the wiring BILB are used as bit lines, the wiring WOL is used as a word line, and the wiring BRL is a wiring for controlling the on state and the off state of the transistor M9 and the transistor M10.

[0510] The wiring VDL is a wiring for supplying a high-level potential, and the wiring GNDL is a wiring for supplying a low-level potential.

[0511] Data is written by applying a high level potential to the wiring WOL and a high level potential to the wiring BRL. Specifically, when the transistor M10 is turned on, a potential corresponding to the information to be recorded is applied to the wiring BIL and written to the second terminal side of the transistor M10.

[0512] The storage unit 958 uses transistors MS1 to MS2 to form an inverter loop, so the inverted signal of the data signal corresponding to the potential is input to the second terminal side of the transistor M8. Since the transistor M8 is in the on state, the potential applied to the wiring BIL, that is, the inverted signal of the signal input to the wiring BIL is output to the wiring BILB. In addition, since the transistors M9 and M10 are in the on state, the potential of the second terminal of the transistor M7 and the potential of the second terminal of the transistor M8 are respectively maintained by the first terminal of the capacitor CD2 and the first terminal of the capacitor CD1. Then, by applying a low-level potential to the wiring WOL and applying a low-level potential to the wiring BRL to turn off the transistors M7 to M10, the potential of the first terminal of the capacitor CD1 and the potential of the first terminal of the capacitor CD2 are maintained.

[0513] Data is read out by the following method: first, after precharging the wiring BIL and the wiring BILB to a predetermined potential, a high-level potential is applied to the wiring WOL and a high-level potential is applied to the wiring BRL, whereby the potential of the first terminal of the capacitor CD1 is refreshed by the inverter loop of the storage unit 958 and output to the wiring BILB. In addition, the potential of the first terminal of the capacitor CD2 is refreshed by the inverter loop of the storage unit 958 and output to the wiring BIL. Since the wiring BIL and the wiring BILB are changed from the precharged potential to the potential of the first terminal of the capacitor CD2 and the potential of the first terminal of the capacitor CD1, respectively, the potential held by the storage unit can be read from the potential of the wiring BIL or the wiring BILB.

[0514] The transistors M7 to M10 are preferably OS transistors. Thus, the transistors M7 to M10 can be used to hold the written data for a long time, thereby reducing the refresh frequency of the memory cell. Alternatively, the refresh operation of the memory cell can be omitted.

[0515] In addition, Si transistors are preferably used as the transistors MS1 to MS4.

[0516] The driving circuit 910 and the memory cell array 920 of the semiconductor device 900 are arranged on the same plane. Fig. 20AAs shown, the driving circuit 910 and the memory cell array 920 may also overlap. By overlapping the driving circuit 910 and the memory cell array 920, the signal transmission distance can be shortened. Fig. 20B As shown, a plurality of memory cell arrays 920 may be stacked on the driving circuit 910 .

[0517] Next, an example of a calculation processing device that may include a semiconductor device such as the above-mentioned storage device will be described.

[0518] Fig.21 It is a block diagram of the computing device 960 . Fig.21 The computing device 960 shown can be used, for example, for a CPU (Central Processing Unit). In addition, the computing device 960 can also be used for a processor such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), or an NPU (Neural Processing Unit) that includes more (tens or hundreds) processor cores capable of parallel processing than a CPU.

[0519] Fig.21 The computing device 960 shown has an ALU 991 (ALU: Arithmetic logic unit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. A semiconductor substrate, an SOI substrate, a glass substrate, etc. can be used as the substrate 990. A rewritable ROM and a ROM interface can also be included. The cache 999 and the cache interface 989 can also be set on different chips.

[0520] The cache memory 999 is connected to a main memory provided on a different chip via a cache interface 989. The cache interface 989 has a function of supplying a part of the data stored in the main memory to the cache memory 999. In addition, the cache interface 989 has a function of outputting a part of the data held in the cache memory 999 to the ALU 991, the register 996, or the like via a bus interface 998.

[0521] As described later, the memory cell array 920 may be provided in a stacked manner on the computing device 960. The memory cell array 920 may be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory cell array 920 to the cache 999. In addition, in this case, it is preferable that a driving circuit 910 is included in a portion of the cache interface 989.

[0522] Note that the cache memory 999 may not be provided and only the memory cell array 920 may be used as a cache memory.

