All-solid-state battery
By forming the laser-treated deactivated area and laser cutting technology on the positive electrode plate of the all-solid-state battery, the problems of uneven precipitation of lithium ions and edge damage are solved, effective control and short-circuit protection of lithium ions are achieved, and the battery is improved stability and safety.
Patent Information
- Application Number
- CN202280094822.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-14
- Filing Date
- 2022-11-16
- Publication Date
- 2024-11-26
AI Technical Summary
The uneven precipitation of lithium ions during charging and discharging of all-solid-state batteries leads to internal short circuits, and the edges of the positive electrode plate are easily damaged, which is prone to short circuits under high voltage conditions.
The deactivated area of laser processing is formed at the peripheral edge of the positive electrode plate, preventing the entry and exit of lithium ions, and reducing edge damage by laser cutting.
It effectively prevents the occurrence of short circuits under high voltage conditions due to damage to the edge of the positive electrode plate and improves the stability and safety of the battery.
Smart Images

Figure CN119032448A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery, and more particularly to an all-solid-state battery having an electrode structure that prevents an internal short circuit so that the battery can operate stably. Background Art
[0002] All-solid-state batteries include a positive electrode plate, a solid electrolyte layer, and a negative electrode plate. The solid electrolyte layer is a medium that conducts lithium ions. In the case of a lithium precipitation type all-solid-state battery, lithium ions moving from the positive electrode are precipitated as metal and accumulated on the negative electrode plate, and when charged, lithium metal is precipitated on the negative electrode plate regardless of whether there is an active substance in the negative electrode plate.
[0003] The all-solid-state battery with a deposited negative electrode plate has no casing, and during charging, lithium ions moved from the positive electrode plate are deposited on the negative electrode plate, and during discharging, lithium ions accumulated on the negative electrode plate are dissociated from the negative electrode plate and move back to the positive electrode plate.
[0004] When charging, lithium is deposited on the negative electrode plate, and the volume of the all-solid-state battery expands, so in a free state without applying pressure to the all-solid-state battery, lithium deposition becomes uneven. As charging and discharging proceed, the uneven deposition of lithium increases, and the solid electrolyte layer is partially destroyed, which can cause an internal short circuit. In order to solve the unevenness of lithium deposition, pressure is applied to the outside of the all-solid-state battery.
[0005] At the same time, a physical scraper is used to punch the continuously supplied electrode plates into unit electrode plates of appropriate shapes, thereby forming positive electrode plates and negative electrode plates. The positive electrode plates and negative electrode plates formed by punching may be damaged due to burrs on the edges of the plates. In other words, the active material may fall off from the edges and cause a short circuit in the battery cell.
[0006] In addition, the edge of the positive electrode plate can be abnormally activated due to the high pressure under the battery manufacturing conditions, which can easily cause a short circuit in the battery. The current density is concentrated at the edge of the positive electrode plate compared to other parts. Therefore, it is necessary to manage the edges of the positive electrode plate, which are easily affected by pressure, because the possibility of a short circuit is higher at the edges. Summary of the invention
[0007] Technical issues
[0008] One embodiment provides an all-solid-state battery that prevents short circuits caused by damage to the edges of a positive electrode plate. In addition, one embodiment provides an all-solid-state battery that prevents the edges of a positive electrode plate from short circuiting under high voltage conditions.
[0009] Technical Solution
[0010] An all-solid-state battery according to an embodiment may include: a positive electrode plate having an active material on a positive electrode current collector, a solid electrolyte layer disposed on one side of the positive electrode plate, and a negative electrode plate disposed on one side of the solid electrolyte layer, wherein the positive electrode plate may include an activated region of the active material and a deactivated region treated by laser on an outer boundary edge of the activated region.
[0011] The positive electrode plate may be formed by laser cutting a positive electrode current collector on which an active material is continuously coated together with an active material layer.
[0012] The deactivation region can be configured to block the entry and exit of lithium ions.
[0013] The deactivated region may be configured to block the entry and exit of lithium ions through deformation of the crystal structure of the active material on the positive electrode plate.
[0014] The deactivation region may be configured to block entry and exit of lithium ions through denaturation of the solid electrolyte in the solid electrolyte layer.
[0015] In the deactivated region, the positive electrode current collector may melt and be modified to be included in the active material.
[0016] The positive electrode plate may be formed by laser cutting a positive electrode current collector on which an active material is pattern-coated.
[0017] The inactivation area may be formed in a raised portion on the peripheral edge.
