Optical glass, optical element, interchangeable lens for camera, objective lens for microscope, cemented lens, optical system, optical device, reflective element, and position measurement device
By adjusting the content of TeO2, ZnO, B2O3 and other components in optical glass, the problem that existing optical glass cannot meet the high refractive, high dispersion and low abnormal dispersion at the same time is solved, and high refractive and suitable for high pixel image sensor equipment are achieved. Low abnormal dispersion characteristics improve the resolution and chromatic aberration performance of the device.
Patent Information
- Application Number
- CN202380028001.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-02-24
- Publication Date
- 2024-11-26
AI Technical Summary
Existing optical glasses are difficult to meet the characteristics of high refractive index, high dispersion, low abnormal dispersion and near infrared region refractive index of about 2, and cannot meet the high resolution and low chromatic aberration requirements of high-pixel image sensor devices.
By adjusting the molar content of each component, the refractive index and devitrification resistance of the glass are optimized, and the refractive index and devitrification resistance of the glass are combined with ZnO, B2O3, Bi2O3, La2O3, WO3, Y2O3, Gd2O3 and other components are used to optimize the refractive index and devitrification resistance of the glass to form a Optical glass with high refractive, high dispersion and low abnormal dispersion.
The high refractive, high dispersion and low abnormal dispersion characteristics of optical glass are realized, and the refractive index in the near infrared region is about 2. It is suitable for high-pixel image sensor equipment, improving the resolution and chromatic aberration performance of optical devices.
Smart Images

Figure CN119032068A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to optical glass, optical elements, interchangeable lenses for cameras, objective lenses for microscopes, cemented lenses, optical systems, optical devices, reflective elements, and position measuring devices. The present invention claims priority to Japanese Patent Application No. 2022-053320 filed on March 29, 2022, and the contents described in the Japanese Patent Application No. 2022-053320 are incorporated into the present application by reference for designated countries that recognize the introduction of contents by reference. Background Art
[0002] In recent years, imaging devices with high-pixel image sensors have been developed. Optical glass used in these devices is required to have high refractive index, high dispersion, low anomalous dispersion, and a refractive index of about 2 in the near-infrared region.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-219365 SUMMARY OF THE INVENTION
[0006] The first mode of the present invention is an optical glass as follows, wherein, in terms of mole %, the percentage of TeO2 is 40-85%, the percentage of ZnO is 10-40%, and the glass contains any one of B2O3 and Bi2O3 and any one of La2O3 and WO3. Alternatively, the optical glass as follows, wherein, in terms of mole %, the percentage of TeO2 is 40-85%, the percentage of ZnO is 10-40%, the percentage of B2O3 is 0-10%, the percentage of Bi2O3 is 0-10%, and the glass further contains at least one of Y2O3, La2O3, and Gd2O3.
[0007] A second aspect of the present invention is an optical element using the above-mentioned optical glass.
[0008] A third aspect according to the present invention is an optical device including the above-mentioned optical element.
[0009] A fourth aspect according to the present invention is a reflective element including the above-mentioned optical element.
[0010] A fifth aspect according to the present invention is a position measuring device including the above-mentioned reflecting element.
[0011] A sixth aspect according to the present invention is an interchangeable lens for a camera including the above-mentioned optical element.
[0012] A seventh aspect according to the present invention is a microscope objective lens including the above-mentioned optical element.
[0013] An eighth aspect according to the present invention is a cemented lens including a first lens element and a second lens element, wherein at least one of the first lens element and the second lens element is made of the above-mentioned optical glass.
[0014] A ninth aspect according to the present invention is an optical system including the above-mentioned cemented lens.
[0015] A tenth aspect according to the present invention is an interchangeable lens for a camera, comprising the above-mentioned optical system.
[0016] An eleventh aspect according to the present invention is a microscope objective lens including the above-mentioned optical system.
[0017] A twelfth aspect according to the present invention is an optical device including the above-mentioned optical system. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a perspective view showing an example of the optical device according to the present embodiment as an imaging device.
[0019] Figure 2 It is a schematic diagram showing another example of the optical device according to the present embodiment as an imaging device, and is a front view of the imaging device.
[0020] Figure 3 It is a schematic diagram showing another example of the optical device according to the present embodiment as an imaging device, and is a rear view of the imaging device.
[0021] Figure 4 This is a block diagram showing an example of the structure of the multiphoton microscope according to the present embodiment.
[0022] Figure 5 This is a schematic diagram showing an example of a cemented lens according to the present embodiment.
[0023] FIG6 shows Fig. 6A , Figure 6B This is a schematic diagram of an example of a position measuring device to which the reflective element according to the present embodiment is applied.
[0024] Figure 7 is ν of each embodiment d With P g,F Graph of the curve. DETAILED DESCRIPTION
[0025] The following is an explanation of an embodiment of the present invention (hereinafter referred to as "this embodiment"). The following this embodiment is an example for explaining the present invention, and does not mean that the present invention is limited to the following content. The present invention can be implemented by appropriately modifying it within the scope of its purpose.
