Tube
By alternately stacking the tensile expanded polytetrafluoroethylene layer and the elastomer layer in the peristaltic pump tube, the wall thickness and number of stacks are controlled, and the problems of degradation of durability and discharge instability caused by uneven wall thickness in the prior art are solved. High durability and stable fluid delivery are achieved.
Patent Information
- Application Number
- CN202280093694.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2022-06-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The wall thickness of the existing peristaltic pump pipe is uneven, resulting in local concentration of load and reduced durability. It is easy to peel and break during repeated occlusion, affecting the stability of discharge volume.
By alternately stacking multiple stretched expanded polytetrafluoroethylene layers and elastomer layers in the flow path direction of the tube, the average value and ratio of the wall thickness are calculated, the number of stacks is limited to ensure the uniformity of the wall thickness, using silicone and urethane Elastomers such as acid ester meet specific wall thickness ratios and stacking conditions, and prevent excessive stacking and thickness deviation.
The uniformity of the pipe wall thickness is achieved, the load concentration is avoided, durability and fluid discharge stability are improved, the inner surface friction is reduced, and foreign matter is prevented from mixing in.
Smart Images

Figure CN119032010A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible tube used for a peristaltic pump for conveying fluid. Background Art
[0002] Peristaltic pumps have been used for the delivery and quantitative transportation of fluids in the fields of biomedicine, pharmaceuticals, and chemistry. Peristaltic pumps use flexible tubes. Such tubes are required to have mechanical resistance to repeated bending, and various types of tubes are manufactured.
[0003] For example, the bending-resistant composite elastomer structure disclosed in Patent Document 1 is a composite material having a plurality of stretched expanded polytetrafluoroethylene layers, wherein the polytetrafluoroethylene layers are impregnated with a liquid elastomer and solidified, and the impregnated polytetrafluoroethylene layers are bonded between layers via the elastomer layer. As for the manufacturing method of the composite elastomer structure, a film made of stretched expanded polytetrafluoroethylene is thinly impregnated with a liquid elastomer and wound around an axis until a specified thickness is reached. After the wound object is solidified, the axis is pulled out to obtain a tube. By winding, layered polytetrafluoroethylene layers and elastomer layers can be alternately formed to prevent the development of cracks. This structure shows the effect of preventing openings and leakages caused by tearing and rupture caused by repeated bending actions, thereby improving durability.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 4327352 Summary of the invention
[0007] Problems to be solved by the invention
[0008] The wall thickness of the existing tubes is not uniform. When there is a thickness deviation or wrinkles or bubbles are contained between the overlapping stretched expanded polytetrafluoroethylene layers, when the tube is repeatedly blocked by the roller of the peristaltic pump, the durability is reduced due to the generation of torsional force and the local concentration of force. In addition, there will be parts where the bonding strength between the stretched expanded polytetrafluoroethylene layers is insufficient. As a result, there will be local parts in the tube that are weak to the load, which will cause peeling and breakage, thereby damaging the durability. When there are parts with thin wall thickness, the load applied to the thin part when blocked by the pump becomes less, and the load is concentrated on the thick wall part. In addition, sometimes when the force deviates to the thin part, a torsional force is applied to the tube, or the original durability is not shown and the tube breaks. Moreover, the thickness deviation hinders the repeated reliable blockage of the flow path of the tube, so the discharge volume during pumping is unstable.
[0009] In the case of the above-mentioned background technology, in the thickness condition of each layer, although there is a limit on the thickness of each layer of the stretched expanded polytetrafluoroethylene layer and the elastomer, there is no limit on the thickness deviation when forming a multi-layer tube, and there is a problem in the durability against repeated occlusion. In addition, with respect to the number of windings (number of stacking) of the stretched expanded polytetrafluoroethylene layer, if the wall thickness is excessively stacked, the tube becomes hard and loses its recovery. However, in the case of the above-mentioned background technology, the number of windings is set to more than 31 layers, and the prevention of excessive stacking is not considered.