[0523] Fig.21 The computing device 960 shown is only an example of a simplified structure, so the actual computing device 960 has various structures depending on its use. For example, it is preferable to use a computing device including Fig.21 The structure of the computing device 960 shown is a so-called multi-core structure in which one core is provided with a plurality of the cores and the cores are made to work simultaneously. The more cores there are, the higher the computing performance can be. The more cores there are, the more preferred it is, for example, preferably 2, more preferably 4, further preferably 8, further preferably 12, and further preferably 16 or more. In addition, when very high computing performance is required, such as when used in a server, it is preferred to adopt a multi-core structure including 16 or more cores, preferably 32 or more, and more preferably 64 or more cores. In addition, the number of bits that can be processed in the internal computing circuit, data bus, etc. of the computing device 960 can be, for example, 8 bits, 16 bits, 32 bits, 64 bits, etc.

[0524] The instructions input to the operation device 960 through the bus interface 998 are input to the instruction decoder 993 and decoded, and then input to the ALU controller 992, the interrupt controller 994, the register controller 997, and the timing controller 995.

[0525] The ALU controller 992, the interrupt controller 994, the register controller 997, and the timing controller 995 perform various controls according to the decoded instructions. Specifically, the ALU controller 992 generates a signal for controlling the operation of the ALU 991. In addition, when executing the program of the computing device 960, the interrupt controller 994 determines the interrupt request from the external input / output device, peripheral circuit, etc. according to its priority, mask status, etc. and processes the request. The register controller 997 generates the address of the register 996 and reads and writes the register 996 according to the state of the computing device 960.

[0526] In addition, the timing controller 995 generates signals for controlling the operation timing of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 has an internal clock generator that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the above-mentioned various circuits.

[0527] exist Fig.21In the illustrated operation device 960, the register controller 997 selects the holding operation in the register 996 according to the instruction of the ALU 991. In other words, the register controller 997 selects whether the data is held by the flip-flop or by the capacitor in the storage unit of the register 996. When the flip-flop is selected to hold the data, the power supply potential is supplied to the storage unit in the register 996. When the capacitor is selected to hold the data, the data is rewritten to the capacitor, and the supply of the power supply potential to the storage unit in the register 996 can be stopped.

[0528] The memory cell array 920 and the computing device 960 may be arranged to overlap. Fig.22A and Fig. 22B 970A. The semiconductor device 970A includes a layer 930 on which a memory cell array is disposed on a computing device 960. The layer 930 includes a memory cell array 920L1, a memory cell array 920L2, and a memory cell array 920L3. The computing device 960 and the memory cell arrays have overlapping regions. Fig. 22B The computing device 960 and the layer 930 are shown separately in FIG.

[0529] By overlapping the layer 930 including the memory cell array and the computing device 960, the connection distance between the two can be shortened. Thus, the communication speed between the two can be increased. In addition, since the connection distance is short, power consumption can be reduced.

[0530] As a stacking method of the layer 930 including the memory cell array and the computing device 960, the following methods can be adopted: directly stacking the layer 930 including the memory cell array on the computing device 960 (also called monolithic stacking); or forming the computing device 960 and the layer 930 on different substrates, bonding the two substrates together, and electrically connecting them using a perforated or conductive film bonding technology (Cu-Cu bonding, etc.). In the former method, there is no need to consider the misalignment during bonding, so it is possible to reduce the chip size and manufacturing cost.

[0531] Here, the storage cell arrays 920L1, 920L2, and 920L3 that do not include the cache 999 in the computing device 960 and are disposed in the layer 930 can all be used as caches. At this time, for example, the storage cell array 920L1, the storage cell array 920L2, and the storage cell array 920L3 can be used as L1 cache (also called first-level cache), L2 cache (also called second-level cache), and L3 cache (also called third-level cache), respectively. Among the three storage cell arrays, the storage cell array 920L3 has the largest capacity and the lowest access frequency. In addition, the storage cell array 920L1 has the smallest capacity and the highest access frequency.

[0532] Note that when the cache 999 provided in the computing device 960 is used as an L1 cache, each memory cell array provided in the layer 930 can be used as a lower level cache or a main memory. The main memory is a memory having a larger capacity and a lower access frequency than the cache.

[0533] In addition, if Fig. 22B As shown, a driving circuit 910L1, a driving circuit 910L2, and a driving circuit 910L3 are provided. The driving circuit 910L1 is connected to the memory cell array 920L1 via the connecting electrode 940L1. Similarly, the driving circuit 910L2 is connected to the memory cell array 920L2 via the connecting electrode 940L2, and the driving circuit 910L3 is connected to the memory cell array 920L3 via the connecting electrode 940L3.

[0534] Note that although the case where three memory cell arrays are used as a cache is shown here, the number may be one, two, or four or more.