[0026] This embodiment relates to an optical glass, wherein, in terms of mole %, the percentage of TeO2 is 40-85%, the percentage of ZnO is 10-40%, and the glass contains any one of B2O3 and Bi2O3 and any one of La2O3 and WO3. Alternatively, the optical glass comprises, in terms of mole %, the percentage of TeO2 is 40-85%, the percentage of ZnO is 10-40%, the percentage of B2O3 is 0-10%, the percentage of Bi2O3 is 0-10%, and the glass further comprises at least one of Y2O3, La2O3, and Gd2O3.
[0027] In this specification, unless otherwise specified, the percentage content of each component is the mole % of each component relative to the total mole number of the glass in oxide conversion composition. In addition, the oxide conversion composition referred to herein refers to the following composition: assuming that the oxides, composite salts, etc. used as raw materials for the glass constituent components of this embodiment are all decomposed into oxides during melting, the total mole number of the oxides is set to 100 mol% to represent the components contained in the glass.
[0028] In addition, the expression "0-N%" of the content percentage of Q includes the case where no Q component is contained and the case where the Q component is more than 0% and less than N%.
[0029] In addition, the expression "does not contain component Q" means that component Q is not substantially contained, and means that the percentage content of the constituent component is lower than the impurity level. For example, lower than the impurity level may be less than 0.01%.
[0030] In addition, the expression "devitrification stability" means the resistance of glass to devitrification. Here, "devitrification" refers to the phenomenon that glass loses its transparency due to crystallization or phase separation when the temperature of glass is raised to above the glass transition temperature or when the temperature is lowered from the molten liquid state to below the liquidus temperature.
[0031] The optical glass involved in this embodiment has high refraction, high dispersion, low anomalous dispersion, and also has the characteristics of a refractive index of about 2 in the near-infrared region.
[0032] Hereinafter, the component composition of the optical glass according to the present embodiment will be described.
[0033] TeO2 is a component that can improve the refractive index and the stability against devitrification. From a related point of view, the percentage of TeO2 is 40-85% in mole %. Moreover, the lower limit of the percentage is preferably 45%, more preferably 47%, and further preferably 50%. In addition, the upper limit of the percentage is preferably 80%, more preferably 70%, and further preferably 65%.
[0034] ZnO is a component that improves the stability against devitrification and reduces the partial dispersion ratio. If the percentage of ZnO is too little, there is a tendency for the stability against devitrification to be reduced. If the percentage of ZnO is too much, there is a tendency for the partial dispersion ratio to be reduced. From this point of view, the percentage of ZnO is 10-40% in mole %. Moreover, the lower limit of the percentage is preferably 12%, more preferably 15%, and further preferably 18%. In addition, the upper limit of the percentage is preferably 35%, more preferably 30%, and further preferably 25%.
[0035] The glass involved in this embodiment preferably contains any one of B2O3 and Bi2O3 in addition to TeO2 and ZnO. For example, when B2O3 is contained, Bi2O3 is a component that may or may not be added to the optical glass of this embodiment. Further, it is preferred to contain any one of La2O3 and WO3. For example, when La2O3 is contained, WO3 is a component that may or may not be added to the optical glass of this embodiment.
[0036] B2O3 is a component that forms a network-forming oxide. B2O3 is a highly volatile component. If introduced in excess, it may cause the composition of the glass to change during manufacturing and produce obvious streaks. From this point of view, the percentage of B2O3 is 0-20% in mole %. Moreover, the lower limit of the percentage is preferably 2%, more preferably 4%, and further preferably 5%. In addition, the upper limit of the percentage is preferably 16%, more preferably 14%, and further preferably 12%.
[0037] Bi2O3 is a component that increases the refractive index and the partial dispersion ratio. If the percentage of Bi2O3 is too much, there is a tendency to reduce the transmittance or increase the dispersion. If the percentage of Bi2O3 is too little, there is a tendency to reduce the meltability. From this point of view, the percentage of Bi2O3 is 0-10% in mole %. Moreover, the lower limit of the percentage is preferably 2%, more preferably 3%, and further preferably 4%. In addition, the upper limit of the percentage is preferably 9%, more preferably 8%, and further preferably 7%.
[0038] La2O3 has the effect of increasing the refractive index without damaging the low dispersion, and can maintain the anti-devitrification stability of the glass. However, as the percentage increases, the specific gravity is also more likely to increase. From this point of view, the percentage of La2O3 is 0-15% in mole %. Moreover, the lower limit of the percentage is preferably 2%, more preferably 4%, and further preferably 6%. In addition, the upper limit of the percentage is preferably 13%, more preferably 11%, and further preferably 10%.
[0039] From the perspective of transmittance, the percentage of WO3 is 0-20% in mole %. Moreover, the lower limit of the percentage is preferably 2%, more preferably 4%, and further preferably 6%. In addition, the upper limit of the percentage is preferably 18%, more preferably 16%, and further preferably 14%.
[0040] Y2O3 is a component that can increase the refractive index without compromising low dispersion, especially when combined with La 3+ When coexisting in glass, the devitrification resistance stability can be further improved. From this viewpoint, the percentage content of Y2O3 is 0-15% by mole %. Moreover, the lower limit of the percentage content is preferably 1%, more preferably 2%, and more preferably 3%. In addition, the upper limit of the percentage content is preferably 13%, more preferably 10%, and more preferably 8%.
