Photosensitive resin composition, resin film having pattern, method for producing resin film having pattern, and semiconductor circuit board
By using a photosensitive resin composition containing specific structural units on the semiconductor circuit substrate to form a patterned resin film with high elongation and high pressure cooker test resistance, the reliability of the insulating film in temperature changes and pressure cooker test is solved. Improves the performance and stability of the circuit substrate.
Patent Information
- Application Number
- CN202380033609.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-14
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-26
AI Technical Summary
The insulating film of the semiconductor circuit substrate is prone to warping and deformation when the temperature changes, resulting in damage, and it is difficult to maintain high reliability elongation in the use environment of the information terminal machine, especially in the pressure cooker test.
A photosensitive resin composition containing a polymer of specific structural units, a naphthoquinone diazide compound and a crosslinking agent is used to form a patterned resin film through exposure and development techniques to improve the elongation of the resin film and the resistance to pressure cooker test.
The resin film with high elongation and high pressure cooker test resistance is achieved, and is suitable for the insulating film of semiconductor circuit substrates, improving the reliability and performance of the circuit substrate.
Smart Images

Figure CN119032324A_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to a photosensitive resin composition, a resin film having a pattern, a method for producing a resin film having a pattern, and a semiconductor circuit board. Background Art
[0002] Various photosensitive resin compositions have been proposed as materials for forming surface protective films and interlayer insulating films used in semiconductor circuit boards among electronic components. For example, a photosensitive resin composition containing a resin having a phenolic hydroxyl group as an alkali-soluble resin has been studied (Patent Documents 1 and 2).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-186300
[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-210606 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In order to increase the density or performance of semiconductor circuit substrates, packaging technology using silicon interposers and fan-out packaging technology using molded substrates have been proposed. However, in such substrate materials and insulating films, due to the difference in their thermal linear expansion coefficients, warping and deformation are sometimes easily caused by temperature changes in the manufacturing process of the semiconductor circuit substrate or the use environment of the information terminal device. In the case where the elongation of the insulating film is small, there is a problem that the insulating film cannot withstand the warping and deformation and is damaged. In addition, it is required to maintain high reliability of elongation in environmental load tests (for example, pressure cooker test (PCT) test) that assume the use environment of the information terminal device.
[0009] Furthermore, the insulating film used in the semiconductor circuit substrate is used between the electrode pads or wirings with fine pitches. Therefore, in the composition for forming the resin film such as the insulating film with pattern (hereinafter also referred to as "patterned resin film"), it is necessary to have photolithography properties that can be patterned by exposure and development.
[0010] The present invention is an invention for solving the above-mentioned problems, and its purpose is to: provide a photosensitive resin composition that can form a resin film with excellent elongation and high PCT resistance and excellent photolithography; provide a patterned resin film with excellent elongation and high PCT resistance and a method for manufacturing the same; and provide a semiconductor circuit substrate including a patterned resin film with excellent elongation and high PCT resistance.
[0011] Technical means of solving problems
[0012] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by a photosensitive resin composition containing a polymer having a specific structural unit, a specific photoacid generator, and a specific crosslinking agent, thereby completing the present invention. The following is an example of the present invention. [1]
[0014] A photosensitive resin composition comprising:
[0015] (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor;
[0016] (B) naphthoquinone diazide compounds;
[0017] (C1) a crosslinking compound having a hydroxymethyl group or an alkoxymethyl group; and
[0018] (D)solvent,
[0019] The polymer (A) comprises a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine,
[0020] The structural unit (a) includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1).
[0021] [Chemistry 1]
[0022]
[0023] [In the above formula (1),
[0024] L independently represents a single bond, an ester bond, or an amide bond,
[0025] R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3 an alkylene group having 1 to 4 carbon atoms bonded to each other,
[0026] n 1 and n 2 Each independently represents an integer from 0 to 3 (wherein, within the same ring, n 1 With n 2 is an integer greater than 1),
[0027] Y 1 represents a structure represented by the following formula (Y1) or formula (Y2);
[0028] *-Ar 1 -*…(Y1)
[0029] *-Ar 2 -Y 2 -Ar 2 -*…(Y2)
[0030] In the above formula (Y1) and formula (Y2), * represents a bond with respect to L in the above formula (1),
[0031] Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms from an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms,
[0032] Y in the formula (Y2) 2 is a single bond, an oxygen atom, a sulfur atom, at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group] [2]
[0034] The photosensitive resin composition according to [1], wherein the polymer (A) has a phenolic hydroxyl group at a polymer terminal. [3]
[0036] The photosensitive resin composition according to [1] or [2], wherein the structural unit (b) derived from a diamine includes a structural unit (b1) derived from a diamine having a phenolic hydroxyl group. [4]
[0038] The photosensitive resin composition according to any one of [1] to [3], further comprising (C2) an epoxy compound (which is different from the crosslinkable compound (C1)). [5]
[0040] A method for producing a resin film having a pattern, comprising: a step (1) of forming a coating film of the photosensitive resin composition according to any one of [1] to [4] on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using an alkaline developer. [6]
[0042] A resin film having a pattern is obtained by curing the photosensitive resin composition according to any one of [1] to [4]. [7]
[0044] A semiconductor circuit substrate includes the resin film having a pattern according to [6].
[0045] Effects of the Invention
[0046] According to one embodiment of the present invention, there can be provided a photosensitive resin composition capable of forming a resin film having excellent elongation and high PCT resistance and having excellent photolithography properties, and further a patterned resin film having excellent elongation and high PCT resistance and a method for manufacturing the same, and a semiconductor circuit substrate comprising a patterned resin film having excellent elongation and high PCT resistance. DETAILED DESCRIPTION
[0047] Hereinafter, the mode for carrying out the present invention including the preferred mode will be described in detail.
[0048] [Photosensitive resin composition]
[0049] The photosensitive resin composition of one embodiment of the present invention (hereinafter, also simply referred to as “the present composition”) contains:
[0050] (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor (hereinafter also referred to as “polymer (A)”);
[0051] (B) a naphthoquinonediazide compound (hereinafter also referred to as "compound (B)");
[0052] (C1) a crosslinking compound having a hydroxymethyl group or an alkoxymethyl group (hereinafter also referred to as "crosslinking compound (C1)"); and
[0053] (D) Solvent.
[0054] <Polymer (A)>
[0055] The polymer (A) contained in the present composition is a polymer (resin) selected from the group consisting of polyimide and polyimide precursor, and contains a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine. Due to the presence of such a structure, the polymer (A) contained in the present composition can have both high i-ray transmittance and high elongation. In addition, the polymer (A) has excellent solvent solubility and can also be given alkali solubility by introducing an alkali-soluble group.
[0056] (Structural unit (a))
[0057] The structural unit (a) is a structural unit derived from an acid anhydride, and includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1). It is believed that the acid anhydride group having an alicyclic structure in the structural unit (a1) contributes to the improvement of i-ray transmittance, solvent solubility, and PCT resistance, and the aromatic group contributes to the improvement of elongation. By including the structural unit (a1) in the polymer (A), the present composition has both high i-ray transmittance and high elongation. The structural unit (a1) may include one or more than two.
[0058] [Chemistry 2]
[0059]
[0060] In the formula (1), Y 1 It represents a structure represented by the following formula (Y1) or formula (Y2), and preferably a structure represented by the following formula (Y1). In the following formula, * represents a bond with respect to L in the above formula (1).
[0061] *-Ar 1 -*…(Y1)
[0062] *-Ar 2 -Y 2 -Ar 2 -*…(Y2)
[0063] In the formula (Y1) and the formula (Y2), Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms on an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms.
