Preparation method and application of in-situ growth FeCoNi catalyst
By growing FeCoNi catalyst in situ on nickel foam, the problem of low degradation efficiency caused by persulfate catalyst agglomeration is solved, efficient degradation of microplastics and good catalyst stability are achieved, and it is suitable for water treatment in complex environments.
Patent Information
- Application Number
- CN202411382811.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, persulfate catalysts are prone to agglomeration in solution, hindering their contact with contaminants and persulfate, and reducing the degradation reaction rate of microplastics.
In situ grown FeCoNi catalyst is used to form a polymetal oxide structure on the foam nickel. As a solid catalyst, the persulfate is activated through a non-radical mechanism to ensure the good dispersion of the catalyst and efficient degradation of microplastics.
It realizes efficient degradation of microplastics, has a wide pH adaptation range, and maintains high degradation efficiency in complex environments. The catalyst remains high stability after multiple cycles, and is suitable for microplastic treatment in actual water environments.
Smart Images

Figure CN119034745A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmental technology, and in particular to a preparation method of an in-situ grown FeCoNi catalyst and application thereof. Background Art
[0002] Microplastics (MPs) refer to solid plastic fragments with a size of less than 5 mm. They are considered to be an emerging environmental pollutant with complex physical and chemical properties that change their mobility, bioavailability, toxicity to organisms, and interactions with surrounding pollutants. The natural decomposition of MPs in the environment may take decades and release a lot of harmful organic matter. Moreover, from a more positive perspective, plastics have potential utilization value. Not only can they be used as resources when they enter the cycle, but some of the products of their cracking can also be used as energy. For example, the degradation of MPs can produce hydrogen and methane, etc. Therefore, whether for the significance of MPs removal or utilization value, research on their degradation needs to increase investment.
[0003] The advanced oxidation process based on persulfate (PS) is recognized as an efficient wastewater treatment method because of its strong oxidation ability and wide pH adaptability range. In fact, PS cannot react directly with most pollutants or cannot quickly degrade pollutants in water due to the slow reaction rate, and often requires external energy to activate it. Transition metal ion activation of PS has the advantages of high activation efficiency and simple operation. However, nano-sized and micron-sized powdered catalysts are easy to agglomerate in the solution, which will hinder the contact between PS, pollutants and catalysts and thus reduce the reaction rate. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing an in-situ grown FeCoNi catalyst and its application. The present invention proposes the concept of growing the catalyst in situ on a three-dimensional substrate, thereby enhancing the application of multiphase catalysts in actual wastewater treatment by improving the low-cost recovery rate of the catalyst; at the same time, the catalyst of the present invention also provides additional advantages, such as good dispersibility and high catalytic performance of metal catalytic sites, ensuring good mechanical stability and conductivity of the catalyst, so as to solve the problems in the prior art that microplastics are difficult to degrade, the catalyst for activating persulfate is easy to agglomerate in the solution, and the contact between persulfate, pollutants and catalyst is hindered, thereby reducing the reaction rate.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A method for preparing an in-situ grown FeCoNi catalyst specifically comprises the following steps:
[0007] Step 1: Clean the surface of nickel foam;
[0008] Step 2: Dissolve Co(NO3)2·6H2O and Fe(NO3)3·9H2O in 35 mL of ultrapure water and stir to form a uniform solution; wherein the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O is 0.5 to 2.2, and the total amount of metal ions is 2 to 4 mmol;
[0009] Step 3: Add CO(NH2)2 and NH4F to the solution obtained in step 2, stir evenly, immerse the nickel foam treated in step 1, and keep it at 90-140°C for 8-17h; wherein the molar ratio of CO(NH2)2 to NH4F is 1-1.5;
[0010] Step 4: washing the nickel foam after the reaction in step 3 with water, and drying at 50-70° C. for 10-14 hours to obtain a nickel foam precursor;
[0011] Step 5: calcining the nickel foam precursor at 300-400° C. for 2-4 hours to obtain a FeCoNi catalyst.
[0012] Preferably, in step 1, the surface of the nickel foam is ultrasonically cleaned with HCl, acetone, ethanol and ultrapure water in sequence.