[0041] Gd2O3 is a component that can increase the refractive index without compromising low dispersion, especially when combined with La 3+ When coexisting in glass, the stability against devitrification can be further improved. From this viewpoint, the percentage content of Gd2O3 is 0-15% by mole %. Moreover, the lower limit of the percentage content is preferably 1%, more preferably 2%, and more preferably 3%. In addition, the upper limit of the percentage content is preferably 13%, more preferably 10%, and more preferably 8%.
[0042] The optical glass involved in this embodiment preferably contains at least one of Y2O3, La2O3 and Gd2O3. The total percentage of Y2O3, La2O3 and Gd2O3 (ΣLn2O3; wherein Ln = Y, La, Gd) is 0-15% in mole %. Moreover, the lower limit of the percentage is preferably 0%, more preferably 3%, and further preferably 4%. In addition, the upper limit of the percentage is preferably 13%, more preferably 11%, and further preferably 10%. By setting (Y2O3+La2O3+Gd2O3) within this range, the refractive index and devitrification resistance stability of the optical glass can be improved.
[0043] Li2O is a kind of g,F, a component that improves the melting property of glass. If the percentage is too large, the devitrification resistance is reduced and the Abbe number becomes higher. From this point of view, the percentage of Li2O is 0-10% in mole %. Moreover, the lower limit of the percentage is preferably 1%, more preferably 2%, and further preferably 3%. In addition, the upper limit of the percentage is preferably 8%, more preferably 6%, and further preferably 5%.
[0044] Na2O is a kind of g,F , a component that improves the melting property of glass. If the percentage is too large, the devitrification resistance is reduced and the Abbe number becomes higher. From this point of view, the percentage of Na2O is 0-10% in mole %. Moreover, the lower limit of the percentage is preferably 1%, more preferably 2%, and further preferably 3%. In addition, the upper limit of the percentage is preferably 8%, more preferably 6%, and further preferably 5%.
[0045] K2O is a kind of ΔP g,F , a component that improves the meltability of glass, but compared with Li2O or Na2O, it has a better effect of reducing the devitrification stability of glass and increasing the Abbe number. From this point of view, the percentage content of K2O is 0-10% in mole %. Moreover, the lower limit of the percentage content is preferably 1%, more preferably 2%, and further preferably 3%. In addition, the upper limit of the percentage content is preferably 8%, more preferably 6%, and further preferably 5%.
[0046] From the viewpoint of high dispersion, the content of SrO is 0-5% in mol%. Moreover, the lower limit of the content is preferably 0.5%, more preferably 1%, and further preferably 2%. In addition, the upper limit of the content is preferably 4%, more preferably 3.5%, and further preferably 3%.
[0047] BaO is a kind of material that does not significantly increase ΔP g,F BaO is a component that can improve the devitrification resistance of glass. In the absence of BaO, the devitrification resistance of glass decreases. From this point of view, the percentage of BaO is 0-5% in mole %. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 2%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3.5%, and further preferably 3%.
[0048] From the viewpoint of high dispersion, the content of CaO is 0-10% in mol%. The lower limit of the content is preferably 1%, more preferably 2%, and further preferably 3%. The upper limit of the content is preferably 9%, more preferably 8%, and further preferably 6%.
[0049] MgO is a component that can increase the Abbe number, but it increases ΔP by g,F From this point of view, the percentage of MgO is 0-10% in mole %. Moreover, the lower limit of the percentage is preferably 1%, more preferably 2%, and further preferably 3%. In addition, the upper limit of the percentage is preferably 9%, more preferably 8%, and further preferably 7%.
[0050] Al2O3 is a component that can improve the melting property and devitrification resistance of optical glass during manufacturing. From this point of view, the percentage of Al2O3 is 0-5% by mole %. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 1.5%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3%, and further preferably 2%.
[0051] TiO2 can increase the refractive index while maintaining a low specific gravity. From the perspective of such effects and the percentage of rare earth components or transition metal components, the percentage of TiO2 is 0-5% by mole %. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 1.5%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3%, and further preferably 2%.
[0052] ZrO2 has the effect of improving the stability against devitrification and the refractive index while maintaining low dispersion. If the percentage is too low, the dispersion becomes high, and if it exceeds 5%, the glass becomes easy to devitrify. From this point of view, the percentage of ZrO2 is 0-5% in mole %. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 1.5%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3.5%, and further preferably 3%.
[0053] Nb2O5 can further improve the low dispersion of glass. From this point of view, the percentage of Nb2O5 is 0-5% in mol%. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 1.5%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3.5%, and further preferably 3%.
[0054] Ta2O5 has the effect of improving the stability against devitrification while maintaining low dispersion. From this point of view, the percentage of Ta2O5 is 0-5% in mol%. Moreover, the lower limit of the percentage is preferably 0.5%, more preferably 1%, and further preferably 1.5%. In addition, the upper limit of the percentage is preferably 4%, more preferably 3.5%, and further preferably 3%.
[0055] The ratio of the total percentage content (mol %) of Bi2O3, B2O3, Y2O3, La2O3 and Gd2O3 to the percentage content (mol %) of TeO2, i.e. (Bi2O3 + B2O3 + Y2O3 + La2O3 + Gd2O3) / TeO2 is 0-0.8. Moreover, the lower limit of the ratio is preferably 0.2, more preferably 0.4, and further preferably 0.6. The upper limit of the ratio is preferably 0.78, more preferably 0.76, and further preferably 0.74. By setting (Bi2O3 + B2O3 + Y2O3 + La2O3 + Gd2O3) / TeO2 within this range, the devitrification resistance stability can be maintained.