[0064] Examples of the aromatic ring include aromatic hydrocarbon compounds such as a benzene ring and a naphthalene ring, and heteroaromatic compounds such as a furan ring and a pyrrole ring. An aromatic hydrocarbon compound having 6 to 10 carbon atoms such as a benzene ring and a naphthalene ring is preferred.
[0065] Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, n-pentyl, and n-hexyl. Examples of the alkoxy group having 1 to 6 carbon atoms include methoxy and ethoxy. Among these, alkyl groups having 1 or 2 carbon atoms, such as methyl and ethyl, or alkoxy groups having 1 or 2 carbon atoms, such as methoxy and ethoxy, are preferred.
[0066] In the formula (Y2), Y 2 It is a single bond, an oxygen atom, a sulfur atom, or at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group.
[0067] In the formula (1), L independently represents a single bond, an ester bond, or an amide bond, wherein the ester bond includes any bond represented by -OC(O)- or -C(O)-O-, and the amide bond includes any bond represented by -NH-C(O)- or -C(O)-NH-.
[0068] In the formula (1), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3 An alkylene group having 1 to 4 carbon atoms formed by bonding to each other. Examples of the alkyl group having 1 to 6 carbon atoms include the same groups as those mentioned above, and a methyl group and an ethyl group are preferred.
[0069] In the formula (1), n 1 and n 2 Each independently represents an integer from 0 to 3, and is preferably 0 or 1. 1 With n 2 At least one of is an integer greater than 1.
[0070] The acid anhydride represented by the formula (1) is preferably 1 ~R 3 All hydrogen atoms, or one R in the same ring 1 With an R 2 , or an R 1 With an R 3 Specific preferred examples of the acid anhydride represented by the formula (1) include acid anhydrides represented by the following formulas (1-1) to (1-3), and more preferred examples are acid anhydrides represented by the following formula (1-1) or (1-2).
[0071] [Chemistry 3]
[0072]
[0073] The structural unit (a) may include a structural unit (a2) derived from an acid anhydride other than the acid anhydride represented by the formula (1) within a range not impairing the effects of the present invention. The structural unit (a2) may include one or more types.
[0074] As the acid anhydride other than the acid anhydride represented by the above formula (1) (hereinafter also referred to as “other acid anhydride”), an acid anhydride represented by the following formula (2) is preferred.
[0075] [Chemistry 4]
[0076]
[0077] In the above formula (2), X can be, for example, a group represented by the following formula: In the following formula, * represents a bond to the carbon atom to which X in the above formula (2) is bonded.
[0078] [Chemistry 5]
[0079]
[0080] [Chemistry 6]
[0081]
[0082] The hydrogen atom (omitted in the formula) in the group represented by the above formula may be substituted by an alkyl group or alkoxy group having 1 to 6 carbon atoms, or a group in which the hydrogen atom in the alkyl group or alkoxy group is substituted by a halogen atom (for example, trifluoromethyl group).
[0083] When the polymer (A) contains the structural unit (a2), the molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is preferably 99 / 1 to 50 / 50, and more preferably 95 / 5 to 60 / 40. The content ratio of each structural unit can be calculated by 13 C-NMR ( 13 C-Nuclear Magnetic Resonance, 13 C-NMR). If the molar ratio of the structural unit (a1) to the structural unit (a2) is within the above range, the above effect brought about by using the structural unit (a1) can be easily obtained. In addition, a polymer in which the molar ratio of each monomer (anhydride, diamine described later, and terminal modifier described later) in the monomer mixture is within the above range can also be said to be a polymer in which the molar ratio of the structural unit derived from the monomer is within the above range.
[0084] (Structural unit (b))
[0085] The structural unit (b) is a structural unit derived from a diamine. The structural unit (b) is not particularly limited as long as it is a structural unit derived from a diamine, but is preferably a structural unit derived from a diamine having a hydroxyl group, and more preferably a structural unit (b1) derived from a diamine having a phenolic hydroxyl group. The structural unit (b1) may include one or more.
[0086] As the diamine having a hydroxyl group, a diamine represented by the following formula (3) is preferred.
[0087] [Chemistry 7]
[0088] H 2 NZ 1 -NH 2 ···(3)
[0089] In the formula (3), Z 1 represents a divalent group having a hydroxyl group, preferably a divalent group represented by the following formula (Z1) or formula (Z2). In the following formula, * represents Z in the above formula (3). 1 The bond to the nitrogen atom.
[0090] [Chemistry 8]
[0091]
[0092] R in the formula (Z1) and formula (Z2) 5 and R 6 Each independently represents a hydrogen atom, an acyl group or an alkyl group. Preferred acyl groups include formyl, acetyl, propionyl, butyryl, isobutyryl, etc., and preferred alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, n-pentyl, n-hexyl, n-octyl, n-decyl, n-dodecyl, etc.
[0093] Z in the formula (Z2) 2 It is a single bond, an oxygen atom, a sulfur atom, or at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group.
[0094] In the formula (Z1), n 5 An integer of 1 or 2.
[0095] In the formula (Z2), n 6 are independently integers from 0 to 2, and there are two n 6 At least one of is an integer greater than 1.
[0096] In addition, in one molecule of the diamine represented by the formula (3), OR 5 Base (OR 6When the base) is one, R 5 (or R 6 ) is a hydrogen atom. There are multiple ORs in one molecule. 5 Base (OR 6 In the case of R 5 (or R 6 ) is a hydrogen atom. According to the above case, the diamine represented by the above formula (3) having a group represented by the above formula (Z1) or formula (Z2) is a diamine having a phenolic hydroxyl group, which can provide the structural unit (b1).
[0097] In the diamine represented by the formula (3) having a group represented by the formula (Z1), Z in the formula (3) 1 Specifically, the following divalent groups are preferred. In the following formula, * represents Z in the above formula (3): 1 The bond to the nitrogen atom.
[0098] [Chemistry 9]
[0099]
[0100] In the diamine represented by the formula (3) having a group represented by the formula (Z2), Z in the formula (3) 1 Specifically, the following divalent groups are preferred. In the following formula, * represents Z in the above formula (3): 1 The bond to the nitrogen atom.
[0101] [Chemistry 10]
[0102]
[0103] In addition to the diamine represented by the formula (3) having a group represented by the formula (Z1) or (Z2), examples of the compound having a phenolic hydroxyl group in the diamine represented by the formula (3) include: 1 In the following formula, * represents Z in the formula (3). 1 The bond to the nitrogen atom.
[0104] [Chemistry 11]
[0105]
[0106] In addition, the structural unit (b) may include a structural unit (b2) derived from a diamine other than the diamine having a phenolic hydroxyl group. The structural unit (b2) may include one or two or more.
[0107] Examples of the diamine other than the diamine having a phenolic hydroxyl group include: diamines not having a phenolic hydroxyl group among the diamines represented by the formula (3); p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-diaminobenzanilide, 4,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane. Methyl indane, 3,4'-diaminodiphenyl ether, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-Bis(3-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 2,7-diaminofluorene, 9,9-bis(4-aminophenyl)fluorene, 4,4'-methylene-bis(2-chloroaniline), 2,2',5,5'-tetrachloro-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diamino-5,5'-dimethoxybiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 1,4,4'-(p-phenylene isopropylidene) dianiline, 4,4'-(m-phenylene isopropylidene) dianiline, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis(4-aminophenoxy)biphenyl , 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-bis[(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl and other aromatic diamines; m-phenylenediamine, p-phenylenediamine, 1,3-propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 4,4'-diaminoheptamethylenediamine, 1,4-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, isophoronediamine, tetrahydrodicyclopentadienyldiamine, hexahydro-4,7-methanodihydroindenyl dimethylenediamine, tricyclo6.2.1.02,7-undecylene dimethyl diamine, 4,4'-methylenebis(cyclohexylamine) and other aliphatic or alicyclic diamines; 1,3-bis(3-aminopropyl)tetramethyldisiloxane and other siloxane-containing diamines; polyether diamines; polyoxyalkylene diamines. .