[0010] In addition, in the manufacturing process shown in the above-mentioned background technology, the film made of stretched expanded polytetrafluoroethylene is passed through the gap between two rollers, and the liquid elastomer is introduced on the film. However, at this time, there is a possibility that the introduced liquid elastomer becomes thinner due to roller slippage. In addition, when the film passes through the gap between the two rollers, the thickness changes if the film is stretched, which affects the wall thickness during lamination. Thickness deviation also occurs when the elastomer is not introduced into the stretched expanded polytetrafluoroethylene layer with a uniform thickness, and no consideration is given to preventing this situation.
[0011] The present invention has been made in view of the above-mentioned problems in the background art, and its object is to provide a tube having a uniform wall thickness, which does not cause localized load concentration during use, has high durability, and has stable discharge when used in a peristaltic pump or the like.
[0012] Solutions for solving problems
[0013] The present invention is a tube, which is a long strip of a certain shape in the long-dimensional direction, and has a flow path penetrating the inside in the long-dimensional direction and a resin part surrounding the flow path, wherein the resin part is configured as a stacked body, which is formed by alternatingly stacking a plurality of stretched expanded polytetrafluoroethylene layers stacked in the radial direction of the flow path and an elastomer layer bonding the polytetrafluoroethylene layers between the layers, the elastomer layer containing at least one elastomer, the polytetrafluoroethylene layer having a void in which a portion of the elastomer is impregnated, the average value of the wall thickness of the resin part in at least four directions intersecting each other in the radial direction of the flow path is calculated, the wall thickness ratio calculated based on the wall thicknesses opposite to each other in the four directions, and the number of stacking of the polytetrafluoroethylene layer and the elastomer layer satisfy the following conditions.
[0014] When the average value of the wall thickness is 0.5 mm or more and less than 2.8 mm, the wall thickness ratio is 1.0 to 1.2, and when the average value of the wall thickness is 2.8 mm or more and less than 10.3 mm, the wall thickness ratio is 1.0 to 1.1.
[0015] Moreover, regarding the number of stacking layers, when the average value of the wall thickness is greater than 0.5 mm and less than 1.4 mm, the number of stacking layers is greater than 5 and less than 35, when the average value of the wall thickness is greater than 1.4 mm and less than 2.0 mm, the number of stacking layers is greater than 14 and less than 50, when the average value of the wall thickness is greater than 2.0 mm and less than 2.8 mm, the number of stacking layers is greater than 20 and less than 70, when the average value of the wall thickness is greater than 2.8 mm and less than 4.0 mm, the number of stacking layers is greater than 28 and less than 100, when the average value of the wall thickness is greater than 4.0 mm and less than 6.2 mm, the number of stacking layers is greater than 40 and less than 155, when the average value of the wall thickness is greater than 6.2 mm and less than 7.7 mm, the number of stacking layers is greater than 62 and less than 193, and when the average value of the wall thickness is greater than 7.7 mm and less than 10.3 mm, the number of stacking layers is greater than 77 and less than 258.
[0016] If the number of layers is excessively stacked within the range of the average values of the wall thicknesses and exceeds the predetermined range of the stacking number, the bonding strength between the elastomers is insufficient, and the elongated polytetrafluoroethylene layer and the elastomer layer are easily peeled off, thereby impairing durability. In addition, the elastomer layer of the tube produced with a small number of layers that does not reach the predetermined range of the number of layers is relatively thick, which causes thickness deviation and does not meet the condition of the wall thickness ratio.
[0017] The elastomer is silicone, urethane, nitrile rubber, styrene-butadiene rubber, chloroprene, phosphazene, fluoroelastomer, perfluoroelastomer, perfluoropolyether elastomer, methyl silicone, phenyl silicone, fluorosilicone, perfluoropolyether elastomer, or a combination thereof. Substances that are not liquid at room temperature are dissolved in a solvent to be liquefied for use.
[0018] Among the elastomers, silicone, methyl silicone, phenyl silicone, fluoroelastomer, perfluoroelastomer, or a combination thereof is particularly preferred.
[0019] The inner peripheral surface of the flow path of the tube is smooth, and the inner peripheral surface of the flow path satisfies at least one of an arithmetic mean roughness Ra of 0.01 to 0.80 and a ten-point average roughness Rz of 0.01 to 3.00.