[0535] When the memory cell array 920L1 is used as a cache, the driver circuit 910L1 may also be used as a part of the cache interface 989, and the driver circuit 910L1 may also be connected to the cache interface 989. Similarly, the driver circuit 910L2 and the driver circuit 910L3 may also be used as a part of the cache interface 989 or connected to a part of the cache interface 989.

[0536] Whether the memory cell array 920 is used as a cache or a main memory depends on the control circuit 912 included in each driver circuit 910. The control circuit 912 can use part of the plurality of memory cells 950 included in the semiconductor device 900 as a RAM according to a signal supplied from the operation device 960.

[0537] In the semiconductor device 900, part of the plurality of storage units 950 can be used as a cache and the other part can be used as a main memory. That is, the semiconductor device 900 can have a function as a cache and a function as a main memory. The semiconductor device 900 according to one embodiment of the present invention can be used as a general-purpose memory, for example.

[0538] Alternatively, a layer 930 including one memory cell array 920 may be provided so as to overlap with the computing device 960 . Fig.23A It is a perspective view of the semiconductor device 970B.

[0539] In the semiconductor device 970B, one memory cell array 920 can be divided into a plurality of regions and different functions can be assigned to the regions for use. Fig.23A An example is shown in which the area L1, the area L2, and the area L3 are used as an L1 cache, an L2 cache, and an L3 cache, respectively.

[0540] In addition, in the semiconductor device 970B, the capacity of each of the regions L1 to L3 can be changed according to the situation. For example, the capacity of the L1 cache can be increased by increasing the area of ​​the region L1. By adopting this structure, the efficiency of the operation processing can be improved and the processing speed can be increased.

[0541] Alternatively, a plurality of memory cell arrays may be stacked. Fig. 23B It is a perspective view of a semiconductor device 970C.

[0542] The semiconductor device 970C is stacked with a layer 930L1 including a memory cell array 920L1, a layer 930L2 including a memory cell array 920L2 thereon, and a layer 930L3 including a memory cell array 920L3 thereon. The memory cell array 920L1 physically closest to the computing device 960 can be used as an upper cache and the memory cell array 920L3 farthest from the computing device 960 can be used as a lower cache or a main memory. By adopting this structure, the capacity of each memory cell array can be increased, and thus the processing capability can be further improved.

[0543] This embodiment mode can be combined with other embodiment modes as appropriate.

[0544] Implementation 4 In this embodiment, an application example of a storage device which is one embodiment of the present invention will be described.

[0545] Generally speaking, in semiconductor devices such as computers, various storage devices are used according to their uses. Fig.24AVarious storage devices used in semiconductor devices are shown in a hierarchical manner. The higher the storage device, the faster the operating speed is required, and the lower the storage device, the larger the storage capacity and the higher the recording density is required. Fig.24A In the example, from the top layer, it includes a memory installed together as a register in a CPU or other arithmetic processing device, an L1 cache, an L2 cache, an L3 cache, a main memory, storage, etc. Note that although an example including up to the L3 cache is shown here, a cache at a lower level may also be included.

[0546] Since the memory installed together with the register in the CPU and other processing devices is used for temporary storage of the calculation results, the access frequency from the processing devices is high. Therefore, the operation speed is required to be faster than the storage capacity. In addition, the register has the function of holding the setting information of the processing device.

[0547] The cache has the function of copying and retaining part of the information held in the main memory. By copying frequently used data to the cache, the speed of accessing the data can be increased. The storage capacity required for the cache is less than that of the main memory, but the operating speed required for the cache is higher than that of the main memory. In addition, the data rewritten in the cache is copied and supplied to the main memory.

[0548] The main memory has a function of holding programs, data, and the like read from the storage.

[0549] Storage has the function of keeping data that needs to be stored for a long time and various programs used by the computing processing device. Therefore, compared with a faster working speed, storage is required to have a larger storage capacity and a higher recording density. For example, a large-capacity non-volatile storage device such as 3D NAND can be used.

[0550] A storage device (OS memory) using an oxide semiconductor according to one embodiment of the present invention has a high operating speed and can retain data for a long period of time. Fig.24A As shown, the storage device according to one embodiment of the present invention can be used in both the hierarchy including the cache and the hierarchy including the main memory. In addition, the storage device according to one embodiment of the present invention can also be used in the hierarchy including the storage.

[0551] As the OS memory, the above-mentioned DOSRAM, NOSRAM, and OS-SRAM can be used appropriately.

[0552] In addition, caches in these memories are required to work faster.