[0108] When the polymer (A) contains the structural unit (b2), the molar ratio of the structural unit (b1) to the structural unit (b2) (structural unit (b1) / structural unit (b2)) is preferably 99 / 1 to 50 / 50, more preferably 90 / 10 to 50 / 50. The content ratio of each structural unit can be determined by 13 C-NMR. If the molar ratio of the structural unit (b1) to the structural unit (b2) is within the above range, the above effect brought about by using the structural unit (b1) can be easily obtained. In addition, a polymer in which the molar ratio of each monomer in the monomer mixture is within the above range can also be regarded as a polymer in which the molar ratio of the structural unit derived from each monomer is within the above range.
[0109] (Terminal structure)
[0110] The polymer (A) used in the present composition preferably has a phenolic hydroxyl group at the polymer terminal. Generally, as a method for introducing phenol into the polymer terminal, it is achieved by using a terminal modifier having a phenolic hydroxyl group as a terminal modifier. As the terminal modifier, for example, 2-aminophenol, 3-aminophenol, and 4-aminophenol can be cited. These react the anhydride terminal in the polymer (A) with the amine in the terminal modifier, and the polymer terminal is self-anhydride modified.
[0111] In the present invention, when a diamine having a phenolic hydroxyl group as described above is used as a monomer, a polymer having a phenolic hydroxyl group at a polymer terminal can be synthesized without using a terminal modifying agent.
[0112] When a terminal modifier is used, the molar ratio (mol %) of the terminal modifier (terminal modifier×100 / (acid anhydride+diamine+terminal modifier)) when the total molar amount of the acid anhydride providing the structural unit (a), the diamine providing the structural unit (b), and the terminal modifier is set to 100 is preferably 1 mol % to 20 mol %, and more preferably 5 mol % to 15 mol %.
[0113] (Characteristics of polymer (A))
[0114] The molar ratio of the structural unit (a) to the structural unit (b) in the polymer (A) (structural unit (a) / structural unit (b)) is preferably 60 / 40 to 40 / 60, and more preferably 55 / 45 to 45 / 55. The content ratio of each structural unit can be determined by 13Furthermore, a polymer in which the molar ratio of each monomer in the monomer mixture is within the above range can also be referred to as a polymer in which the molar ratio of the structural unit derived from each monomer is within the above range.
[0115] Regarding polymer (A), the polystyrene-equivalent weight average molecular weight (hereinafter also referred to as "Mw") measured by gel permeation chromatography (GPC) is preferably about 2,000 to 800,000. When the polymer (A) is used in a photosensitive resin composition, it is preferably about 2,000 to 100,000, more preferably about 2,000 to 70,000, and further preferably about 3,000 to 50,000. When the polymer (A) is used in a photosensitive resin composition, if Mw is less than 2,000, there is a tendency that sufficient mechanical properties as an insulating film cannot be obtained. On the other hand, if Mw exceeds 100,000, there is a tendency that the exposed portion of the photosensitive resin composition obtained using the polymer (A) lacks solubility in a solvent or a developer.
[0116] In addition, the resin film obtained from the polymer (A) is excellent in elongation, PCT resistance, and i-ray transmittance. Therefore, it is considered that the patterned resin film obtained by curing the present composition using the polymer (A) is excellent in elongation, PCT resistance, and lithography properties.
[0117] The polymer (A) may be used alone or in combination of two or more.
[0118] The lower limit of the content of the polymer (A) in 100% by mass of the solid content of the present composition is usually 20% by mass, preferably 40% by mass, and more preferably 60% by mass; the upper limit is usually 99% by mass, preferably 95% by mass. In addition, the solid content refers to all components that may be contained in the present composition except the solvent (D) described later.
[0119] The polymer (A) has at least one structure selected from the group consisting of polyimide and polyimide precursor. The polyimide precursor includes polyamic acid and polyamic acid ester. The structure of the polymer (A) can be 1 H-NMR etc. to confirm.
[0120] (Method for producing polymer (A))
[0121] Polymer (A) can be obtained, for example, by the following method: using anhydrides, diamines (for example, diamines with phenolic hydroxyl groups) represented by the formula (1), and anhydrides, diamines, and terminal modifiers other than the anhydrides as needed, reacting in a polymerization solvent to synthesize polyamic acid, and then performing imidization to synthesize polyimide. The terminal modifier can be reacted before the synthesis of polyamic acid, during the synthesis of polyamic acid, or after the imidization according to the introduction site (main chain end or side chain end). At this time, the polyamic acid synthesized midway can be used as a polymer (A) having the polyimide precursor structure. In addition, polyamic acid esters obtained by esterifying polyamic acid according to an existing method can also be used as a polymer (A) having the polyimide precursor structure.
[0122] At this time, the synthesis sequence of the polyamic acid for obtaining the polyimide can be applied to the following two methods, or can be synthesized by any method. That is, the following methods: (i) a method of dissolving an acid anhydride in a polymerization solvent and then reacting a diamine; (ii) a method of dissolving a diamine in a polymerization solvent and then reacting an acid anhydride.
[0123] As the polymerization solvent, a solvent that can dissolve the raw materials and products during the synthesis of the polymer (A) is selected. As the polymerization solvent, it is preferred to use at least one selected from the group consisting of N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, and γ-butyrolactone. These compounds can be used alone as the polymerization solvent, or two or more can be mixed and used.
[0124] In addition to the polymerization solvent, other solvents may be used in combination as needed. Examples of other solvents include: diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether and diethylene glycol diethyl ether; ethylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate; diethylene glycol monoalkyl ether acetates such as diethylene glycol monomethyl ether acetate; propylene glycol monoalkyl ether acetates such as propylene glycol monomethyl ether acetate; ketones such as methyl ethyl ketone and cyclohexanone; alcohols such as methanol, ethanol, and propanol; ether solvents such as diethylene glycol dimethyl ether and triethylene glycol dimethyl ether; and aromatic hydrocarbons such as toluene and xylene.
[0125] The imidization reaction for obtaining the polymer (A) having a polyimide structure can be applied to existing methods such as thermal imidization reaction and chemical imidization reaction. In the case of synthesizing the polymer (A) by thermal imidization reaction, it is preferably carried out by heating the synthetic solution of polyamic acid at 120° C. to 210° C. for 1 to 16 hours. In addition, the reaction can be carried out while removing water in the system using an azeotropic solvent such as toluene or xylene as needed.
[0126] <Compound (B)>
[0127] The present composition contains (B) a naphthoquinonediazide compound.
[0128] Compound (B) is a compound that functions as a photoacid generator and generates an acid by a treatment including light irradiation. By subjecting the resin film formed from the present composition to an exposure treatment, an acid is generated in the exposed portion based on compound (B), and the solubility of the exposed portion in an alkaline developer changes based on the action of the acid.
[0129] The compound (B) generates carboxylic acid by a process including light irradiation and development using an alkaline developer. The resin film obtained from the composition containing the compound (B) is a film that is insoluble in an alkaline developer. Therefore, by using the compound (B), a positive pattern can be formed.