[0013] Preferably, in step 3, the reaction temperature is 120° C. and the reaction time is 12 h.
[0014] Preferably, in step 4, drying is performed at 60° C. for 12 h.
[0015] Preferably, in step 5, calcination is performed at 350° C. for 3 h.
[0016] Preferably, in step 5, the heating rate is 5°C / min, and the calcination is performed under an air atmosphere.
[0017] The invention provides an application of an in-situ grown FeCoNi catalyst. The FeCoNi catalyst prepared by the preparation method can be used to activate persulfate to degrade plastics.
[0018] Preferably, the persulfate is peroxymonosulfate.
[0019] Preferably, the size of the plastic is less than or equal to 5 mm.
[0020] Preferably, the pH value during the degradation process is 3 to 7.6.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention synthesizes a multi-metal FeCoNi oxide structure (FeCoNi-NF) in situ on nickel foam (NF), and uses it as a solid catalyst in the degradation process to activate peroxymonosulfate (PMS) for degrading polylactic acid (PLA), wherein NF not only plays an important role as a substrate support, but also serves as an internal Ni source for material manufacturing.
[0023] 2. The catalyst of the present invention activates persulfate (PMS) through a non-radical mechanism of mediated electron transfer, thereby being able to efficiently degrade microplastics. Due to this mechanism, the catalyst exhibits a wide pH adaptability range in the degradation of microplastics and is effective in the presence of high ions (such as SO4 2- 、NO3 - ) and humic acid in the complex environment, the degradation efficiency of microplastics will not be inhibited. Compared with the traditional powder catalyst, the catalyst prepared by the present invention has obvious advantages in separation and recycling after use, and can still maintain its high stability after five consecutive cycles. In addition, the catalyst also shows excellent performance when applied to the degradation of microplastics in actual water environments, and has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Diagram of the mechanism and experimental setup for FeCoNi-NF catalyst to activate PMS and degrade PLA.
[0025] Figure 2 middle, Figure 2 A is a physical photo of NF and a physical photo of FeCoNi-NF (Example 3); Figure 2 B is the SEM image of FeCoNi-NF (Example 3); Figure 2 C is the mapping diagram of each element on FeCoNi-NF (Example 3); Figure 2 D is an O element; Figure 2 E is Fe element; Figure 2 F is Co element; Figure 2 H is the EDS spectrum.
[0026] Figure 3 middle, Figure 3 A is the XRD pattern of NF; Figure 3 B is the XRD pattern of FeCoNi-NF; Figure 3 C is the powder XRD pattern of FeCoNi obtained after ultrasonic treatment of FeCoNi-NF.
[0027] Figure 4 is the XPS spectrum; Figure 4 A is C1s, which comes from the conductive glue used in testing XPS; Figure 4B is O1s; Figure 4 C is Fe 2p; Figure 4 D is Co 2p; Figure 4 E is Ni 2p; Figure 4 F is FeCoNi-NF.
[0028] Figure 5 middle, Figure 5 A is the EIS spectra of the Ni-NF catalyst, CoNi-NF catalyst, FeNi-NF catalyst and the FeCoNi-NF catalyst of the present invention prepared by the prior art; Figure 5 B is the degradation process of PLA degradation by Ni-NF catalyst, CoNi-NF catalyst, FeNi-NF catalyst and the FeCoNi-NF catalyst of the present invention.
[0029] Figure 6 middle, Figure 6 A is the degradation process of PLA under different system conditions; Figure 6 B is the degradation effect of the catalyst FeCoNi-NF being used repeatedly for 5 times to activate PMS and degrade PLA.
[0030] Figure 7 middle, Figure 7 A is the effect of free radical quencher on the degradation of PLA in FeCoNi-NF / PMS system; Figure 7 B is the EPR spectrum of 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) in different reaction systems.
[0031] Figure 8 SO4 is commonly found in actual industrial wastewater 2- 、HCO3 - 、NO3 - and Cl - Effect of anions on the activation of PMS by FeCoNi-NF for PLA degradation.
[0032] Fig. 9 This is the effect of humic acid (HA) on the degradation of PLA by FeCoNi-NF activated PMS in actual environment.