[0020] Effects of the Invention
[0021] The wall thickness of the tube of the present invention is constant, and there is no unevenness caused by deformed parts. When used, the load is not locally concentrated, and the durability is high. Therefore, when the tube of the present invention is used in a peristaltic pump, etc., the discharge of the fluid is stable. In addition, the surface roughness of the inner surface of the tube of the present invention is small and smooth, so when the tube is flattened to block the internal space, the friction when the inner wall of the tube is closely fitted is reduced, and the slight separation of the innermost surface can be prevented. Therefore, it is possible to suppress the mixing of foreign matter into the discharged fluid. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a cross-sectional view of a tube according to one embodiment of the present invention.
[0023] Figure 2 This is a schematic diagram of the manufacturing process of the pipe according to the present embodiment. DETAILED DESCRIPTION
[0024] Hereinafter, embodiments of the present invention will be described based on the drawings. Figure 1 The present invention is shown as an embodiment. The tube 10 of this embodiment is an elongated object having a constant shape in the longitudinal direction and includes a flow path 12 having a circular cross section penetrating the inside in the longitudinal direction and a cylindrical resin portion 13 surrounding the flow path 12 . Figure 1 The cross-sectional structure which is substantially perpendicular to the longitudinal direction of the tube 10 is shown.
[0025] The resin portion 13 is configured as a laminated body in which a plurality of polytetrafluoroethylene layers 16 are alternately laminated in the radial direction of the flow path 12 and an elastic layer 18 is bonded between the polytetrafluoroethylene layers 16. The polytetrafluoroethylene layer 16 is wound spirally around the flow path 12 multiple times to form a cylindrical body. The polytetrafluoroethylene layer 16 has many fine voids, and a part of the material of the elastic layer 18 is impregnated in the voids.
[0026] Here, the polytetrafluoroethylene layer 16 is described. The polytetrafluoroethylene layer 16 is formed by a polytetrafluoroethylene film 17 made of stretched expanded polytetrafluoroethylene, and the polytetrafluoroethylene film 17 is adjusted using a reactive lubricant. The reactive lubricant contains uncured silicone and a desired solvent such as kerosene, naphtha or mineral spirits. The polytetrafluoroethylene film 17 is manufactured as follows: fine powder of polytetrafluoroethylene is lubricated, extruded, and then stretched and expanded. During the stretching and expansion process, silicone solidifies on the spot to form a polymer network structure (IPN) in which polytetrafluoroethylene and silicone elastomer are entangled with each other. Such a stretched and expanded polytetrafluoroethylene film 17 has residual pores, high strength and moderate resilience. Here, the polytetrafluoroethylene film 17 is, for example, 30 μm thick and 0.1 μm in pore size.
[0027] Next, the elastomer layer 18 is described. The elastomer layer 18 contains at least one elastomer, such as silicone in a liquid state during the coating process, with a hardness of 60 in a type A durometer, a viscosity of 25 Pa·S, a tensile strength of 7.3 MPa, and an elongation of 180%. In addition to silicone, it can also be a fluorine-based resin, which has excellent chemical resistance and has sufficient bending resistance even in the presence of corrosive chemicals (acids; alkalis; solvents such as toluene and MEK). In the case where the viscosity of the coated elastomer is high and it is not impregnated in the gaps of the polytetrafluoroethylene layer 16 during the coating process, it is diluted with a solvent for use.
[0028] The inner peripheral surface of the flow channel 12 is formed smooth. The smoothness of the inner peripheral surface of the flow channel 12 satisfies at least one of an arithmetic mean roughness Ra of 0.01 to 0.80 and a ten-point mean roughness Rz of 0.01 to 3.00.