[0130] Compound (B) is, for example, a compound having one or more phenolic hydroxyl groups, and an ester compound with 1,2-naphthoquinonediazide-4-sulfonic acid or 1,2-naphthoquinonediazide-5-sulfonic acid. Specific examples of compounds having one or more phenolic hydroxyl groups include compounds described in paragraphs
[0065] to
[0070] of Japanese Patent Laid-Open No. 2014-186300, which are described in this specification.
[0131] The compound (B) may be used alone or in combination of two or more.
[0132] In the present composition, the content of the compound (B) is usually 5 to 50 parts by mass, preferably 10 to 40 parts by mass, and more preferably 15 to 35 parts by mass, relative to 100 parts by mass of the polymer (A). If the content of the compound (B) is above the lower limit, the residual film rate of the unexposed portion is increased, and an image faithful to the pattern mask is easily obtained. If the content of the compound (B) is below the upper limit, there is a tendency to easily obtain a resin film with excellent pattern shape and prevent foaming during film formation.
[0133] <Crosslinking agent (C)>
[0134] In order to improve the curability of the resin film and to balance the chemical resistance and crack resistance of the cured film, the present composition contains a crosslinking agent (C). The crosslinking agent (C) functions as a crosslinking component (hardening component) that reacts with the polymer (A) or the crosslinking agents react with each other. The crosslinking agent (C) can be used alone or in combination of two or more.
[0135] The present composition contains (C1) a crosslinking compound having a hydroxymethyl group or an alkoxymethyl group as a crosslinking agent (C). Regarding the crosslinking compound (C1) used in the present composition, the crosslinking group is composed only of a hydroxymethyl group or an alkoxymethyl group, and does not include a crosslinking compound containing other crosslinking groups, such as an epoxy group (oxirane ring). The crosslinking agent (C1) can be used alone or in combination of two or more.
[0136] The hydroxymethyl or alkoxymethyl is -CH 2 The base represented by OR.
[0137] In the above formula, R is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an acyl group having 2 to 10 carbon atoms, preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group include methyl, ethyl, propyl, and butyl. Examples of the acyl group include acetyl. Here, -CH 2 The gene represented by OR is acidic and the methylene group is activated, and has high reactivity with the phenolic hydroxyl group of the polymer (A) or the ortho position thereof, so that the crosslinking reaction proceeds easily.
[0138] Examples of the crosslinkable compound (C1) include phenol compounds containing a methylol group, phenol compounds containing an alkylmethylol group, and phenol compounds containing an acyloxymethyl group. Specifically, the following compounds are preferred.
[0139] [Chemistry 12]
[0140]
[0141] Examples of crosslinking compounds (C1) other than the above compounds include nitrogen compounds such as polymethylolated melamine, polymethylolated glycoluril, polymethylolated guanamine, and polymethylolated urea; active hydroxymethyl groups (CH bonds to nitrogen atoms) in the above nitrogen compounds; 2 A compound in which all or part of a hydroxymethyl group (OH group) is alkyl-etherified or acyloxylated. Here, examples of the alkyl group constituting the alkyl ether include methyl, ethyl, propyl, and butyl, which may be the same as or different from each other. In addition, an active hydroxymethyl group that is not alkyl-etherified or acyloxylated may self-condense within one molecule or condense between two molecules, and as a result, an oligomer component may be formed.
[0142] Examples of the crosslinkable compound (C1) include crosslinking agents described in JP-A-6-180501, JP-A-2006-178059, and JP-A-2012-226297. Specifically, examples include melamine-based crosslinking agents such as polymethylolated melamine, hexamethoxymethyl melamine, hexaethoxymethyl melamine, hexapropoxymethyl melamine, and hexabutoxymethyl melamine; glycoluril-based crosslinking agents such as polymethylolated glycoluril, tetramethoxymethyl glycoluril, and tetrabutoxymethyl glycoluril; compounds in which guanamines such as 3,9-bis[2-(3,5-diamino-2,4,6-triazaphenyl)ethyl]2,4,8,10-tetraoxospiro[5.5]undecane and 3,9-bis[2-(3,5-diamino-2,4,6-triazaphenyl)propyl]2,4,8,10-tetraoxospiro[5.5]undecane are hydroxymethylated; and guanamine-based crosslinking agents such as compounds in which all or part of the active methylol groups in the above compounds are alkyl-etherified or acyloxylated. Among these, melamine-based crosslinking agents and guanamine-based crosslinking agents are preferred.
[0143] Specifically, the following compounds are preferred as the crosslinkable compound (C1).
[0144] [Chemistry 13]
[0145]
[0146] In addition, in the present composition, as a crosslinking agent (C), in addition to the crosslinking compound (C1), an epoxy compound (C2) may also be included. In the present invention, the epoxy compound (C2) is a compound containing an epoxy group (oxirane ring) as a crosslinking group, and even if it is a compound containing a hydroxymethyl group or an alkoxymethyl group, as long as it contains an epoxy group, it is equivalent to the epoxy compound (C2). That is, the epoxy compound (C2) is different from the crosslinking compound (C1). The crosslinking agent (C2) can be used alone, or two or more can be used in combination.
[0147] Examples of the epoxy compound (C2) include phenol novolac type epoxy resins, cresol novolac type epoxy resins, naphthol novolac type epoxy resins, naphthol-phenol co-condensation novolac type epoxy resins, naphthol-cresol co-condensation novolac type epoxy resins, bisphenol type epoxy resins, biphenyl type epoxy resins, trisphenol type epoxy resins, tetraphenol type epoxy resins, phenol-xylylene type epoxy resins, naphthol-xylylene type epoxy resins, phenol-dicyclopentadiene type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, resorcin type epoxy resins, hydroquinone type epoxy resins, catechol type epoxy resins, dihydroxynaphthalene type epoxy resins, alicyclic epoxy resins, and aliphatic epoxy resins.
[0148] The epoxy compound (C2) is preferably an alicyclic epoxy resin or an aliphatic epoxy resin in terms of solvent solubility. Specific examples of such epoxy compounds (C2) include pentaerythritol glycidyl ether (commercial product example: manufactured by Nagase ChemteX Co., Ltd., trade name: Denacol EX411), trimethylolpropane polyglycidyl ether (commercial product example: manufactured by Nagase ChemteX Co., Ltd., trade name: Denacol EX321, 321L), glycerol polyglycidyl ether (commercial product example: manufactured by Nagase ChemteX Co., Ltd., trade name: Denacol EX313, EX314), neopentyl glycol diglycidyl ether (commercial product example: manufactured by Nagase ChemteX Co., Ltd., trade name: Denacol EX314), (Product name: Denacol EX211, manufactured by Nagase ChemteX Co., Ltd.), ethylene / polyethylene glycol diglycidyl ether (Product examples: Denacol EX810, 850, manufactured by Nagase ChemteX Co., Ltd.), propylene / polypropylene glycol diglycidyl ether (Product examples: Denacol EX911, 941, 920, manufactured by Nagase ChemteX Co., Ltd.), 1,6-hexanediol diglycidyl ether (Product examples: Denacol EX212, manufactured by Nagase ChemteX Co., Ltd.), sorbitol polyglycidyl ether (Product examples: Denacol EX911, 941, 920, manufactured by Nagase ChemteX Co., Ltd.), (commercially available product example: manufactured by Kyoei Co., Ltd., trade name: Epolight 70P), trimethylolpropane triglycidyl ether (commercially available product example: manufactured by Kyoei Co., Ltd., trade name: Epolight 100MF).