[0018] The inactivation region may be formed to have a width of 0.1 mm to 1 mm.
[0019] Beneficial Effects
[0020] The all-solid-state battery according to the embodiment has a deactivation area of a predetermined range by laser cutting the positive electrode plate and by laser processing the active material on the peripheral edge of the positive electrode plate, and accordingly, can prevent short circuits caused by damage to the edges of the positive electrode plates and short circuits at the edges of the positive electrode plates due to high voltage conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A cross-sectional view showing a charging state of an all-solid-state battery according to an embodiment of the present invention.
[0022] Figure 2 For application Figure 1 Top view of the positive electrode plate.
[0023] Figure 3 For along Figure 2 A cross-sectional view taken along line III-III.
[0024] Figure 4 An image of energy dispersive X-ray spectroscopy (EDS) for a cross section of a physically cut positive electrode plate is shown as a comparative example.
[0025] Figure 5 An electron microscope (SEM) image of a cross section of a laser-cut positive electrode plate is shown as an embodiment.
[0026] Figure 6 An image of energy dispersive X-ray spectroscopy (EDS) for a cross section of a laser-cut positive electrode plate is shown as an embodiment.
[0027] Figure 7 To show Figure 6 Figure 2. EDS analysis results of a first selected area of a cross section of a laser cut positive electrode plate.
[0028] Figure 8 To show Figure 6 Figure 2. EDS analysis results of a second selected area of a cross section of a laser cut positive electrode plate.
[0029] Fig. 9 To show Figure 6 Diagram of the EDS analysis results of the third selected area of the cross section of the laser-cut positive electrode plate.
[0030] Fig.10 To show Figure 6 Figure 2. EDS analysis results of a fourth selected area of a cross section of a laser cut positive electrode plate.
[0031] Fig.11 To show Figure 6 Figure 2. EDS analysis results of the fifth selected area of the cross section of the laser cut positive electrode plate.
[0032] Fig.12 An image of a cross section of a laser-cut positive electrode plate.
[0033] Fig.13 for Fig.12 Raman mapping image of a cross section of a laser-cut positive electrode plate.
[0034] Fig.14 : is a graph showing the results of Raman spectroscopic analysis in a cross section of a positive electrode plate physically cut as a comparative example.
[0035] Fig.15 : is a diagram showing the results of Raman spectroscopy analysis in a cross section of a positive electrode plate cut by laser, as an embodiment.
[0036] Fig.16 FIG. 1 is a cross-sectional view showing another embodiment of a positive electrode plate applied to an all-solid-state battery according to an embodiment of the present invention. DETAILED DESCRIPTION
[0037] The present disclosure will be described more fully below with reference to the attached drawings in which embodiments of the present disclosure are shown. As will be appreciated by those skilled in the art, the described embodiments may be modified in various ways, all without departing from the spirit or scope of the present disclosure. The drawings and descriptions are considered to be illustrative in nature, rather than restrictive. Throughout the specification, the same reference numerals represent the same elements.
[0038] Figure 1 It can be a cross-sectional view of a charging state of an all-solid-state battery according to an embodiment of the present invention. Figure 1 The all-solid-state battery of the embodiment may include: a positive electrode plate 11, a solid electrolyte layer 12 arranged on one side of the positive electrode plate 11, a negative electrode plate 13 arranged on one side of the solid electrolyte layer 12, and a buffer film 20 arranged on one side of the negative electrode plate 13.
[0039] The stacked structure of the positive electrode plate 11 , the solid electrolyte layer 12 , and the negative electrode plate 13 may form a unit cell. The unit cell may be formed as a single cell (not shown) that is charged and discharged at one side of the positive electrode plate 11 .
[0040] like Figure 1 As shown in FIG. 1 , the unit cell may be formed as a bi-cell charged and discharged at both sides of the positive electrode plate 11. The positive electrode plate 11 may be formed by laser cutting a positive electrode current collector 111 on which a positive active material is continuously coated together with positive active material layers 112 and 114.
[0041] Figure 2 For application Figure 1 A top view of the positive electrode plate, and Figure 3 For along Figure 2 At the same time, refer to Figure 1 to Figure 3 , the positive electrode plate 11 may include active material layers 112 and 114 formed by applying a positive active material on both surfaces of a positive electrode collector 111 made of aluminum.
[0042] The positive electrode active material layers 112 and 114 may include an activated region 112 of the positive electrode active material and an inactivated region 114 of the positive electrode active material. The inactivated region 114 is a portion processed by laser on the peripheral edge of the activated region 112, and may be formed by irradiating laser on the positive electrode active material on the periphery of the activated region 112 after forming an active material layer with the positive electrode active material.