[0056] From the viewpoint of meltability, refractive index and chemical durability, the total percentage content of Li2O, Na2O and K2O (ΣA2O; wherein A = Li, Na, K) is 0-10% in mol%. Moreover, the lower limit of the total percentage content is preferably 0.5%, more preferably 1%, and further preferably 2%. The upper limit of the total percentage content is preferably 8%, more preferably 6%, and further preferably 5%.
[0057] As a preferred combination of the percentages of these, the percentage of Li2O is 0-10%, the percentage of Na2O is 0-10%, and the percentage of K2O is 0-10%. By adopting such a combination, the meltability can be improved and the chemical durability can be prevented from being reduced.
[0058] From the viewpoint of meltability, refractive index and chemical durability, the total percentage content of SrO, BaO, CaO, MgO and ZnO (ΣEO; wherein E = Sr, Ba, Ca, Mg, Zn) is 10-40% in mol%. Moreover, the lower limit of the total percentage content is preferably 11%, more preferably 12%, and further preferably 13%. The upper limit of the total percentage content is preferably 35%, more preferably 30%, and further preferably 25%. By adopting such a combination, meltability can be maintained and the refractive index and chemical durability can be improved.
[0059] The manufacturing method of the optical glass involved in the present embodiment is not limited, and publicly known methods can be used. In addition, suitable production conditions can be appropriately selected. For example, the following manufacturing method can be used: raw materials such as oxides, carbonates, nitrates, sulfates, etc. are mixed to achieve the target composition, preferably melted at 1100-1400°C, and stirred to make it uniform, after defoaming, injected into a mold for molding. The lower limit of the above-mentioned melting temperature is more preferably 1200°C, and the upper limit is more preferably 1350°C, and further preferably 1300°C. The optical glass obtained in this way can be processed into a desired shape by reheat pressing molding as needed, and made into a desired optical element by grinding, etc.
[0060] The raw material is preferably a high-purity product with a small percentage of impurities. A high-purity product means a product containing 99.85% by mass or more of the component. By using a high-purity product, the amount of impurities is reduced, and there is a tendency to increase the internal transmittance of the optical glass.
[0061] In addition, as required, for the purpose of clarification, coloring, decolorization, or fine adjustment of optical constant values, a suitable amount of publicly known clarifiers, colorants, degassing agents, fluorine compounds and other components can be added to the glass composition. In addition, it is not limited to the above components, and other components can also be added within the range of obtaining the effect of the optical glass involved in this embodiment.
[0062] Next, the physical property values of the optical glass according to the present embodiment will be described.
[0063] From the viewpoint of reducing the thickness of the lens, the optical glass according to the present embodiment preferably has a high refractive index (refractive index (n d ) is larger). However, in general, the refractive index (n d ) is higher, the transmittance is lower. Based on this fact, the refractive index (n) of the optical glass of this embodiment with respect to the d line is d ) is preferably in the range of 1.95-2.2. d The lower limit of ) is more preferably 1.96, and further preferably 1.98. d ) is preferably 2.15, more preferably 2.1, and further preferably 2.07.
[0064] From the viewpoint of use in the near-infrared region, the refractive index (n) of the optical glass according to the present embodiment at 1550 nm in the optical glass according to the present embodiment is 1550 ) is preferably in the range of 1.9-2.1. The refractive index at 1550nm (n 1550 The lower limit of ) is more preferably 1.91, and further preferably 1.93. The refractive index at 1550 nm (n 1550 ) is more preferably 2.0, and further preferably 1.997.
[0065] The Abbe number (ν d ) is preferably in the range of 15-30. Moreover, the Abbe number (ν d The lower limit of ) is more preferably 16, and further preferably 18. The Abbe number (ν d ) is more preferably 27, and further preferably 25.
[0066] From the viewpoint of lens aberration correction, the optical glass according to the present embodiment preferably has a large partial dispersion ratio (P g,F). According to this actual situation, the partial dispersion ratio (P g,F ) preferably satisfies the following formula (1)
[0067] -0.00607×vd+0.752 <P g,F <-0.00607×vd+0.762…(1)
[0068] Or 0.55-0.68. Moreover, the partial dispersion ratio (P g,F The lower limit of the partial dispersion ratio (P g,F ) is more preferably 0.68, further preferably 0.66.
[0069] From the viewpoint of lens aberration correction, the optical glass according to the present embodiment preferably has a large anomalous dispersion (P g,F ). Based on this fact, the value indicating the anomalous dispersion of the optical glass involved in this embodiment (ΔP g,F ) is preferably 0.002 or more. And the value indicating anomalous dispersion (ΔP g,F The lower limit of ) is more preferably 0.004, and further preferably 0.006. g,F ) is not particularly limited and may be set to 0.040, for example.