[0149] Furthermore, as a crosslinking agent (C), other crosslinking agents (C3) other than the crosslinking compound (C1) and the epoxy compound (C2) may also be used within the scope of not damaging the purpose and characteristics of the present invention. As other crosslinking agents (C3), for example, compounds containing oxetane rings, compounds containing oxazoline rings, compounds containing isocyanate groups (including compounds formed by block formation), compounds containing maleimide groups, and compounds containing cyanate groups can be listed. One type of crosslinking agent (C3) can be used, or two or more types can be used in combination.
[0150] In the present composition, the content of the crosslinking agent (C) is usually 1 to 60 parts by mass, preferably 3 to 50 parts by mass, and more preferably 5 to 40 parts by mass, relative to 100 parts by mass of the polymer (A). If the content of the crosslinking agent (C) is within the above range, a cured film having excellent tensile elongation or PCT resistance can be formed. In addition, the composition has excellent curability.
[0151] When an epoxy compound (C2) is used in addition to the crosslinking compound (C1) as the crosslinking agent (C), the epoxy compound (C2) is preferably less than 50% by mass in 100% by mass of the crosslinking agent (C). When the epoxy compound (C2) is used, chemical resistance tends to be improved.
[0152] <Solvent(D)>
[0153] The present composition contains a solvent (D). By using a solvent (D), the handleability of the present composition can be improved, or the viscosity or storage stability can be adjusted.
[0154] The solvent (D) is not particularly limited as long as it is an organic solvent that can dissolve or disperse the components such as the polymer (A), the compound (B) and the crosslinking agent (C). Examples of the solvent (D) include ketone solvents, alcohol solvents, ether solvents, ester solvents, amide solvents, hydrocarbon solvents, and lactone solvents. As the solvent (D), it is preferred that at least one selected from the group consisting of an amide solvent and a lactone solvent is included because of its excellent solubility.
[0155] Examples of the amide solvent include cyclic amide solvents such as N-methyl-2-pyrrolidone (NMP) and dimethylimidazolidinone (DMI), and examples of the lactone solvent include cyclic lactone solvents such as γ-butyrolactone (GBL).
[0156] The solvent (D) may be used alone or in combination of two or more.
[0157] The content of the solvent (D) in the present composition is an amount such that the solid content concentration in the composition is usually 10% by mass to 50% by mass.
[0158] <Other ingredients>
[0159] In addition to the above-mentioned components, the present composition may also contain other components within the range that does not impair the purpose and characteristics of the present invention. Examples of other components include polymers other than polymer (A), low molecular weight phenol compounds, silane coupling agents, rust inhibitors, adhesion aids, crosslinked microparticles, leveling agents, sensitizers, inorganic fillers, and quenchers.
[0160] <Method for producing photosensitive resin composition>
[0161] The present composition can be produced by uniformly mixing the components constituting the present composition using a conventional method. In addition, after uniformly mixing the components, the obtained mixture can be filtered through a filter or the like to remove foreign matter.
[0162] <Characteristics of the photosensitive resin composition>
[0163] The tensile elongation and PCT tolerance of the patterned resin film formed by curing the present composition are excellent. In order to obtain such characteristics, the i-ray transmittance, tensile elongation and PCT tolerance of the polymer used are preferably excellent, and from the viewpoint of the above, polymer (A) is preferred. Furthermore, by introducing a phenolic hydroxyl group or a high hydrophilic polar functional group into the polymer (A) in the repeating structural unit of the polymer or at the polymer end, so that when using an aqueous solution containing an alkaline compound as a developer, it is easy to appropriately adjust the solubility relative to the developer, in addition, it is also possible to adjust the curability based on the reaction with the crosslinking agent (C).
[0164] [Resin film having a pattern]
[0165] The resin film with a pattern (patterned resin film) of one embodiment of the present invention is formed by curing the present composition. Specifically, it is obtained by the manufacturing method described below, and the patterned resin film can be preferably used as an insulating film (for example: surface protection film, interlayer insulating film, planarization film) possessed by a semiconductor circuit substrate.
[0166] [Method for producing a resin film having a pattern]
[0167] The patterned resin film can be produced by the following method, which comprises: a step (1) of forming a coating film of the present composition on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using an alkaline developer.
[0168] <Process (1)>
[0169] In step (1), the present composition is usually applied to a substrate so that the thickness of the patterned resin film finally obtained is, for example, 0.1 μm to 100 μm. The substrate coated with the composition is heated using an oven or a hot plate, usually at 50° C. to 140° C. for 10 seconds to 360 seconds. In this way, a coating film containing the present composition is formed on the substrate.
[0170] Examples of the substrate include silicon wafers, compound semiconductor wafers, wafers with metal thin films, glass substrates, quartz substrates, ceramic substrates, aluminum substrates, and substrates having semiconductor chips on the surfaces of these substrates. Examples of the coating method include dipping, spraying, bar coating, roll coating, spin coating, curtain coating, gravure printing, screen coating, and inkjet.
[0171] <Process (2)>
[0172] In step (2), the coating film is selectively exposed using, for example, a contact aligner, a stepper, or a scanner. Specifically, the term "selectively" refers to exposure via a photomask having a predetermined mask pattern.
[0173] As exposure light, ultraviolet rays, visible light, etc. can be cited, and light with a wavelength of 200nm to 500nm is usually used (for example, i-ray (365nm)). The irradiation amount based on exposure varies depending on the type of each component in the composition, the mixing ratio, the thickness of the coating film, etc., and is usually 100mJ / cm 2 ~1500mJ / cm 2 .
[0174] <Step (3)>
[0175] In step (3), the resin film is developed with an alkaline developer to dissolve and remove the exposed portion, thereby forming a desired pattern on the substrate. Examples of the developing method include a shower developing method, a spray developing method, an immersion developing method, and a liquid coating developing method. The developing conditions are, for example, 1 minute to 10 minutes at 5° C. to 40° C. In addition, after the resin film is developed with an alkaline developer, it can be washed with water and dried.
[0176] As the alkaline developer, for example, there can be mentioned an alkaline aqueous solution obtained by dissolving an alkaline compound such as sodium hydroxide, potassium hydroxide, ammonia water, tetramethylammonium hydroxide, choline, etc. in water at a concentration of 1% to 10% by mass. For example, a water-soluble organic solvent such as methanol or ethanol and a surfactant may be added in appropriate amounts to the alkaline aqueous solution.
[0177] The shape of the pattern in the patterned resin film is not particularly limited as long as it has a concavo-convex structure, and examples thereof include a line and space pattern, a dot pattern, a hole pattern, and a lattice pattern.
[0178] <Step (4)>
[0179] In order to fully demonstrate the characteristics as an insulating film, the method for manufacturing a patterned resin film according to one embodiment of the present invention may, after step (3), optionally include a step (4) of fully curing the patterned resin film by heat treatment (post-baking). The curing conditions are not particularly limited, and may be, for example, heated at a temperature of 100° C. to 350° C. for about 30 minutes to 10 hours depending on the use of the patterned resin film.
[0180] [Semiconductor circuit substrate]
[0181] By using the present composition, a semiconductor circuit substrate including the patterned resin film can be manufactured. The semiconductor circuit substrate has a patterned resin film formed from the present composition, preferably a patterned insulating film such as a surface protection film, an interlayer insulating film, and a planarizing film, and is therefore useful as a circuit substrate with high reliability.
[0182] Example
[0183] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples. In the following Examples and the like, "parts" are used to mean "parts by mass" unless otherwise specified.