[0029] In the tube 10, the wall thickness t of the resin portion 13 and the wall thickness ratio, and the number of layers I of the polytetrafluoroethylene layer 16 and the elastomer layer 18 satisfy the conditions shown in Table 1 below. By satisfying these conditions, the durability is good. The wall thickness t of the resin portion 13 is the thickness of the tube 10 measured from the cross section of a plane substantially perpendicular to the longitudinal direction of the tube 10. Figure 1 The wall thickness ratio is the average value of the wall thickness ta, tb, tc, and td of the resin portion 13 in at least four directions A, B, C, and D that intersect each other from the center 0 shown, that is, the average value of the wall thickness ta, tb, tc, and td of the resin portion 13 in the radial direction of the flow path 12, for example, at least four directions A, B, C, and D that are orthogonal to each other. The wall thickness ratio is the average value of the ratio between the wall thicknesses that are opposite to each other in the four directions. The tube 10 of this embodiment is manufactured as follows: the optimal wall thickness ratio of the ratio between the wall thicknesses that are opposite to each other in the four directions and the values of the stacking number I and the wall thickness t are set to meet the optimal conditions for obtaining high durability performance. The optimal conditions of the wall thickness t, the wall thickness ratio, and the stacking number I are shown in the following Table 1.
[0030] [Table 1]
[0031] Wall thickness t(mm) Wall thickness ratio Number of layers: 1 0.5≤t<1.4 1.00~1.22 5≤I<35 1.4≤t<2.0 1.00~1.24 14≤I<50 2.0≤t<2.8 1.00~1.16 20≤I<70 2.8≤t<4.0 1.00~1.11 28≤I<100 4.0≤t<6.2 1.00~1.14 40≤I<155 6.2≤t<7.7 1.00~1.13 62≤I<193 7.7≤t<10.3 1.00~1.10 77≤1<258
[0032] Here, for each value in Table 1 of the wall thickness t, the wall thickness ratio, and the wall thickness ratio in the stacking number I, the values after the decimal point are rounded off to 2 decimal places in consideration of the allowable error. Thus, the preferred wall thickness, the wall thickness ratio, and the stacking number I with high durability become the following conditions. When the average value of the wall thickness t is greater than 0.5 mm and less than 2.8 mm, the wall thickness ratio is 1.0 to 1.2, and when the average value of the wall thickness t is greater than 2.8 mm and less than 10.3 mm, the wall thickness ratio is 1.0 to 1.1. Moreover, regarding the stacking number I, as shown in Table 1.
[0033] Next, based on Figure 2 The method for producing the tube 10 of the present embodiment will be described. This method produces the tube 10 in which the conditions of the wall thickness t, the wall thickness ratio, and the number of layers I are in the optimal range for achieving high durability as shown in Table 1 above.
[0034] First, the polytetrafluoroethylene film 17 to be the polytetrafluoroethylene layer 16 is pulled out from a raw roll 20 through a plurality of film support rollers 22 and sent to a coating step 24 for coating a liquid elastomer 19 to form the elastomer layer 18. In the coating step 24, the polytetrafluoroethylene film 17 impregnated with and thinly coated with the liquid elastomer 19 is wound around a winding shaft 26 in a spiral shape.
[0035] The winding shaft 26 has a circular cross-sectional shape corresponding to the shape of the flow path 12. The winding shaft 26 is coated with a fluororesin so as to be easily peeled off. In addition, since the surface state of the shaft 26 is transferred to the inner surface of the tube, the surface of the shaft 26 is finished to be as smooth as possible, or a tube with a smooth inner surface can be obtained by covering it with a fluororesin heat shrink tube. As the surface roughness of the inner peripheral surface of the flow path 12 of the tube 10, the preferred range satisfies at least one of the conditions of the arithmetic mean roughness Ra being 0.01 to 0.07 and the ten-point average roughness Rz being 0.01 to 0.3.
[0036] The object wound around the winding shaft 26 is subjected to a heat treatment to cause the cross-linking reaction of the liquid elastomer 19 to proceed, thereby bonding the interlayers of the polytetrafluoroethylene film 17 to form a laminated body in which the polytetrafluoroethylene layer 16 and the elastomer layer 18 are alternately laminated. The heat treatment is performed by, for example, placing the object in an oven for heating. After that, the winding shaft 26 is pulled out, the flow path 12 is formed, and the tube 10 is completed.
[0037] The coating step 24 of coating the liquid elastic body 19 is performed near the film support roll 22a immediately before the winding shaft 26. First, the apparatus of the coating step 24 will be described.