[0070] From the above viewpoints, the optical glass involved in this embodiment is suitable for use as an optical element, and the optical element can be used in optical equipment. Such optical elements include mirrors, lenses, prisms, filters, reflective devices, reflective elements, etc. In addition, as an optical system using the above optical elements, it can be, for example, an objective lens, a converging lens, an imaging lens, a camera interchangeable lens, a position measuring device, etc. In addition, these optical systems are suitable for use as imaging devices such as interchangeable lens cameras and non-interchangeable lens cameras, various optical devices such as fluorescence microscopes and multiphoton microscopes, and position measuring devices such as laser trackers. The optical device is not limited to the above imaging devices or microscopes, but also includes telescopes, binoculars, laser rangefinders, projectors, etc. An example thereof is introduced below.
[0071] <Camera>
[0072] Figure 11 is a stereoscopic diagram of an example of an optical device according to the present embodiment as an imaging device. The imaging device 1 is a so-called digital single-lens reflex camera (interchangeable lens camera), and the photographic lens 103 (optical system) has an optical element whose base material is the optical glass according to the present embodiment. The lens barrel 102 is mounted on a lens mount (not shown) of a camera body 101 in a freely detachable manner. In addition, light from the lens 103 passing through the lens barrel 102 is imaged on a sensor chip (solid-state imaging element) 104 of a multi-chip module 106 disposed on the back side of the camera body 101. The sensor chip 104 is a bare chip such as a so-called CMOS image sensor, and the multi-chip module 106 is a COG (Chip On Glass) type module in which, for example, the sensor chip 104 is mounted on a glass substrate 105 in a bare chip manner.
[0073] Figure 2 and Figure 3 This is a schematic diagram of another example of the optical device involved in this embodiment as an imaging device. Figure 2 A front view showing the camera device CAM, Figure 3 The rear view of the imaging device CAM is shown. The imaging device CAM is a so-called digital still camera (non-interchangeable lens camera), and the taking lens WL (optical system) includes an optical element using the optical glass according to the present embodiment as a base material.
[0074] In the camera device CAM, if the power button (not shown) is pressed, the shutter (not shown) of the photographic lens WL is opened, and the light from the subject (object) is condensed by the photographic lens WL and formed on the imaging element arranged on the image plane. The subject image formed on the imaging element is displayed on the liquid crystal display M arranged behind the camera device CAM. The photographer determines the composition of the subject image while observing the liquid crystal display M, and then presses the release button B1, and the subject image is photographed by the imaging element and recorded and stored in the memory (not shown).
[0075] The imaging device CAM is provided with an auxiliary light emitting unit EF for emitting auxiliary light when the subject is dark, a function button B2 for setting various conditions of the imaging device CAM, and the like.
[0076] Optical systems used in digital cameras and the like are required to have higher resolution, lower chromatic aberration, and be smaller. In order to achieve these requirements, it is effective to use glasses with different dispersion characteristics in the optical system. In particular, for low dispersion and a higher partial dispersion ratio (P g,F) is in high demand. From this aspect, the optical glass involved in this embodiment is suitable as a component of the optical device. In addition, the optical device applicable to this embodiment is not limited to the above-mentioned camera device, and a projector, etc., for example, can also be used. The optical element is not limited to the lens, and a prism, etc., for example, can also be used.
[0077] <Microscope>
[0078] Figure 4 2 is a block diagram of a configuration example of a multiphoton microscope 2 according to the present embodiment. The multiphoton microscope 2 includes an objective lens 206, a converging lens 208, and an imaging lens 210. At least one of the objective lens 206, the converging lens 208, and the imaging lens 210 includes an optical element having an optical glass according to the present embodiment as a base material. The following description will focus on the optical system of the multiphoton microscope 2.
[0079] The pulse laser device 201 emits ultrashort pulse light with a near-infrared wavelength (about 1000 nm) and a pulse width of femtoseconds (e.g., 100 femtoseconds). The ultrashort pulse light immediately after being emitted from the pulse laser device 201 is generally linearly polarized light polarized in a predetermined direction.
[0080] The pulse splitting device 202 splits the ultrashort pulse light, increases the repetition frequency of the ultrashort pulse light, and then emits the split pulse light.
[0081] The beam adjustment unit 203 has the following functions: a function of adjusting the beam diameter of the ultrashort pulse light incident from the pulse splitting device 202 in comparison with the pupil diameter of the objective lens 206; a function of adjusting the convergence and divergence angles of the ultrashort pulse light in order to correct the axial chromatic aberration (focal difference) between the wavelength of the light emitted from the sample S and the wavelength of the ultrashort pulse light; a function of pre-chirping the ultrashort pulse light with an opposite group velocity dispersion (group velocity dispersion compensation function) in order to correct the situation in which the pulse width of the ultrashort pulse light becomes wider due to group velocity dispersion while passing through the optical system, etc.
[0082] The repetition frequency of the ultrashort pulse light emitted from the pulse laser device 201 is increased by the pulse splitting device 202, and the above adjustment is performed by the beam adjusting unit 203. In addition, the ultrashort pulse light emitted from the beam adjusting unit 203 is reflected in the direction of the dichroic mirror 204, passes through the dichroic mirror 205, and is converged by the objective lens 206 to irradiate the sample S. At this time, the ultrashort pulse light can be scanned on the observation surface of the sample S by using a scanning device (not shown).