[0033] Fig.10 This is the degradation process of PLA in actual water environment (tap water and river water). DETAILED DESCRIPTION
[0034] The present invention will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.
[0035] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values listed when defining the range.
[0036] 1. A method for preparing a FeCoNi catalyst, comprising the following steps:
[0037] Step 1: Clean the surface of nickel foam;
[0038] Step 2: Dissolve Co(NO3)2·6H2O and Fe(NO3)3·9H2O in 35 mL of ultrapure water and stir to form a uniform solution; wherein the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O is 0.5 to 2.2, and the total molar concentration of metal ions is 2 to 4 mmol;
[0039] Step 3: Add CO(NH2)2 and NH4F to the solution obtained in step 2, stir evenly, immerse the nickel foam treated in step 1, and keep it at 90-140°C for 8-17h; wherein the molar ratio of CO(NH2)2 to NH4F is 1-1.5;
[0040] Step 4: washing the nickel foam after the reaction in step 3 with water, and drying at 50-70° C. for 10-14 hours to obtain a nickel foam precursor;
[0041] Step 5: calcining the nickel foam precursor at 300-400° C. for 2-4 hours to obtain a FeCoNi catalyst.
[0042] After studying the catalysts in the prior art, the present invention found that persulfate (PS), as a strong oxidant, has attracted widespread attention in advanced oxidation processes (AOPs) because of its high oxidizing ability and the ability to maintain activity over a wide pH range. This process is considered to be an effective means of wastewater treatment because it can effectively decompose organic pollutants, especially those that are difficult to biodegrade. However, although persulfate itself has a strong oxidizing ability, it cannot directly react effectively with most organic pollutants, or even if it can react, its rate may be very slow and insufficient to achieve effective degradation of pollutants. In order to solve this problem, the prior art usually needs to activate persulfate by external means to increase its reaction rate with pollutants. One common activation method is to use transition metal ions to promote the decomposition of persulfate to produce stronger oxidants, such as hydroxyl radicals (·OH) and sulfate radicals (SO4 -·). The advantage of this method is that the activation efficiency is high and the operation is relatively simple. However, in order to improve the activation effect of such catalysts on persulfate, the prior art often makes the catalyst into nano or micron-sized powders. These particles may agglomerate in aqueous solution, resulting in a reduction in the effective surface area of the catalyst, thereby affecting its contact with persulfate and pollutants, and ultimately resulting in a decrease in the efficiency of the entire activation process. In order to solve this technical problem, the present invention conceives and designs a new catalyst form, using a porous material to carry the catalyst to prevent the agglomeration of the catalyst particles, while increasing the contact area between the catalyst and the pollutant, thereby ensuring the activation effect of the catalyst on persulfate, especially the degradation effect on microplastics. At the same time, the present invention also notes that due to the broad-spectrum oxidizing property of free radicals, they will react with other substances other than the target pollutants, thereby reducing their degradation effect on the target pollutants. Based on this, the present invention conceives to use non-free radicals for degradation, which can avoid reacting with other substances other than the target pollutants. Therefore, based on this inventive concept, the present invention adjusts the design of the catalyst to prepare a FeCoNi catalyst grown in situ on nickel foam. The FeCoNi grown in situ on nickel foam is in the shape of nano needles and can be evenly distributed on the surface of nickel foam. At the same time, after further analysis of the FeCoNi catalyst grown in situ on nickel foam, it is found that the in situ grown FeCoNi-NF may have Fe 0.5 Ni 0.5 Co2O4 and NiCo2O4 are two spinel structures. The metal elements in these structures have multiple valence states and can be quickly converted between different titanium oxides, promoting electron transfer in redox reactions. Figure 1 As shown in FIG. 1 , the degradation mechanism of the catalyst of the present invention is as follows: First, PMS undergoes a redox reaction with the FeCoNi-NF catalyst. PMS accepts electrons from the FeCoNi-NF catalyst and decomposes into SO4 2- , so that FeCoNi-NF reaches an electron-deficient oxidation state with strong electron absorption capacity. Then, PLA is rapidly oxidized by providing electrons to the oxidized FeCoNi-NF, and the FeCoNi-NF catalyst returns to its initial state. As a result, FeCoNi-NF acts as an electron mediator to transfer electrons from PLA to PMS. This is a catalyst-mediated electron transfer process and belongs to the non-radical oxidation mechanism in PMS activation, which can avoid the catalyst from reacting with substances other than the target pollutant, thereby reducing the degradation effect.