[0553] On the other hand, since the capacity of the main memory is larger than that of the cache, the storage element used for the main memory preferably has a structure that further reduces power consumption. The OS memory of one embodiment of the present invention can realize a memory with a longer retention time by utilizing the characteristics of the extremely small off-state current of the OS transistor. By using the OS memory as the main memory, a longer retention time can be achieved, thereby reducing the power consumption of the storage device. As the main memory, for example, a DOSRAM with an operating speed of less than 15ns and a long retention time can be used. In a DRAM composed of transistors using silicon, the retention time is about 64ms (milliseconds). In a DOSRAM using an OS transistor, a retention time of about 10 times can be achieved. By extending the retention time, the refresh frequency can be reduced, and the power consumption of the storage device can be reduced. By setting the write time and read time of the DOSRAM to less than 15ns (nanoseconds), it can be appropriately used as a main memory. In addition, the retention time of the DOSRAM is preferably more than 0.64s (seconds). The write time and read time of the DOSRAM of one embodiment of the present invention are preferably less than 15ns. In addition, at least one of the write time and the read time of the DOSRAM of one embodiment of the present invention is, for example, greater than 1ns and less than 15ns. Or, for example, greater than 2ns and less than 15ns. In addition, the retention time of the DOSRAM of one embodiment of the present invention is preferably greater than 0.16s, more preferably greater than 0.32s, and further preferably greater than 0.64s. In addition, the memory preferably operates in an ambient temperature range of, for example, greater than -40°C and less than 110°C.

[0554] In OS memory, by using Figures 1A to 1C and FIG. 2A to FIG. 2C The transistor shown in the figure can further reduce the occupied area of ​​the transistor compared to the case of using a planar transistor, and by using FIG. 14A to FIG. 14C , Fig.15A and Fig. 15B The structure of the DOSRAM shown in FIG. 1 can stack transistors on capacitors, thereby enabling high-density configuration of memory cells. In addition, by using OS transistors, high-speed operation and long-term data retention can be achieved.

[0555] also, Fig. 24B An example is shown in which an SRAM is used for a part of the cache and an OS memory according to one embodiment of the present invention is used for the other part.

[0556] The cache at the lowest level can be called LLC (Last Level Cache). LLC does not need to work faster than the cache above it, but is required to have a larger storage capacity. The OS memory of one embodiment of the present invention has a fast working speed and can retain data for a long time, so it can be suitable for LLC. Note that the OS memory of one embodiment of the present invention can also be used for FLC (Final Level Cache).

[0557] For example, Fig. 24B As shown, SRAM can be used for upper cache (L1 cache, L2 cache, etc.) and the OS memory of one embodiment of the present invention can be used for LLC. Fig. 24B As shown, in the main memory, DRAM can be used in addition to the OS memory.

[0558] This embodiment mode can be combined with other embodiment modes as appropriate.

[0559] Implementation method 5 In this embodiment, a display device which is one embodiment of the present invention is described.

[0560] A semiconductor device of one embodiment of the present invention can be used in a display device or a module including the display device. As a module including the display device, there can be cited a module in which the display device is equipped with a connector such as a flexible printed circuit (Flexible printed circuit, hereinafter referred to as FPC) or TCP (Tape Carrier Package), a module in which an integrated circuit (IC) is installed by a COG (Chip On Glass) method or a COF (Chip On Film) method, etc.

[0561] The display device of this embodiment may also have a touch panel function. For example, various detection elements (also referred to as sensor elements) that can detect the approach or contact of a detection object such as a finger may be used in the display device.

[0562] For example, as the type of sensor, there are electrostatic capacitance type, resistance film type, surface acoustic wave type, infrared type, optical type, and pressure sensitive type.

[0563] As the electrostatic capacitance type, for example, there are surface type electrostatic capacitance type, projected type electrostatic capacitance type, etc. In addition, as the projected type electrostatic capacitance type, for example, there are self capacitance type, mutual capacitance type, etc. It is preferable to use the mutual capacitance type, which can perform multi-point detection at the same time.

[0564] Examples of touch panels include out-cell, on-cell, and in-cell types. Note that an in-cell touch panel has a structure in which electrodes constituting a detection element are provided on one or both of a substrate supporting a display element and a counter substrate.

[0565] [Display module] Fig.25A 1 is a perspective view of the display module 170. The display module 170 includes a display device 600A and an FPC 298. Note that the display device included in the display module 170 is not limited to the display device 600A, and may be a display device 600B described later.

[0566] The display module 170 includes a substrate 291 and a substrate 299. The display module 170 includes a display portion 297. The display portion 297 is an image display region in the display module 170, and light from each pixel provided in a pixel portion 294 described below can be viewed.