[0083] For example, when performing fluorescence observation on sample S, in the area where sample S is irradiated with ultrashort pulse light and its vicinity, the fluorescent pigment that dyes sample S is subjected to multi-photon excitation and emits fluorescence having a wavelength shorter than the infrared wavelength of the ultrashort pulse light (hereinafter referred to as "observation light").
[0084] The observation light emitted from the sample S toward the objective lens 206 is collimated by the objective lens 206 , and is reflected by the dichroic mirror 205 or passes through the dichroic mirror 205 according to its wavelength.
[0085] The observation light reflected by the dichroic mirror 205 enters the fluorescence detection unit 207. The fluorescence detection unit 207 is composed of, for example, a barrier filter, a PMT (photo multiplier tube), etc., receives the observation light reflected by the dichroic mirror 205, and outputs an electrical signal corresponding to the light quantity. In addition, when the ultrashort pulse light scans the observation surface of the sample S, the fluorescence detection unit 207 detects the observation light on the observation surface of the sample S.
[0086] In addition, the fluorescence detection unit 211 can be used to detect all observation light emitted from the sample S in the direction of the objective lens 206 by removing the dichroic mirror 205 from the optical path. In this case, the observation light is reversely scanned by a scanning device (not shown), passes through the dichroic mirror 204, is converged by the convergent lens 208, passes through the small hole 209 set at a position roughly conjugate with the focal position of the objective lens 206, passes through the imaging lens 210, and enters the fluorescence detection unit 211.
[0087] The fluorescence detection unit 211 is composed of, for example, a barrier filter, a PMT, etc., receives the observation light imaged on the light receiving surface of the fluorescence detection unit 211 by the imaging lens 210, and outputs an electrical signal corresponding to the light quantity. In addition, when the ultrashort pulse light scans the observation surface of the sample S, the fluorescence detection unit 211 detects the observation light on the observation surface of the sample S.
[0088] In addition, the observation light emitted from the sample S in the direction opposite to the objective lens 206 is reflected by the dichroic mirror 212 and enters the fluorescence detection unit 213. The fluorescence detection unit 113 is composed of, for example, a barrier filter, a PMT, etc., receives the observation light reflected by the dichroic mirror 212, and outputs an electrical signal corresponding to the light amount. In addition, when the ultrashort pulse light scans the observation surface of the sample S, the fluorescence detection unit 213 detects the observation light on the observation surface of the sample S.
[0089] The electrical signals outputted from the fluorescence detection units 207 , 211 , and 213 are inputted into, for example, a computer (not shown), and the computer can generate an observation image based on the input electrical signals, and display the generated observation image or store the observation image data.
[0090] <Joint lens>
[0091] Figure 5 3 is a schematic diagram of an example of a combined lens according to the present embodiment. Combined lens 3 is a composite lens having a first lens element 301 and a second lens element 302. At least one of the first lens element and the second lens element adopts the optical glass according to the present embodiment. The first lens element and the second lens element are combined by a combination component 303. As the combination component 303, a publicly known adhesive or the like can be used. In addition, "lens element" refers to each lens constituting a single lens or a combined lens.
[0092] The joint lens involved in this embodiment is useful in the aspect of chromatic aberration correction, and can be applied to the above-mentioned optical element, optical system or optical device, etc. In addition, the optical system including the joint lens is particularly suitable for use in camera interchangeable lenses or optical devices, etc. In addition, in the above-mentioned method, a joint lens using two lens elements is described, but it is not limited to this, and it can also be a joint lens using more than three lens elements. In the case of making a joint lens using more than three lens elements, at least one of the more than three lens elements can be formed using the optical glass involved in this embodiment.
[0093] like Fig. 6A As shown, the glass involved in this embodiment can also be used as a reflective element (reply reflector) 402 of a position measuring device 401 such as a laser tracker. The position measuring device 401 integrates an irradiating unit 403 and a light receiving unit 404, and the irradiating unit projects light onto the reflective element 402, and the light receiving unit receives the light reflected by the reflector. The reflective element 402 can be installed on a part of a workpiece (measurement object) 405 such as a robot arm, a machine tool, or an aircraft shell. Any number of reflective elements can be installed on the workpiece. The shape of the reflective element 402 can be a shape in which the hemispherical glass involved in this embodiment and the glass of this embodiment other than the hemispherical shape are bonded together, preferably a cat's eye glass (spherical glass).
[0094] Next, use Fig. 6A , Figure 6B The operation of the position measuring device 401 will be described. First, Fig. 6A As shown in FIG. 4 , the position measuring device 401 directs the irradiation unit 403 in the direction of the reflective element 402 provided on the workpiece 405 and irradiates the measuring light. Figure 6BAs shown, the light reflected by the reflective element 402 is received by the light receiving unit 404. The position measuring device 401 measures the distance to the reflective element 402 based on the time from when the light is irradiated to the reflective element to when the reflected light is received, and determines the three-dimensional position of the reflective element 402 based on the measured distance and the direction (elevation angle and azimuth angle) of the irradiated measurement light. As a distance measuring method, a method of using interference between a reference light serving as a reference and the measurement light reflected from the reflective element 402 to obtain the distance based on the phase difference between the two lights may be used.
[0095] [Example]
[0096] Next, examples and comparative examples of the present invention will be described, but the present invention is not limited thereto.