[0043] That is, the activated region 112 enables lithium ions to enter and exit during charge and discharge, while the deactivated region 114 is formed in a predetermined range to block the entry and exit of lithium ions.
[0044] By irradiating the active material layer of the positive electrode plate 11 with laser, the inactivation region 114 can block the entry and exit of lithium ions by deformation of the crystal structure of the active material. In addition, when the focus of the laser is close to the positive electrode collector 111, the positive electrode collector 111 can be melted and deformed, so that the components of the positive electrode collector 111 can be included in the positive active material, so that the inactivation region 114 can block the entry and exit of lithium ions.
[0045] As an example, the inactivation region 114 is formed to have a width of 0.1 to 1 mm. If it is less than 0.1 mm, it may not be sufficient to function as an inactivation region due to its small area, and if it exceeds 1 mm, the capacity of the battery may be deteriorated due to its excessively large area.
[0046] In addition, the deactivated region can block the entry and exit of lithium ions by denaturing the solid electrolyte in the solid electrolyte layer. In this case, the solid electrolyte can be denatured by irradiating the laser to the outside of the solid electrolyte layer, and the solid electrolyte can be denatured by irradiating the laser to the outside of the solid electrolyte layer while laminating the solid electrolyte membrane to the active material layer of the negative electrode plate.
[0047] Even under high voltage conditions of the all-solid-state battery, the deactivated region 114 can prevent short circuits caused by the edges of the positive electrode plate 11. In addition, in order to prevent short circuits caused by damage to the edges of the positive electrode plate 11, the positive electrode plate 11 can be manufactured by laser cutting, and laser cutting will be described in detail below compared with physical cutting.
[0048] When the positive electrode plate 11 is manufactured by laser cutting, the occurrence of burrs on the edges of the positive electrode plate 11 can be minimized, and thus a short circuit due to damage of the edges of the positive electrode plate 11 can be minimized.
[0049] Figure 4 An image of energy dispersive X-ray spectroscopy (EDS) for a cross section of a positive electrode plate physically cut is shown as a comparative example. Table 1 shows an image of an energy dispersive X-ray spectroscopy (EDS) for a cross section of a positive electrode plate physically cut by using a scraper. Figure 4 EDS analysis results of the cross section of the positive electrode plate. The unit is atomic %.
[0050] K indicates the K edge of an element. The K edge is caused by the transition of electrons in the K shell of an atom. In spectroscopy, K is an energy band released after being activated when energy is applied to an element, and the type of the element is determined using this specific signal. Therefore, K represents a specific position value used to find the quantitative value of an element in energy dispersive X-ray spectroscopy (EDS).
[0051] [Table 1]
[0052] K Co K Al K Select Area 1 86.4 8.5 5.1 Select Area 2 87.5 8.7 3.7 Select Area 3 87.0 6.6 6.4 Select Area 4 85.8 8.9 5.3 Select Area 5 90.1 5.0 4.9
[0053] Figure 5 An electron microscope (SEM) image of a cross section of a laser-cut positive electrode plate is shown as an embodiment, and Figure 6 An image of energy dispersive X-ray spectroscopy (EDS) for a cross section of a laser-cut positive electrode plate is shown as an embodiment. Table 2 shows the Figure 5 and Figure 6 EDS analysis results of the cross section of the laser-cut positive electrode plate 11. The unit is atomic %.
[0054] [Table 2]
[0055] K Co K Al K Select Area 1 87.7 5.6 6.7 Select Area 2 90.0 6.0 4.0 Select Area 3 84.5 6.5 9.0 Select Area 4 54.6 5.0 40.4 Select Area 5 53.20 4.1 42.7
[0056] Figure 7 to Figure 11 : is a graph showing the EDS analysis results in the first to fifth selected regions of the cross section of the laser-cut positive electrode plate. The EDS analysis results are expressed as a relative value (au) of intensity relative to energy (eV).
[0057] refer to Figure 5 to Figure 11 , the positive active material formed on the cross section of the laser-cut positive electrode plate 11 is changed due to the irradiation of the laser. That is, in the laser-cut cross section, the positive electrode collector 111 may be melted and modified to be included in the positive active material. That is, the positive active material of the laser-cut cross section may be formed into an aluminum (Al) composite containing the positive electrode collector 111.