[0567] Fig.25B 2 is a perspective view of a structure on one side of a substrate 291. A circuit portion 292, a pixel circuit portion 293 on the circuit portion 292, and a pixel portion 294 on the pixel circuit portion 293 are stacked on the substrate 291. In addition, a terminal portion 295 for connecting to an FPC 298 is provided on a portion of the substrate 291 that does not overlap with the pixel portion 294. The terminal portion 295 is electrically connected to the circuit portion 292 via a wiring portion 296 composed of a plurality of wirings.

[0568] The semiconductor device of one embodiment of the present invention can be applied to one or both of the circuit portion 292 and the pixel circuit portion 293 .

[0569] The pixel portion 294 includes a plurality of pixels 294 a arranged periodically. Fig.25B An enlarged view of one pixel 294a is shown on the right side of FIG. Fig.25B An example is shown in which one pixel 294 a includes a sub-pixel 130R that emits red light, a sub-pixel 130G that emits green light, and a sub-pixel 130B that emits blue light.

[0570] The sub-pixel includes a display element. Various elements can be used as the display element, for example, a liquid crystal element and a light-emitting element. In addition, MEMS (Micro ElectroMechanical Systems) elements using a shutter method or an optical interference method, display elements using a microcapsule method, an electrophoresis method, an electrowetting method, or an electronic powder fluid (registered trademark) method, etc. can also be used. In addition, QLED (Quantum-dot LED: quantum dot LED) using a light source and color conversion technology using quantum dot materials can also be used.

[0571] Examples of the light emitting element include self-luminous light emitting elements such as LED (Light Emitting Diode), OLED (Organic LED), and semiconductor lasers. Examples of the LED include Mini LED and Micro LED.

[0572] There is no particular limitation on the arrangement of pixels in the display device of this embodiment, and various methods can be used. Examples of pixel arrangements include stripe arrangement, S-stripe arrangement, matrix arrangement, Delta arrangement, Bayer arrangement, and Pentile arrangement. Fig.25B An example is shown in which the pixels are arranged in a stripe arrangement.

[0573] The pixel circuit portion 293 includes a plurality of pixel circuits 293 a arranged periodically.

[0574] One pixel circuit 293a controls the driving of multiple elements included in one pixel 294a. Three circuits for controlling the light emission of one light emitting element may be provided in one pixel circuit 293a. For example, the pixel circuit 293a may adopt a structure having at least one selection transistor, one current control transistor (driving transistor) and a capacitor for one light emitting element. At this time, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. Thus, an active matrix display device is realized.

[0575] The circuit unit 292 includes a circuit for driving each pixel circuit 293a of the pixel circuit unit 293. For example, it preferably includes one or both of a gate line driving circuit and a source line driving circuit. In addition, it may include at least one of a calculation circuit, a storage circuit, and a power supply circuit.

[0576] The FPC 298 is used as wiring for supplying video signals, power supply potential, etc. from the outside to the circuit portion 292. In addition, an IC may be mounted on the FPC 298.

[0577] The display module 170 can adopt a structure in which one or both of the pixel circuit unit 293 and the circuit unit 292 are overlapped and arranged on the lower side of the pixel unit 294, so that the display unit 297 can have an extremely high aperture ratio (effective display area ratio). In addition, the pixels 294a can be arranged at an extremely high density, thereby making the display unit 297 have an extremely high definition.

[0578] This high-definition display module 170 is suitable for use in VR devices such as HMD or glasses-type AR devices. For example, because the display module 170 has an extremely high-definition display unit 297, in the structure of viewing the display unit of the display module 170 through a lens, even if the display unit is magnified by a lens, the user cannot see the pixels, thereby achieving a highly immersive display. In addition, the display module 170 can also be applied to electronic devices with a relatively small display unit. For example, it is suitable for use in the display unit of wearable electronic devices such as watch-type devices.

[0579] [Configuration Example 1 of Display Device] Fig.26 2 is a cross-sectional view of a display device 600A. The display device 600A is an example of a display device using an MML (Metal Mask Less) structure. That is, the display device 600A includes a light-emitting element that is not manufactured using a high-definition metal mask.

[0580] The island-shaped light-emitting layer in the light-emitting element included in the display device using the MML structure is formed by depositing the light-emitting layer on the entire surface and then processing it using photolithography. Therefore, a high-definition display device or a display device with a high aperture ratio that has been difficult to achieve so far can be realized. Furthermore, since the light-emitting layer can be formed separately for each color, a display device with extremely bright, high contrast and high display quality can be realized. For example, when a display device is composed of three types of light-emitting elements that emit blue light, light-emitting elements that emit green light and light-emitting elements that emit red light, three types of island-shaped light-emitting layers can be formed by repeatedly forming the light-emitting layer three times and processing using photolithography.