[0038] A first blade 28 for scraping the liquid elastomer 19 to make it uniform in thickness is provided upstream of the film support roller 22a and between the previous film support roller 22b located upstream. The first blade 28 is pressed from above the surface of the polytetrafluoroethylene film 17 approximately vertically to the upper surface of the polytetrafluoroethylene film 17. The lower end 28a of the first blade 28 pressed to the upper surface of the polytetrafluoroethylene film 17 is located at a position lower than the film support roller 22a, and the polytetrafluoroethylene film 17 is pressed down to a position lower than the film support roller 22a. The film support roller 22b located upstream of the film support roller 22a is located below the film support roller 22a and is approximately at the same height as the lower end 28a of the first blade 28. The polytetrafluoroethylene film 17 flows approximately horizontally between the film support roller 22b and the first blade 28.
[0039] A liquid elastic body supply device (not shown) is provided between the first blade 28 and the film support roller 22 b , and the liquid elastic body 19 is placed on the upper surface of the polytetrafluoroethylene film 17 .
[0040] A second blade 30 is provided downstream of the film support roller 22a and between the winding shaft 26 for further scraping the liquid elastomer 19 to make it more uniform in thickness. The second blade 30 is pressed from above the surface of the polytetrafluoroethylene film 17 to the upper surface of the polytetrafluoroethylene film 17. The second blade 30 is tilted so that the lower end 30a in contact with the polytetrafluoroethylene film 17 is directed toward the downstream side. The lower end 30a of the second blade 30 is located slightly lower than the upper end of the film support roller 22a, and the polytetrafluoroethylene film 17 is pressed down to a position slightly below the upper end of the film support roller 22a. The winding shaft 26 located downstream of the second blade 30 is located slightly below the lower end 30a, and the polytetrafluoroethylene film 17 flows obliquely downward toward the downstream between the second blade 30 and the winding shaft 26.
[0041] Next, the coating process 24 will be described. The liquid elastomer 19 is supplied from a liquid elastomer supply device (not shown) and placed on the upper surface of the polytetrafluoroethylene film 17 that is in contact with the film support roller 22b and flows, and then contacts the first blade 28 to scrape off the excess portion to make it uniform in thickness. Then, it passes through the film support roller 22a and further contacts the second blade 30 to scrape off the excess portion again to make it uniform in thickness. The first blade 28 and the second blade 30 can apply the liquid elastomer 19 with a uniform thickness, and at the same time, the micropores of the polytetrafluoroethylene film 17 can be reliably impregnated with the liquid elastomer 19.
[0042] According to the tube 10 of the present embodiment, regarding the conditions of the wall thickness t of the resin portion 13, the wall thickness ratio, and the number of stacking I, the wall thickness ratio is suppressed to a small range, the durability is stabilized, and the durability is improved. Moreover, with the wall thickness t being 2.8 mm as the boundary, when the wall thickness is above it, by relatively suppressing the value of the wall thickness ratio to a small range, the absolute value of the uneven wall thickness is suppressed, and the durability is improved even for the tube 10 with a thicker wall thickness t. Moreover, by setting the number of stacking I to the above-mentioned preferred range, higher durability can be obtained. That is, according to the above-mentioned conditions, the wall thickness of the tube 10 can be set more evenly within the prescribed range, there is no unevenness caused by the position when the tube 10 is deformed, the load is not locally concentrated, and the durability is improved. Therefore, when used for a peristaltic pump, the discharge of the fluid is stable. Moreover, by making the wall thickness uniform within the prescribed range, the uneven durability caused by setting the tube 10 in the direction of the peristaltic pump can be prevented.
[0043] In addition, according to the tube 10 of this embodiment, the inner surface has a small surface roughness and is smooth, so when the tube is flattened to close the internal space, the friction when the inner wall of the tube is tightly fitted is reduced, and the innermost surface can be prevented from being slightly separated. As a result, it is possible to suppress the mixing of foreign matter into the fluid such as the discharged liquid. The tube 10 can be easily manufactured by coating the liquid elastomer 19 on the polytetrafluoroethylene film 17. In the coating process 24 of the liquid elastomer 19, it contacts the first blade 28 and the second blade 30 twice, and the excess liquid elastomer 19 can be scraped to make it uniform in thickness. It can be reliably impregnated in the gaps of the polytetrafluoroethylene film 17, and the tube 10 that meets the optimal conditions for obtaining high durability performance can be manufactured.