[0184] <Polymer Synthesis>
[0185] The weight average molecular weight (Mw) of the polymers obtained in the following synthesis examples was measured by gel permeation chromatography (GPC) under the following conditions.
[0186] Column: Product name "TSKgel α-M" (manufactured by Tosoh Corporation)
[0187] Solvent: N-methyl-2-pyrrolidone (NMP)
[0188] Temperature: 40℃
[0189] Detection method: Refractive index method
[0190] ·Standard material: polystyrene
[0191] ·GPC device: Device name: "HLC-8320-GPC" (manufactured by Tosoh Co., Ltd.)
[0192] [Synthesis Example 1] Synthesis of polymer (A1)
[0193] Into a 100 mL three-necked flask including a reflux tube, 6.67 mmol of BzDAxx (manufactured by ENEOS (Co., Ltd.), the following formula (a1-1)) as an acid anhydride and 19.89 g of N-methyl-2-pyrrolidone (NMP) as a polymerization solvent were placed, and stirred and dissolved under a nitrogen environment. 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 1.67 mmol of 1,3-bis(4-aminophenoxy)propane were added as diamines, and the mixture was stirred at 60°C for 1 hour and then at 180°C for 4 hours. After cooling to room temperature, the reaction solution was poured into 500 mL of distilled water to obtain a white solid component. The solid component was separated by filtration, washed three times with distilled water, and then vacuum dried at 70°C for 48 hours to obtain a polymer (A1). By 1 The obtained polymer (A1) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A1) was 601,900.
[0194] [Chemistry 14]
[0195]
[0196] [Synthesis Example 2] Synthesis of polymer (A2)
[0197] In Synthesis Example 1, the same operation as in Synthesis Example 1 was performed except that the diamine used was set to 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 1.67 mmol of ED-900 (manufactured by Huntsman, the following formula (b2-2)), and the polymerization solvent was set to 24.16 g of NMP, to obtain a polymer (A2). 1 The obtained polymer (A2) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A2) was 637,700.
[0198] [Chemistry 15]
[0199]
[0200] [Synthesis Example 3] Synthesis of polymer (A3)
[0201] In Synthesis Example 1, except that the acid anhydride used was 6.67 mmol of PPHT (manufactured by Nippon Seika Co., Ltd., formula (a1-2) below) and the polymerization solvent was 21.54 g of NMP, the same operation as in Synthesis Example 1 was performed to obtain a polymer (A3). 1The obtained polymer (A3) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A3) was 634,900.
[0202] [Chemistry 16]
[0203]
[0204] [Synthesis Example 4] Synthesis of polymer (A4)
[0205] In Synthesis Example 3, except that the diamine used was 4.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 2.67 mmol of 1,3-bis(4-aminophenoxy)propane, and the polymerization solvent was 21.11 g of NMP, the same operation as Synthesis Example 3 was performed to obtain a polymer (A4). 1 The obtained polymer (A4) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A4) was 657,500.
[0206] [Synthesis Example 5] Synthesis of polymer (A5)
[0207] Into a 100 mL three-necked flask including a reflux tube, 7.41 mmol of BzDAxx as an acid anhydride and 25.37 g of NMP as a polymerization solvent were placed, and stirred and dissolved under a nitrogen environment. 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 1.67 mmol of ED-900 as diamines, and 1.48 mmol of 3-aminophenol as a terminal modifier were added thereto, and the mixture was stirred at 60°C for 1 hour, and then stirred at 180°C for 4 hours. After cooling to room temperature, the reaction solution was poured into 500 mL of distilled water to obtain a white solid component. The solid component was separated by filtration, washed three times with distilled water, and then vacuum dried at 70°C for 48 hours to obtain a polymer (A5). By 1 The obtained polymer (A5) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A5) was 29,200.
[0208] [Synthesis Example 6] Synthesis of polymer (A6)
[0209] In Synthesis Example 5, the acid anhydride used was set to 9.26 mmol of PPHT, the diamine was set to 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 3.33 mmol of 1,3-bis(4-aminophenoxy)propane, the terminal modifier was set to 1.85 mmol of 3-aminophenol, and the polymerization solvent was set to 28.12 g of NMP. Except for this, the same operation as Synthesis Example 5 was performed to obtain a polymer (A6). 1 The obtained polymer (A6) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A6) was 24,700.
[0210] [Synthesis Example 7] Synthesis of polymer (A7)
[0211] In a 100mL three-necked flask including a reflux tube, 7.41mmol of BzDAxx, 10.00g of methanol, and 0.5mL of pyridine were placed as an acid anhydride, and refluxed and stirred for 5 hours under a nitrogen environment. After cooling to room temperature, it was transferred to an eggplant-shaped flask, and the methanol was distilled off using an evaporator to obtain the hemimethyl ester of BzDAxx. Next, the total amount of the obtained hemimethyl ester of BzDAxx and 20g of NMP were placed in a 100mL three-necked flask A, stirred and dissolved under a nitrogen environment, and cooled using an ice bath. After adding 15.56mmol of thionyl chloride, the ice bath was removed and stirred at 50°C for 1 hour. Then, to another 100mL three-necked flask B, 5.00mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 1.67mmol of 1,3-bis(4-aminophenoxy)propane as diamines, 1.48mmol of 3-aminophenol as a terminal modifier, 15.00g of NMP, and 0.5g of pyridine were added, stirred and dissolved under a nitrogen environment, and cooled with an ice bath. After transferring the contents of flask A cooled to room temperature to flask B using a Teflon (registered trademark) tube and nitrogen, the ice bath was removed and stirred at room temperature for 3 hours. The reaction solution was poured into 500mL of distilled water to obtain a white solid component. The solid component was separated by filtration, washed three times with distilled water, and then vacuum dried at 70°C for 48 hours to obtain a polymer (A7). By 1 The obtained polymer (A7) was analyzed by H-NMR and the like, and the methyl esterification rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A7) was 27,800.
[0212] [Synthesis Example 8] Synthesis of polymer (A8)
[0213] In Synthesis Example 6, except that the polymerization solvent used was changed to 28.12 g of 1,3-dimethyl-2-imidazolidinone (DMI), the same operation as Synthesis Example 6 was carried out to obtain a polymer (A8). 1 The obtained polymer (A8) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A8) was 24,000.
[0214] [Synthesis Example 9] Synthesis of polymer (A9)
[0215] In a 100 mL three-necked flask including a stoppered connecting tube and a reflux tube, 9.26 mmol of PPHT as an acid anhydride and 28.12 g of γ-butyrolactone (GBL) as a polymerization solvent were placed and stirred and suspended under a nitrogen atmosphere. 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 3.33 mmol of 1,3-bis(4-aminophenoxy)propane as diamines and 1.85 mmol of 3-aminophenol as a terminal modifier were added thereto and stirred at 90° C. for 1 hour.
[0216] Next, 14.06 g of pyridine as an imidization catalyst was added, stirred at 115°C for 2 hours, and then stirred at 180°C for 2 hours while removing pyridine from the system. After cooling to room temperature, the reaction solution was added to 500 mL of distilled water to obtain a white solid component. The solid component was filtered and separated, washed with distilled water three times, and then vacuum dried at 70°C for 48 hours to obtain a polymer (A9). 1 The obtained polymer (A9) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) was 23,900.
[0217] [Synthesis Example 10] Synthesis of polymer (A10)
[0218] In Synthesis Example 6, except that the acid anhydride used was 6.95 mmol of PPHT and 2.31 mmol of 4,4′-oxydiphthalic anhydride, the same operation as in Synthesis Example 6 was carried out to obtain a polymer (A10). 1 The obtained polymer (A10) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A10) was 25,100.