[0043] In some embodiments of the present invention, the molar ratio of Co(NO3)2·6H2O and Fe(NO3)3·9H2O is 0.5 to 2.2. Controlling the molar ratio of Co(NO3)2·6H2O and Fe(NO3)3·9H2O within this range can ensure that the catalyst has a high degradation efficiency for microplastics after persulfate activation, while a molar ratio that is too low or too high outside this range will lead to a decrease in degradation efficiency. Therefore, the molar ratio of Co(NO3)2·6H2O and Fe(NO3)3·9H2O can be 0.5, 1.0, 1.8, 1.9, 2.0, 2.1, 2.2, etc., as well as all ranges and sub-ranges between the above values. At the same time, the metal ions described in the present invention mainly include Co 2+ and Fe 3+ These two metal ions, in the whole reaction system, the total amount of these two metal ions is 2 to 4 mmol. It can be considered here that in every 35 mL of liquid reaction system, the total amount of the two metal ions is controlled at 2 to 4 mol. Controlling the amount of the total amount of metal ions within this range can ensure that the appropriate amount of precursor material is loaded on the nickel foam. If the amount of the total amount of metal ions is lower than this range, the precursor material loading amount will be insufficient, resulting in reduced catalyst performance; but the amount of the total amount of metal ions is higher than this range, which will cause too much loading, and metal ion leaching may be increased during the reaction. Therefore, the amount of the total amount of metal ions can be 2mmol, 2.8mmol, 2.9mmol, 3.0mmol, 3.1mmol, 3.2mmol, 4mmol, etc., and all ranges and sub-ranges between the above values. It should be understood that in an embodiment, any of the above ranges can be combined with any other range.
[0044] In some embodiments of the present invention, the molar ratio of CO(NH2)2 and NH4F is 1 to 1.5. The molar ratio of CO(NH2)2 and NH4F is controlled within the range to ensure that the metal ions can be completely precipitated to form a precursor, thereby further ensuring that there are no defects in the crystal structure of the generated material, and ultimately ensuring the activation effect of the catalyst on the persulfate. When the molar ratio is lower than this range, it means that the amount of CO(NH2)2 in the raw material system is too small, which will cause the metal ions to not be completely precipitated to form a precursor; but when the molar ratio is higher than this range, it means that the amount of NH4F in the raw material system is too small, which will cause structural defects in the crystals of the final generated catalyst material, resulting in a decrease in material performance. Therefore, the molar ratio of CO(NH2)2 and NH4F can be 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0045] In some embodiments of the present invention, in step 1, the surface of the nickel foam is ultrasonically cleaned with HCl, acetone, ethanol and ultrapure water in sequence to thoroughly clean the surface of the nickel foam, especially the surface where the catalyst grows. The concentration of HCl used for washing is 3M, the acetone is analytically pure, and the ethanol is analytically pure.