[0097] <Production of optical glass>
[0098] The optical glass involved in each embodiment and each comparative example is produced according to the following procedure. First, glass raw materials selected from oxides, hydroxides, phosphoric acid compounds (phosphates, orthophosphoric acid, etc.), carbonates and nitrates are weighed in a manner to achieve the composition (mass %) recorded in each table. Next, the weighed raw materials are mixed, put into a platinum crucible, melted at a temperature of 750-1100°C and stirred evenly. After defoaming, the temperature is lowered to an appropriate level, then cast into a mold, annealed, and formed to obtain each sample.
[0099] <Physical Property Evaluation>
[0100] Figure 7 is the P of each embodiment and comparative example g,F and ν d Graph of the curve.
[0101] Refractive index (n d ) and the Abbe number (ν d )
[0102] The refractive index of each sample (n d ) and the Abbe number (ν d ) was measured and calculated using a refractometer (manufactured by Shimadzu Device Co., Ltd.: KPR-2000). d Indicates the refractive index of glass for light of 587.562nm. d From the following formula (2), we can find: C 、n F They represent the refractive index of glass for light with wavelengths of 656.273nm and 486.133nm respectively.
[0103] ν d =(n d -1) / (n F -nC )…(2)
[0104] Partial dispersion ratio (P g,F )
[0105] The partial dispersion ratio (P g,F ) represents partial dispersion (n g -n F ) relative to the main dispersion (n F -n C ) is calculated by the following formula (3): g It indicates the refractive index of glass for light with a wavelength of 435.835nm. g,F ) value is rounded to three decimal places.
[0106] P g,F =(n g -n F ) / (n F -n C )…(3)
[0107] Anomalous dispersion (ΔP g,F )
[0108] The anomalous dispersion (ΔP g,F ) shows the deviation of the partial dispersion ratio standard line of the glass with normal dispersion from the two glass types of F2 and K7. That is, the vertical axis is the partial dispersion ratio (P g,F ), the horizontal axis is the Abbe number ν d The difference between the vertical coordinate of the straight line connecting the two glass types and the vertical coordinate of the glass value of the comparison object is the deviation of the partial dispersion ratio, that is, the anomalous dispersion (ΔP g,F In the above coordinate system, when the value of the partial dispersion ratio is located above the straight line connecting the glass types used as the reference, the glass shows positive anomalous dispersion (+ΔP g,F ), when it is located at the lower side, the glass shows negative anomalous dispersion (-ΔP g,F ). In addition, the Abbe numbers ν of F2 and K7 d And the partial dispersion ratio (Pg,F) is as follows:
[0109] F2: Abbe number ν d =36.33, partial dispersion ratio (P g,F )=0.5834
[0110] K7: Abbe number ν d =60.47, partial dispersion ratio (P g,F )=0.5429
[0111] ΔP g,F =P g,F-(-0.0016777×ν d +0.6443513)···(4)
[0112] Each table shows the composition and physical property values of each example. In addition, unless otherwise specified, the percentage of each component is based on mole %. The "ΣA2O" in the formula is the total percentage of Li2O, Na2O and K2O; where (A=Li, Na, K). The "ΣEO" in the formula is the total percentage of SrO, BaO, CaO, MgO and ZnO; where (E=Sr, Ba, Ca, Mg, Zn). The "ΣLn2O3" in the formula is the total percentage of Y2O3, La2O3 and Gd2O3, where (Ln=Y, La, Gd). Since the comparative example cannot obtain optical glass, its physical properties are "unable to measure".
[0113] [Table 1]
[0114]
[0115] [Table 2]
[0116]
[0117] [Table 3]
[0118]
[0119] [Table 4]
[0120]
[0121] [Table 5]
[0122]
[0123] [Table 6]
[0124]
[0125] [Table 7]
[0126]
[0127] [Table 8]
[0128]
[0129] [Table 9]
[0130]
[0131] [Table 10]
[0132]
[0133] [Table 11]
[0134]
[0135] [Table 12]
[0136]
[0137] [Table 13]
[0138]
[0139] In summary, it is confirmed that the optical glass of this embodiment has high refraction, high dispersion, low anomalous dispersion, and has a near-infrared refractive index of about 2.
[0140] Explanation of symbols
[0141] 1 Camera device
[0142] 101 Camera Body
[0143] 102 Lens barrel
[0144] 103 Lens
[0145] 104 sensor chip
[0146] 105 Glass Substrate
[0147] 106 Multi-chip Module
[0148] CAM camera (non-interchangeable lens camera)
[0149] WL Photo Lenses
[0150] M LCD display
[0151] EF auxiliary light emitting unit
[0152] B1 Release button
[0153] B2 Function Button
[0154] 2 Multiphoton Microscopy
[0155] 201 Pulse Laser Device
[0156] 202 Pulse splitting device
[0157] 203 Beam adjustment unit
[0158] 204,205,212 dichroic mirror
[0159] 206 objective lens
[0160] 207,211,213 Fluorescence detection unit
[0161] 208 Converging lens
[0162] 209 Small hole
[0163] 210 Imaging lens
[0164] S specimen
[0165] 3 Cemented lens
[0166] 301 First lens element
[0167] 302 Second lens element
[0168] 303 Joint parts
[0169] 401 Position measuring device
[0170] 402 Reflective element
[0171] 403 Irradiation Department
[0172] 404 Light receiving unit
[0173] 405 Work
Claims
1. An optical glass, in, In mole %, TeO 2 The percentage content is 40-85%, The percentage of ZnO is 10-40%, Also contains B 2 O 3 and Bi 2 O 3 Any of and La 2 O 3 and WO 3 Any one of .