[0219] [Synthesis Example 11] Synthesis of polymer (A11)
[0220] In Synthesis Example 6, except that the acid anhydride used was set to 9.26 mmol of PPHT, and the diamine used was set to 5.00 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2.50 mmol of 1,3-bis(4-aminophenoxy)propane, and 0.83 mmol of 1,3-bis(3-aminopropyl)tetramethyldisiloxane, the same operation as Synthesis Example 6 was performed to obtain a polymer (A11). 1 The obtained polymer (A11) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A11) was 23,200.
[0221] [Comparative Synthesis Example 1] Synthesis of Polymer (RA1)
[0222] Into a 100mL three-necked flask including a reflux tube, 12.00mmol of 4,4'-oxydiphthalic anhydride as an acid anhydride and 32.47g of NMP as a polymerization solvent were placed, and stirred and dissolved under a nitrogen environment. 12.00mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane as a diamine was added thereto, and after stirring at 60°C for 1 hour, it was further stirred at 180°C for 4 hours. After cooling to room temperature, the reaction solution was poured into 700mL of distilled water to obtain a white solid component. The solid component was separated by filtration, washed with distilled water 3 times, and then vacuum dried at 70°C for 48 hours to obtain a polymer (RA1). By 1 The obtained polymer (RA1) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA1) was 871,400.
[0223] [Comparative Synthesis Example 2] Synthesis of Polymer (RA2)
[0224] In Comparative Synthesis Example 1, except that the acid anhydride used was set to 15.00 mmol of 4,4'-oxydiphthalic anhydride, the diamine was set to 11.25 mmol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 3.75 mmol of 1,3-bis(4-aminophenoxy)propane, and the polymerization solvent was set to 38.97 g of NMP, a polymer (RA2) was obtained by the same operation as in Comparative Synthesis Example 1. 1 The obtained polymer (RA2) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA2) was 969,700.
[0225] [Comparative Synthesis Example 3] Synthesis of Polymer (RA3)
[0226] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and the polymerization solvent was 47.01 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA3). 1 The obtained polymer (RA3) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA3) was 755,900.
[0227] [Comparative Synthesis Example 4] Synthesis of Polymer (RA4)
[0228] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride and the polymerization solvent was 38.01 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA4). 1 The obtained polymer (RA4) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA4) was 855,100.
[0229] [Comparative Synthesis Example 5] Synthesis of Polymer (RA5)
[0230] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of 1,2,3,4-butanetetracarboxylic dianhydride and the polymerization solvent was 32.24 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA5). 1 The obtained polymer (RA5) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA5) was 589,100.
[0231] [Comparative Synthesis Example 6] Synthesis of Polymer (RA6)
[0232] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of 1,2,3,4-cyclobutanetetracarboxylic dianhydride and the polymerization solvent was 32.12 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA6). 1 The obtained polymer (RA6) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA6) was 634,800.
[0233] [Comparative Synthesis Example 7] Synthesis of Polymer (RA7)
[0234] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of 1,2,4,5-cyclohexanetetracarboxylic dianhydride and the polymerization solvent was 33.81 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA7). 1 The obtained polymer (RA7) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA7) was 845,300.
[0235] [Comparative Synthesis Example 8] Synthesis of Polymer (RA8)
[0236] In Comparative Synthesis Example 2, except that the acid anhydride used was 15.00 mmol of dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride and the polymerization solvent was 38.74 g of NMP, the same operation as in Comparative Synthesis Example 2 was carried out to obtain a polymer (RA8). 1 The obtained polymer (RA8) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA8) was 672,600.
[0237] [Comparative Synthesis Example 9] Synthesis of Polymer (RA9)
[0238] In Synthesis Example 6, except that the acid anhydride used was changed to 9.26 mmol of 4,4'-oxydiphthalic anhydride, the same operation as in Synthesis Example 6 was carried out to obtain a polymer (RA9). 1 The obtained polymer (RA9) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA9) was 24,000.
[0239] The obtained polymer was evaluated as follows.
[0240] Tensile elongation
[0241] A 20% by weight NMP solution of the polymer obtained in the synthesis example or the comparative synthesis example is applied to a substrate with a release material, and then heated in an oven at 200°C for 1 hour (wherein the polymer (A7) is heated at 300°C for 1 hour) and dried to prepare a coating film with a thickness of 20 μm.
[0242] The substrate with a release material is peeled off by post-baking and heating the coating to obtain a resin film with a thickness of 20 μm. The obtained resin film is cut into strips of 5 cm in length and 0.5 cm in width to make a tensile test piece. The tensile elongation at break (%) of the tensile test piece is measured using a tensile compression tester (product name "AGS-500NX", manufactured by Shimadzu Corporation). The measurement conditions are: chuck distance = 2.5 cm, tensile speed = 5 mm / min, and measurement temperature = 23°C. The average value of the 5 measured values is set as "elongation (polymer)" and evaluated according to the following criteria.
[0243] ○: Elongation is 50% or more
[0244] ×: Elongation is less than 50% or cannot be measured
[0245] "PCT Patience"
[0246] The prepared tensile test piece was exposed to an environment of 130°C / 85%RH / 96hr. The exposed test piece was dissolved in NMP, and the Mw was measured under the same measurement conditions as the weight average molecular weight (Mw) of the polymer based on the GPC method. The Mw after polymer synthesis was set as "Mw (initial value)", and the Mw of the test piece after the PCT test was set as "Mw (after PCT test)".
[0247] The "molecular weight change" was calculated from the measured Mw (initial value) and Mw (after PCT test) using the following formula: "Mw (initial value) - Mw (after PCT test)" / "Mw (initial value)" × 100 = molecular weight change (%), and evaluated according to the following criteria.
[0248] ○: Molecular weight change is less than 30%
[0249] ×: Molecular weight changes by 30% or more or cannot be measured
[0250] 《i-ray transparency》
[0251] A 20 mass % NMP solution of the polymer obtained in the synthesis example or the comparative synthesis example was applied on a glass substrate, and then heated in an oven at 200° C. for 1 hour (wherein the polymer (A7) was heated at 300° C. for 1 hour) to prepare a coating film with a film thickness of 10 μm.
[0252] The transmittance of the produced coating film at a wavelength of 365 nm was measured using a spectrophotometer (manufactured by Shimadzu Corporation, model number “SolidSpec 3700”), and evaluated based on the following criteria.
[0253] ○: Transmittance is 80% or more
[0254] ×: Transmittance is less than 80% or cannot be measured
[0255] The types and amounts of monomers used in Synthesis Examples 1 to 11 and Comparative Synthesis Examples 1 to 9, various physical properties of the obtained polymers, and the results of the various evaluations are shown in the following Tables 1-1 and 1-2.
[0256]
[0257]
[0258] The details of the acid anhydrides and diamines used in Table 1-1 and Table 1-2 are shown below.
[0259] ·Acid anhydride
[0260] (a1-1): BzDAxx (manufactured by ENEOS)
[0261] (a1-2): PPHT (manufactured by Nippon Seika Co., Ltd.)