[0581] Since the device having the MML structure can be manufactured without using a metal mask, the upper limit of the clarity caused by the alignment accuracy of the metal mask can be exceeded. In addition, when the device is manufactured without using a metal mask, the equipment related to the manufacture of the metal mask and the cleaning process of the metal mask can be unnecessary. In addition, in the processing using photolithography, the same or common equipment as the equipment used in the manufacture of transistors can be used, so there is no need to introduce special equipment for the manufacture of devices having the MML structure. In this way, with the help of the MML structure, the manufacturing cost can be reduced, so it is suitable for mass production of devices.

[0582] In a display device having an MML structure, for example, there is no need to adopt a special pixel arrangement such as a Pentile arrangement to improve clarity in a pseudo manner, thereby realizing a display device in which the so-called stripe arrangement in which the R, G, and B sub-pixels are arranged in one direction is adopted and the clarity is high (for example, above 500ppi, above 1000ppi, above 2000ppi, above 3000ppi or above 5000ppi).

[0583] In addition, by providing a sacrificial layer on the light-emitting layer, damage to the light-emitting layer during the manufacturing process of the display device can be reduced, thereby improving the reliability of the light-emitting element. The sacrificial layer can remain in the completed display device or be removed during the manufacturing process. For example, Fig.26 and Fig. 27 The illustrated sacrificial layer 618a is a portion of a sacrificial layer disposed on the light emitting layer.

[0584] Furthermore, by adopting a deposition step using a range mask and a processing step using a resist mask, a light-emitting element can be manufactured using a relatively simple process.

[0585] Fig.26 FIG. 4 is a schematic cross-sectional view of a display device 600A (semiconductor device) according to one embodiment of the present invention. In the display device 600A, a pixel circuit, a driving circuit, and the like are provided on a substrate 410. Fig.26 In the display device 600A, in addition to the element layer 620, the element layer 630, and the element layer 660, a wiring layer 670 is shown. The wiring layer 670 is a layer provided with wiring.

[0586] The pixel circuit of the display device is preferably provided in the element layer 630. The driving circuit of the display device (one or both of the gate driver and the source driver) is preferably provided in the element layer 620. In addition, one or more of various circuits such as an operation circuit and a storage circuit may also be provided in the element layer 620.

[0587] As an example, the element layer 620 includes a substrate 410, on which a transistor 400d is formed. In addition, a wiring layer 670 is provided above the transistor 400d, and a conductive layer or transistor provided in the element layer 630 is provided in the wiring layer 670 ( Fig.26 In addition, the wiring layer 670 is provided with the element layer 630 and the element layer 660, and the element layer 630 includes, for example, the transistor MTCK, etc. The element layer 660 includes the light emitting element 650 ( Fig.26 The light-emitting element 650R, the light-emitting element 650G and the light-emitting element 650B) etc.

[0588] The transistor 400d is an example of a transistor included in the element layer 620. The transistor MTCK is an example of a transistor included in the element layer 630. The light-emitting elements (the light-emitting element 650R, the light-emitting element 650G, and the light-emitting element 650B) are examples of light-emitting elements included in the element layer 660.

[0589] As the transistor MTCK, for example, an OS transistor can be used. Fig.26An example in which the transistor 200 described in the above embodiment is used as the transistor MTCK is shown.

[0590] As the substrate 410, for example, a semiconductor substrate (for example, a single crystal substrate made of silicon or germanium) can be used. In addition, as the substrate 410, in addition to the semiconductor substrate, for example, an SOI (Silicon On Insulator) substrate, a glass substrate, a quartz substrate, a plastic substrate, a sapphire glass substrate, a metal substrate, a stainless steel substrate, a substrate including a stainless steel foil, a tungsten substrate, a substrate including a tungsten foil, a flexible substrate, a laminated film, paper including a fibrous material, or a base film can be used. In this embodiment, the case where the substrate 410 is a semiconductor substrate including silicon as a material is described. Therefore, the transistor in the element layer 620 can be a Si transistor.

[0591] The transistor 400d includes an element isolation layer 412, a conductive layer 416, an insulating layer 415, an insulating layer 417, a semiconductor region 413 formed by a portion of the substrate 410, a low resistance region 414a serving as a source region or a drain region, and a low resistance region 414b. Therefore, the transistor 400d is a Si transistor. Fig.26 In the illustrated structure, the source or drain of the transistor 400d is electrically connected to the conductive layer 514 provided in the element layer 630 through the conductive layer 428, the conductive layer 430, and the conductive layer 456; however, the electrical connection structure of the display device of one embodiment of the present invention is not limited thereto.