[0044] It should be noted that the tube of the present invention is not limited to the above-mentioned embodiment, and the method for manufacturing the polytetrafluoroethylene film to be the polytetrafluoroethylene layer may be a method other than the above-mentioned method. The raw material of the elastomer layer may also be a raw material other than the above-mentioned raw material. The number and position of the film support rollers in the manufacturing process, the position of the coating process, etc. may be appropriately changed. The length of the tube in the long dimension direction is free, and the tube can be used for various purposes.
[0045] Description of Reference Numerals
[0046] 10: tube; 12: flow path; 13: resin portion; 16: polytetrafluoroethylene layer; 17: polytetrafluoroethylene film; 18: elastomer layer; 19: liquid elastomer.
Claims
1. A tube, characterized in that It is a long object with a certain shape in the longitudinal direction, and has a flow path penetrating the inside in the longitudinal direction and a resin part surrounding the flow path, wherein: The resin portion is configured as a laminate, wherein a plurality of stretched expanded polytetrafluoroethylene layers laminated in the radial direction of the flow path and an elastomer layer bonded between the polytetrafluoroethylene layers are alternately laminated, wherein the elastomer layer contains at least one elastomer, and the polytetrafluoroethylene layer has a void in which a portion of the elastomer is impregnated. The average value of the wall thickness of the resin portion in at least four directions intersecting each other in the radial direction of the flow path is calculated, and the wall thickness ratio calculated based on the wall thicknesses facing each other in the four directions and the number of stacking layers of the polytetrafluoroethylene layer and the elastomer layer are calculated. When the average value of the wall thickness is 0.5 mm or more and less than 2.8 mm, the wall thickness ratio is 1.0 to 1.2, and when the average value of the wall thickness is 2.8 mm or more and less than 10.3 mm, the wall thickness ratio is 1.0 to 1.
1. Moreover, regarding the stacking number, When the average value of the wall thickness is 0.5 mm or more and less than 1.4 mm, the number of stacking layers is 5 or more and less than 35, When the average value of the wall thickness is 1.4 mm or more and less than 2.0 mm, the number of layers is 14 or more and less than 50, When the average value of the wall thickness is 2.0 mm or more and less than 2.8 mm, the number of stacking layers is 20 or more and less than 70, When the average value of the wall thickness is 2.8 mm or more and less than 4.0 mm, the number of stacking layers is 28 or more and less than 100, When the average value of the wall thickness is 4.0 mm or more and less than 6.2 mm, the number of stacking layers is 40 or more and less than 155, When the average value of the wall thickness is 6.2 mm or more and less than 7.7 mm, the number of layers is 62 or more and less than 193, When the average value of the wall thickness is 7.7 mm or more and less than 10.3 mm, the number of stacked layers is 77 or more and less than 258.
2. The tube according to claim 1, wherein The elastomer is silicone, urethane, nitrile rubber, styrene-butadiene rubber, chloroprene, phosphazene, perfluoropolyether elastomer, perfluoropolyether elastomer, or a combination thereof.
3. The tube according to claim 1, wherein The elastomer is methyl silicone, phenyl silicone, or a combination thereof.
4. The tube according to claim 1, wherein The elastomer is a fluoroelastomer, a perfluoroelastomer, or a combination thereof.
5. The tube according to claim 1, wherein The inner peripheral surface of the flow path of the tube is smooth.
6. The tube according to claim 5, wherein The inner peripheral surface of the flow channel of the tube has an arithmetic mean roughness Ra of 0.01 to 0.80 and / or a ten-point average roughness Rz of 0.01 to 3.00.
Citation Information
Patent Citations
Flex-resistant composite elastomer composition
JP2002502735A
Tube and pump using same
WO2021149783A1