[0262] (a2-1): 4,4'-oxydiphthalic anhydride
[0263] (a2-2): 4,4'-(hexafluoroisopropylidene)diphthalic anhydride
[0264] (a2-3): 3,3',4,4'-biphenyltetracarboxylic dianhydride
[0265] (a2-4): 1,2,3,4-butanetetracarboxylic dianhydride
[0266] (a2-5): 1,2,3,4-cyclobutanetetracarboxylic dianhydride
[0267] (a2-6): 1,2,4,5-cyclohexanetetracarboxylic dianhydride
[0268] (a2-7): dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride
[0269] ·Diamine
[0270] (b1-1): 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane
[0271] (b2-1): 1,3-bis(4-aminophenoxy)propane
[0272] (b2-2): ED-900 (polyether diamine, manufactured by Huntsman)
[0273] (b2-3): 1,3-bis(3-aminopropyl)tetramethyldisiloxane
[0274] <Production of photosensitive resin composition>
[0275] [Example 1 to Example 14 and Comparative Example 1, Comparative Example 2]
[0276] The polymers (polymers (A5) to (A11), polymer (RA9)) shown in Table 2 below, naphthoquinonediazide compounds, crosslinking agents, and other components were uniformly mixed in the amounts shown in Table 2 using the solvents shown in Table 2 to give the solid content concentrations shown in Table 2, and the photosensitive resin compositions of Examples 1 to 14 and Comparative Examples 1 and 2 were prepared at the curing temperatures and curing times shown in Table 2. The obtained photosensitive resin compositions were evaluated as follows. The results are shown in Table 2.
[0277] 《Solubility of the exposed part》
[0278] The photosensitive resin composition was spin-coated on a 6-inch silicon wafer, and then heated and dried at 110° C. for 5 minutes using a hot plate to prepare a coating film with a thickness of 10 μm. Subsequently, an alignment machine (manufactured by Suss Microtec Co., Ltd., model “MA-150”) was used, and the exposure wavelengths of g-ray, h-ray, and i-ray were used, and the exposure amount was 1000 mJ / cm through a photomask. 2 The coating film was exposed to ultraviolet rays from a high pressure mercury lamp in a manner of . The solubility of the exposed portion in a developer (aqueous solution of tetramethylammonium hydroxide at a concentration of 2.38 wt %) was observed and evaluated based on the following criteria.
[0279] ○: Complete dissolution of the exposed part within 120 seconds
[0280] ×: Complete dissolution of the exposed part exceeds 120 seconds
[0281] Tensile elongation
[0282] The photosensitive resin composition was applied onto a substrate with a release material, and then heated in an oven at 110° C. for 5 minutes to prepare a coating film. Then, an alignment machine (manufactured by Suss Microtec Co., Ltd., model “MA-150”) was used to expose the film at a wavelength of 365 nm at an exposure dose of 500 mJ / cm 2 The entire surface of the coating film was irradiated with ultraviolet rays from a high pressure mercury lamp in a manner. Subsequently, the coating film was heated in an oven under a nitrogen atmosphere under the heating conditions (curing temperature, curing time) shown in Table 2.
[0283] The substrate with a release material is peeled off by post-baking and heating the coating to obtain a resin film with a thickness of 10 μm. The obtained resin film is cut into strips of 5 cm in length and 0.5 cm in width to make a tensile test piece. The tensile breaking elongation (%) of the long strip resin film is measured using a tensile compression tester (product name "AGS-500NX", manufactured by Shimadzu Corporation (Co., Ltd.)). The measurement conditions are: chuck distance = 2.5 cm, tensile speed = 5 mm / min, and measurement temperature = 23°C. The average value of the 5 measured values is set as "elongation (composition)" and evaluated according to the following criteria.
[0284] ◎: Elongation is 50% or more
[0285] ○: Elongation is 30% or more and less than 50%
[0286] ×: Elongation is less than 30% or cannot be measured
[0287] "PCT Patience"
[0288] The prepared tensile test piece was subjected to three reflows (maximum temperature 260°C) in the atmosphere and then exposed to an environment of 130°C / 85%RH / 96hr. The tensile elongation of the test piece after exposure was measured in the same manner as in "Elongation (composition)" and evaluated according to the following criteria.
[0289] ○: Elongation is 20% or more
[0290] ×: Elongation is less than 20% or cannot be measured
[0291]
[0292] The details of the compound (B), the crosslinking compound (C1), the epoxy compound (C2), and the solvent (D) used in Table 2 are shown below.
[0293] Compound (B)
[0294] (B1): Condensate of 4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol and 1,2-naphthoquinonediazide-5-sulfonic acid (molar ratio = 1.0:2.0)
[0295] ·Crosslinking compound (C1)
[0296] (C1-1): HMOM-TPPA (4,4'-[1-[4-[1-[4-hydroxy-3,5-bis(methoxymethyl)phenyl]-1-methylethyl]phenyl]ethylidene]bis[2,6-bis(methoxymethyl)phenol], manufactured by Honshu Chemical Industry Co., Ltd.)
[0297] (C1-2): TMOM-BP (3,3',5,5'-tetrakis(methoxymethyl)-[1,1'-biphenyl]-4,4'-diol, manufactured by Honshu Chemical Industry Co., Ltd.)
[0298] (C1-3): HMOM-TPHAP (4,4',4"-ethylenetri[2,6-(methoxymethyl)phenol], manufactured by Honshu Chemical Industry Co., Ltd.)
[0299] (C1-4): Nikalac MW-100LM (hexamethoxymethylated melamine, manufactured by Sanwa Chemical Co., Ltd.)
[0300] ·Epoxy compounds (C2)
[0301] (C2-1): Denacol EX-321L (trimethylolpropane polyglycidyl ether, manufactured by Nagase Chemtex Co., Ltd.)
[0302] (C2-2): EXA-4850-150 (bisphenol A epoxy resin, manufactured by DIC Corporation)
[0303] ·Solvent(D)
[0304] (D1): N-methyl-2-pyrrolidone (NMP)
[0305] (D2): 1,3-dimethyl-2-imidazolidinone (DMI)
[0306] (D3): γ-butyrolactone (GBL).
Claims
1. A photosensitive resin composition comprising: (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor; (B) naphthoquinone diazide compounds; (C1) a crosslinking compound having a hydroxymethyl group or an alkoxymethyl group; and (D)solvent, The polymer (A) comprises a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine, The structural unit (a) includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1). [Chemistry 1] [In the above formula (1), L independently represents a single bond, an ester bond, or an amide bond, R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3 an alkylene group having 1 to 4 carbon atoms bonded to each other, n 1 and n 2 Each independently represents an integer from 0 to 3 (wherein, In the same ring, n 1 With n 2 At least one of is an integer greater than 1. ), Y 1 Represents a structure represented by the following formula (Y1) or formula (Y2); *-Ar 1 -*…(Y1) *-On 2 -Y 2 -On 2 -*…(Y2) In the above formula (Y1) and formula (Y2), * represents a bond with respect to L in the above formula (1), Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms from an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms, Y in the formula (Y2) 2 is a single bond, an oxygen atom, a sulfur atom, or at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group. 2 . The photosensitive resin composition according to claim 1 , wherein the polymer (A) has a phenolic hydroxyl group at a polymer terminal. 3 . The photosensitive resin composition according to claim 1 , wherein the structural unit (b) derived from a diamine comprises a structural unit (b1) derived from a diamine having a phenolic hydroxyl group.
4. The photosensitive resin composition according to claim 1, further comprising (C2) an epoxy compound (wherein: Different from the cross-linking compound (C1)).
5. A method for producing a resin film having a pattern, comprising: a step (1) of forming a coating film of the photosensitive resin composition according to any one of claims 1 to 4 on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using an alkaline developer. 6 . A resin film having a pattern, which is obtained by curing the photosensitive resin composition according to claim 1 .
7. A semiconductor circuit substrate comprising the resin film having a pattern according to claim 6.