[0592] The transistor 400d can realize a Fin-type structure by, for example, adopting a structure in which the top surface of the semiconductor region 413 and the side surface in the channel width direction are covered by a conductive layer 416 via an insulating layer 415 used as a gate insulating layer. By forming the Fin-type transistor 400d, the effective channel width can be increased, so the on-state characteristics of the transistor 400d can be improved. In addition, since the effect of the electric field of the gate electrode can be enhanced, the off-state characteristics of the transistor 400d can be improved. In addition, the transistor 400d can also have a planar structure instead of a Fin-type structure.

[0593] The transistor 400d may be a p-channel transistor or an n-channel transistor. A plurality of transistors 400d may be provided, and both a p-channel transistor and an n-channel transistor may be used.

[0594] The channel formation region of the semiconductor region 413, the region near it, the low resistance region 414a and the low resistance region 414b used as the source region or the drain region preferably contain a silicon-based semiconductor, specifically, preferably contain single crystal silicon. Alternatively, the above-mentioned regions can also be formed using, for example, germanium, silicon germanium, gallium arsenide, aluminum gallium arsenide or gallium nitride. Silicon that applies stress to the lattice to change the interplanar spacing to control the effective mass can be used. In addition, the transistor 400d can also be a HEMT (High Electron Mobility Transistor: High Electron Mobility Transistor) using gallium arsenide and aluminum gallium arsenide, for example.

[0595] As the conductive layer 416 used as the gate electrode, a semiconductor material such as silicon containing an element imparting n-type conductivity such as arsenic or phosphorus or an element imparting p-type conductivity such as boron or aluminum can be used. Alternatively, as the conductive layer 416, for example, a conductive material such as a metal material, an alloy material, or a metal oxide material can be used.

[0596] In addition, since the material of the conductive layer determines the work function, the threshold voltage of the transistor can be adjusted by selecting the material of the conductive layer. Specifically, it is preferred to use one or both of titanium nitride and tantalum nitride as the conductive layer. In order to have both conductivity and embedding properties, it is preferred to use a laminate of one or both of tungsten and aluminum as the conductive layer, and tungsten is particularly preferred in terms of heat resistance.

[0597] An element isolation layer 412 is provided to isolate a plurality of transistors formed on the substrate 410. The element isolation layer can be formed by, for example, a LOCOS (Local Oxidation of Silicon) method, an STI (Shallow Trench Isolation) method, or a mesa isolation method.

[0598] Fig.26 In the transistor 400 d shown, an insulating layer 420 and an insulating layer 422 are stacked in sequence from the substrate 410 side.

[0599] As the insulating layer 420 and the insulating layer 422 , for example, one or more sel...

Claims

1. A semiconductor device comprising: a transistor on a first insulating layer; as well as The second insulating layer, The transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer and a gate electrode on the first insulating layer. The second insulating layer is located between the first conductive layer and the second conductive layer. The second conductive layer is located on the second insulating layer, The second insulating layer and the second conductive layer have openings reaching the first conductive layer. The semiconductor layer is in contact with the side surface of the second insulating layer in the opening and the side surface of the second conductive layer in the opening, The gate insulating layer is located on the semiconductor layer. The gate electrode has a region in the opening that overlaps with the semiconductor layer via the gate insulating layer. The semiconductor layer includes a first oxide layer and a second oxide layer, The first oxide layer has a first region and a second region, The first region and the second region each have a plurality of crystal parts, Furthermore, the second oxide layer is located between the first region and the second region. 2 . The semiconductor device according to claim 1 , wherein the plurality of crystal portions have a c-axis orientation. 3 . The semiconductor device according to claim 1 , wherein the second oxide layer includes a crystal portion having the same crystal structure as that of the plurality of crystal portions. 4 . The semiconductor device according to claim 1 , wherein the second oxide layer includes a crystal portion connected to one of the plurality of crystal portions. 5 . The semiconductor device according to claim 1 , wherein a boundary between the first oxide layer and the second oxide layer is not observed in a cross-sectional TEM image.

6. The semiconductor device according to claim 1, wherein the first conductive layer has a recessed portion overlapping the opening, And the semiconductor layer has a region embedded in the recess.

7. The semiconductor device according to claim 1, The opening has an eighth region whose sidewall is tapered and a ninth region whose sidewall is steeper than that of the eighth region. The eighth region has an upper end of the opening, The ninth area is located below the eighth area, The eighth region has the side surface of the second conductive layer, And the ninth region has the side surface of the second insulating layer.