[0058] When Table 1 and Figure 4 Compared with Table 2 and Figure 5 When compared, the melted and pressed shape (MPS) of the positive electrode active material due to heat was observed in the laser cut section, but was not found in the physically cut section.
[0059] The melt and press shape (MPS) can prevent the edge of the laser-cut section of the positive electrode plate 11 from being damaged, that is, prevent the positive active material from falling off, thereby preventing an internal short circuit caused by the falling positive active material.
[0060] refer to Figure 6 , in the fourth selected region (selected region 4) and the fifth selected region (selected region 5) in the laser cut cross section of the positive electrode plate 11, the aluminum (Al) complex of the positive electrode current collector 111 is highly revealed due to heat.
[0061] That is, in the first to third selected regions (selected regions 1 to 3) on the positive electrode plate 11 away from the positive electrode current collector 111, the aluminum complex does not exceed 10%, while in the fourth selected region (selected region 4) and the fifth selected region (selected region 5) adjacent to the positive electrode current collector 111, the aluminum complex is found to be more than 20%. That is, in the laser cut cross section of the positive electrode plate 11, 40.4% of the aluminum complex is found in the fourth selected region (selected region 4), and 42.7% of the aluminum complex is found in the fifth selected region (selected region 5).
[0062] Fig.12 is an image of a cross section of a laser-cut positive electrode plate, and Fig.13 for Fig.12 Raman mapping image of a cut cross section of a laser-cut positive electrode plate. Fig.12 and Fig.13 , in the laser cut cross section of the positive electrode plate 11, the positive electrode active material was melted by heat, and a melt and pressed shape (MPS) was also observed.
[0063] The melt and press shape (MPS) can prevent the edge of the laser-cut section of the positive electrode plate 11 from being damaged, that is, prevent the positive active material from falling off, thereby preventing an internal short circuit caused by the falling positive active material.
[0064] Fig.14 is a graph showing the results of Raman spectroscopy analysis in a cross section of a physically cut positive electrode plate as a comparative example, and Fig.15 : is a diagram showing the results of Raman spectroscopy analysis in a cross section of a positive electrode plate cut by laser, as an embodiment. The results of Raman spectroscopy analysis are expressed as a relative value (au) of intensity to Raman shift.
[0065] refer to Figure 12 to Figure 15 , Fig.14 is a graph showing the results of Raman spectroscopy analysis in a cross section of a physically cut positive electrode plate as a comparative example, and Fig.15 The results of Raman spectroscopy analysis in the cross section of the laser-cut positive electrode plate 11 are shown as an embodiment.
[0066] Refer to Raman spectroscopy analysis, which is different from physical cutting cross-section (see Fig.14 ), in the laser cut section, at a Raman shift of 1100 cm -1 A new peak appears at Fig.15 ). It can be seen that this peak is related to the aluminum (Al) complex.
[0067] In addition, after laser cutting, it can be observed that the thickness direction of the positive electrode active material ( Fig.12A large amount of aluminum (Al) complex is generated in the middle of the positive electrode plate 11 in the vertical direction. The aluminum complex contained and observed in the positive electrode active material can prevent the edge of the positive electrode plate 11 from being damaged on the cross section, that is, prevent the positive electrode active material from falling off, thereby preventing a short circuit caused by the falling positive electrode active material.
[0068] Meanwhile, the deactivation region 114 provided on the edge of the positive electrode plate 11 may be formed in the positive electrode active material layer, similar to a structure formed on a laser-cut cross section by irradiating a laser on the edge. The deactivation region 114 may play a deactivating role in the movement of lithium ions during charging and discharging of the all-solid-state battery.
[0069] Return to reference Figure 1 In the activated region 112 of the positive electrode plate 11, when lithium ions pass through the solid electrolyte 12 and are precipitated on the first surface of the negative electrode current collector 131, the lithium precipitation layer 135 is not formed in the discharge state, but the lithium precipitation layer 135 may be formed in the charge state. When discharging, the lithium ions of the lithium precipitation layer 135 dissociate, pass through the solid electrolyte layer 12, and move to the activated region 112 of the positive electrode plate 11, so that the lithium precipitation layer 135 disappears.
[0070] Even when charging, in the deactivated region 114, lithium ions do not move to the negative electrode plate 13, and lithium ions dissociated from the lithium precipitation layer 135 during discharge do not move to the deactivated region 114 of the positive electrode plate 11. That is, the deactivated region 114 does not affect charging and discharging. Accordingly, the deactivated region 114 does not participate in the internal short circuit of the all-solid-state battery.