2. The optical glass according to claim 1, in, In mole %, B 2 O 3 The percentage content is 0-20%, Bi 2 O 3 The percentage content is 0-10%.
3. The optical glass according to claim 1 or 2, in, In mole %, La 2 O 3 The percentage content is 0-15%, WO 3 The percentage content is 0-20%.
4. The optical glass according to any one of claims 1 to 3, in, In mole %, Y 2 O 3 The percentage content is 0-15%, G 2 O 3 The percentage content is 0-15%.
5. An optical glass, in, In mole %, TeO 2 The percentage of B is 40-85%, the percentage of ZnO is 10-40%, 2 O 3 The percentage content is 0-20%, Bi 2 O 3 The percentage content is 0-10%. and contains Y 2 O 3 ,La 2 O 3 , Gd 2 O 3 At least one of .
6. The optical glass according to claim 5, in, In mole %, B 2 O 3 The percentage content is more than 0-20%, Bi 2 O 3 The percentage content is more than 0-10%.
7. The optical glass according to claim 5 or 6, in, In mole %, Y 2 O 3 The percentage content is 0-15%, La 2 O 3 The percentage content is 0-15%, G 2 O 3 The percentage content is 0-15%.
8. The optical glass according to any one of claims 5 to 7, in, WO 3 The percentage content is 0-20%.
9. The optical glass according to any one of claims 1 to 8, in, Y 2 O 3 ,La 2 O 3 and Gd 2 O 3 Total percentage ΣLn 2 O 3 It is 0-15%, where Ln = Y, La, Gd.
10. The optical glass according to any one of claims 1 to 9, in, In mole %, Li 2 The percentage of O is 0-10%, Na 2 The percentage of O is 0-10%, K 2 The percentage of O is 0-10%.
11. The optical glass according to any one of claims 1 to 10, in, In mole %, The percentage of SrO is 0-5%, The percentage of BaO is 0-5%, The percentage of CaO is 0-10%, The percentage of MgO is 0-10%.
12. The optical glass according to any one of claims 1 to 11, in, In mole %, Al 2 O 3 The percentage content is 0-5%, TiO 2 The percentage content is 0-5%, ZrO 2 The percentage content is 0-5%, Nb 2 O 5 The percentage content is 0-5%, Ta 2 O 5 The percentage content is 0-5%.
13. The optical glass according to any one of claims 1 to 12, in, In mole %, Bi 2 O 3 , B 2 O 3 , Y 2 O 3 ,La 2 O 3 and Gd 2 O 3 The total percentage of TeO 2 The percentage ratio of 2 O 3 +B 2 O 3 +Y 2 O 3 +La 2 O 3 +Gd 2 O 3 ) / TeO 2 It is 0-0.
8.
14. The optical glass according to any one of claims 1 to 13, in, In mole %, Li 2 O、Na 2 O and K 2 Total percentage of O (ΣA 2 O; wherein A=Li, Na, K) is 0-10%.
15. The optical glass according to any one of claims 1 to 14, in, In mole %, The total percentage content ΣEO of SrO, BaO, CaO and MgO is 10-40%, where E = Sr, Ba, Ca, Mg.
16. The optical glass according to any one of claims 1 to 15, in, The refractive index on the d line (n d ) is 1.95-2.
2.
17. The optical glass according to any one of claims 1 to 16, in, The Abbe number is 15-30.
18. The optical glass according to any one of claims 1 to 17, in, Partial dispersion ratio (P g,F ) is 0.55-0.
68.
19. The optical glass according to any one of claims 1 to 18, in, Refractive index at 1550nm (n 1550 ) is 1.9-2.
1.
20. An optical element, comprising the optical glass according to any one of claims 1 to 19.
21. An optical device comprising the optical element according to claim 20.
22. A reflective element comprising the optical element according to claim 20.
23. A position measuring device comprising: A reflective element is provided on the object to be measured. an irradiation unit for irradiating the measuring light to the reflecting element, a light receiving unit for receiving the measurement light reflected by the reflecting element; The reflective element is the reflective element according to claim 22.
24. An interchangeable lens for a camera, comprising the optical element according to claim 20.
25. An objective lens for a microscope, comprising the optical element according to claim 20.
26. A cemented lens, in, having a first lens element and a second lens element, At least one of the first lens element and the second lens element is the optical glass according to any one of claims 1 to 19. An optical system comprising the cemented lens according to claim 26 .
28. An interchangeable lens for a camera, comprising the optical system according to claim 27.
29. An objective lens for a microscope, comprising the optical system according to claim 27.
30. An optical device comprising the optical system according to claim 27.
Citation Information
Patent Citations
Process for producing optical glass element
CN101184699A
Optical glass, optical element and perform product for precise pressure forming
CN102070298A
Optical glass, optical element, and preform for precision press molding
CN102414137A
Optical glass
CN102414138A
Optical glass and lens
JP2004043294A