8. The method for manufacturing a semiconductor device according to claim 7, wherein an angle formed by the side wall of the eighth region and the top surface of the first insulating layer is greater than 20 degrees and less than 75 degrees, Furthermore, an angle formed by the side wall of the ninth region and the top surface of the first insulating layer is greater than 75 degrees and less than 90 degrees.

9. A method for manufacturing a semiconductor device, comprising the following steps: forming a first insulating layer on the first conductive layer; forming a second conductive layer on the first insulating layer; By removing a portion of the second conductive layer and a portion of the first insulating layer, a first opening reaching the first conductive layer is formed to expose a top surface of the first conductive layer; and forming a semiconductor layer in contact with the top surface of the first conductive layer, the side surface of the first insulating layer in the first opening, the side surface of the second conductive layer in the first opening, and the top surface of the second conductive layer, in, The semiconductor layer is formed by a first step of forming a first oxide layer, a second step of forming a second oxide layer, and a third step of performing a heat treatment. The first oxide layer is formed by sputtering. The second oxide layer is formed by atomic layer deposition. forming a second insulating layer in contact with a top surface of the semiconductor layer and a top surface of the first insulating layer, Furthermore, a third conductive layer is formed on the second insulating layer.

10. A storage device, comprising: a first insulating layer; Capacitors; as well as The transistor on the capacitor, The transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer and a gate electrode. The capacitor includes a third conductive layer, a second insulating layer on the third conductive layer, and the first conductive layer on the second insulating layer, The first insulating layer is located between the first conductive layer and the second conductive layer. The second conductive layer is located on the first insulating layer, The first insulating layer and the second conductive layer have openings reaching the first conductive layer. The semiconductor layer is in contact with the side surface of the first insulating layer in the opening and the side surface of the second conductive layer in the opening, The gate insulating layer is located on the semiconductor layer. The gate electrode has a region in the opening that overlaps with the semiconductor layer via the gate insulating layer. The semiconductor layer comprises a metal oxide, The Id-Vgs characteristic of the transistor is measured at a drain-source voltage of 0.05 V or more and 1 V or less, Id is the drain current and Vgs is the gate-source voltage, Furthermore, in the Id-Vgs characteristic, Id is 1×10 -12 Vgs at [A] is greater than 0V and less than 0.5V.

11. The storage device according to claim 10, wherein the metal oxide is In-M-Zn oxide, The element M is one or more selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium and antimony.

12. The storage device according to claim 10, wherein a retention time of the storage device is greater than or equal to 0.64 seconds.

13. The memory device according to claim 10, wherein when the gate of the transistor is set to 0 V, the source of the transistor is set to 0 V, and a voltage of 0.05 V or more and 1 V or less is applied to the drain of the transistor, the accumulated amount of charge flowing through the transistor for 0.64 seconds is 3×10 -15 [F]×0.1[V] or less. The memory device according to claim 10 , wherein a write time of the memory device is less than 15 ns.

15. The memory device according to claim 10, wherein a read time of the memory device is 15 ns or less.

16. The storage device according to claim 14, wherein the write time is calculated using a circuit including a first load connected to the gate of the transistor and a second load connected to the drain of the transistor, The first load includes 256 first circuits, Each of the plurality of first circuits includes a first resistor and a second capacitor, The second load includes 32 second circuits, Each of the plurality of second circuits includes a second resistor and a third capacitor, The first circuit includes a plurality of first resistors connected in series, The second circuit includes a plurality of second resistors connected in series, The resistance value of the first resistor is greater than or equal to 1Ω and less than or equal to 100Ω. The resistance value of the second resistor is greater than or equal to 1Ω and less than or equal to 100Ω. The capacitance value of the second capacitor is greater than or equal to 1aF and less than or equal to 0.5fF. And the capacitance value of the third capacitor is greater than 1aF and less than 0.5fF.

17. The storage device according to claim 15, wherein the readout time is calculated using a circuit including a first load connected to the gate of the transistor and a second load connected to the drain of the transistor, The first load includes 256 first circuits, Each of the plurality of first circuits includes a first resistor and a second capacitor, The second load includes 32 second circuits, Each of the plurality of second circuits includes a second resistor and a third capacitor, The first circuit includes a plurality of first resistors connected in series, The second circuit includes a plurality of second resistors connected in series, The resistance value of the first resistor is greater than or equal to 1Ω and less than or equal to 100Ω. The resistance value of the second resistor is greater than or equal to 1Ω and less than or equal to 100Ω. The capacitance value of the second capacitor is greater than or equal to 1aF and less than or equal to 0.5fF. And the capacitance value of the third capacitor is greater than 1aF and less than 0.5fF.

Citation Information

Patent Citations

  • Semiconductor device and method for manufacturing semiconductor device

    WO2021053473A1