[0071] Fig.16 FIG. 2 is a cross-sectional view showing another embodiment of a positive electrode plate applied to an all-solid-state battery according to an embodiment of the present invention. Fig.16 , the positive electrode plate 21 may be formed by patterning the positive electrode current collector 211 coated with the positive active material by laser cutting.
[0072] In this case, the positive electrode active material layer may have an activation region 212 formed in a pattern and its periphery, that is, a convex portion on the pattern edge. At this time, the deactivation region 214 may be formed by irradiating a laser on the convex portion on the peripheral edge, and the deactivation region 214 may block the movement of lithium ions during charge and discharge.
[0073] Return to reference Figure 1 , the negative electrode plate 13 may include a negative active material layer 132 formed by applying a negative active material on a cross section of a negative electrode collector 131 made of stainless steel (SUS) or nickel-plated copper (Ni-coated Cu).
[0074] For convenience, the negative electrode active material layer 132 is illustrated here, but the negative electrode active material layer 132 may not exist. In this case, the precipitated lithium precipitation layer 135 may serve as the negative electrode active material layer. In addition, only a polymer layer (such as a polyvinylidene fluoride layer) may be formed on the cross section of the negative electrode current collector 131.
[0075] The solid electrolyte (SE) layer 12 is laminated on the negative electrode active material layer 132. The lamination method may be achieved by direct coating of a solid electrolyte slurry, transfer of a solid electrolyte layer, or lamination bonding between a free-standing solid electrolyte layer and a negative electrode active material layer.
[0076] The buffer film 20 is disposed on the rear surface of the negative electrode collector 131 of the negative electrode plate 13 in the unit cell and may be configured to provide an elastic force corresponding to the lithium precipitation layer 135 according to the precipitation and dissociation of lithium on the negative active material layer 132 and the negative electrode collector 131 during charge and discharge.
[0077] In addition, the positive electrode plate 11 has an uncoated area 113 protruding outward on a first side, and has an uncoated area 133 protruding outward on a second side. When the unit cells are stacked to form a module of an all-solid-state battery, the uncoated areas 113 of the positive electrode plates 11 can be stacked on each other to be electrically connected to each other, and the uncoated areas 113 of the negative electrode plates 13 can be stacked on each other to be electrically connected to each other.
[0078] While the disclosure has been described in connection with what are presently considered to be practical example embodiments, it is to be understood that the disclosure is not limited to the disclosed embodiments, but on the contrary, the disclosure is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims.
[0079] -Description of Reference Numerals-
[0080] 11, 21: Positive electrode plate 12: Solid electrolyte layer
[0081] 13: Negative electrode plate 20: Buffer film
[0082] 111, 211: Positive electrode current collector
[0083] 112, 212: Activation area
[0084] 114, 214: deactivation area
[0085] 131: Negative electrode current collector
[0086] 132: Negative electrode active material layer
[0087] 135: Lithium precipitation layer
Claims
1. An all-solid-state battery, include: a positive electrode plate having an active material on a positive electrode current collector; a solid electrolyte layer disposed on one side of the positive electrode plate; as well as A negative electrode plate disposed on one side of the solid electrolyte layer, The positive electrode plate comprises an activated region of the active substance; and A laser treated deactivated region is located on the peripheral edge of the activated region. 2 . The all-solid-state battery according to claim 1 , wherein the positive electrode plate is formed by laser cutting the positive electrode current collector on which the active material is continuously coated together with the active material layer.
3. The all-solid-state battery of claim 1, wherein the deactivation region is configured to block entry and exit of lithium ions. 4 . The all-solid-state battery of claim 1 , wherein the deactivation region is configured to block entry and exit of lithium ions by deformation of a crystal structure of the active material on the positive electrode plate. 5 . The all-solid-state battery according to claim 1 , wherein the deactivation region is configured to block entry and exit of lithium ions by denaturation of a solid electrolyte in the solid electrolyte layer.
6. The all-solid-state battery according to claim 1, in, In the deactivation region, the positive electrode current collector is melted and modified to be contained in the active material. 7 . The all-solid-state battery of claim 1 , wherein the positive electrode plate is formed by laser cutting the positive electrode current collector on which the active material is pattern-coated.
8. The all-solid-state battery of claim 7, wherein the deactivation region is formed in a raised portion of a peripheral edge. 9 . The all-solid-state battery according to claim 1 , wherein the deactivated region is formed to have a width of 0.1 to 1 mm.