[0046] In some embodiments of the present invention, in step 3, the reaction temperature is controlled between 90 and 140°C. If the reaction temperature is too low, the hydrolysis of CO(NH2)2 will be slow, and the solution after hydrothermal treatment will be yellow, which indicates that there are still a large number of unreacted metal ions. Incomplete reaction will cause less precursor substances to be deposited on the surface of nickel foam; but if the reaction temperature is too high, urea will be condensed to generate ammonia, which will weaken the binding force between the precursor substance and the nickel foam, making it difficult to deposit on its surface and unevenly distributed. Therefore, the reaction temperature can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C. etc., and all ranges and sub-ranges between the above values; the reaction time is controlled at 8 to 17 hours. If the reaction time is too short, too little catalyst will be formed on the surface of the nickel foam, thereby affecting the activation effect of persulfate and the degradation effect of microplastics; if the reaction time is too long, the catalyst on the surface of the nickel foam will be stacked, which will adversely affect the activation effect of persulfate and the degradation effect of microplastics. Therefore, the reaction time can be 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0047] In some embodiments of the present invention, in step 4, drying is performed at 50 to 70°C for 10 to 14 hours. The drying temperature may be 50°C, 60°C, 70°C, etc., and all ranges and sub-ranges between the above values; the drying time may be 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0048] In some embodiments of the present invention, in step 5, the calcination temperature is controlled between 300 and 400°C. If the calcination temperature is too low, the reaction will be incomplete and amorphous materials will be generated, thereby affecting the crystallization and electrochemical properties of the catalyst material; if the calcination temperature is too high, the pore structure on the surface of the catalyst material will become smaller, and the catalyst activity will be reduced, so the calcination temperature can be 300°C, 320°C, 350°C, 370°C, 400°C, etc., and all ranges and sub-ranges between the above values; the calcination time is controlled between 2 and 4 hours. If the calcination time is too short, the reaction will be incomplete, and if the calcination time is too long, the material may be over-sintered and the structure may be damaged, so the calcination time can be 2 hours, 3 hours, 4 hours, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0049] In some embodiments of the present invention, in step 5, the heating rate is 5°C / min, and the calcination is performed in an air atmosphere. If the heating rate is too fast, the catalyst body on the surface of the nickel foam may crystallize prematurely, resulting in coarse catalyst particles. After high-temperature reduction, the surface is not only rougher, but also prone to precipitation, which will reduce the catalytic performance of the catalyst; while if the heating rate is too slow, the preparation efficiency of the catalyst is affected, and the material calcination time may be too long, which will eventually lead to excessive sintering and structural damage of the material.
[0050] 2. Application of a FeCoNi catalyst
[0051] The FeCoNi catalyst prepared by the preparation method of the present invention can be used to activate persulfate to degrade plastics, wherein the persulfate is peroxymonosulfate.
[0052] In some embodiments of the present invention, the size of the plastic is less than or equal to 5 mm. Such plastics can be considered as microplastics, and the specific shape of the plastic is not limited here, and the average particle size is less than or equal to 5 mm.
[0053] In some embodiments of the present invention, the pH value of the degradation environment has a significant effect on the degradation effect. The catalyst can activate persulfate to degrade plastic in an environment with a pH value of 3 to 11, but the degradation effect will be different in different pH ranges; therefore, the pH value during the degradation process can be 3, 4, 5, 6, 7, 8, 9, 10, 11, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0054] 3. Examples and Comparative Examples
[0055] 1. Effect of catalyst preparation method on catalytic effect
[0056] Example 1
[0057] Step 1: NFs were cut into 2 cm × 3 cm pieces and then sonicated with HCl, acetone, ethanol, and ultrapure (UP) water;
[0058] Step 2: Dissolve Co(NO3)2·6H2O and Fe(NO3)3·9H2O in 35 mL of ultrapure water and stir to form a uniform solution; wherein the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O is 0.5, and the total amount of metal ions is 3 mmol;
[0059] Step 3: Add CO(NH2)2 and NH4F to the solution obtained in step 2, stir evenly, immerse the nickel foam treated in step 1, and keep it at 120°C for 12 hours; wherein the molar ratio of CO(NH2)2 to NH4F is 1.0;
[0060] Step 4: washing the nickel foam after the reaction in step 3 with water, and drying at 60° C. for 12 hours to obtain a nickel foam precursor;
[0061] Step 5: calcine the nickel foam precursor at 350° C. for 3 h to obtain a FeCoNi catalyst.
[0062] The above catalyst was subjected to degradation experiment under the conditions of pH=7.6, [PMS]=0.5mmol / L, [methylene blue (MB)]=10mg / L, T=25°C (0.2mol / L borate buffer, 100ml), and a FeCoNi-NF catalyst with a length×width×height of 2cm×3cm×1mm was added to detect the degradation rate of MB by the catalyst within 20 minutes. Example 1 The MB degradation efficiency within 20 minutes was 97.3%.
[0063] Example 2
[0064] The method was adjusted based on Example 1, except that the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O was 1.0. The other steps were exactly the same as those in Example 1. The MB degradation efficiency of Example 2 was 86.7% within 20 minutes.
[0065] Example 3
[0066] The method was adjusted based on Example 1, except that the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O was 2.0. The other steps were exactly the same as those in Example 1. In Example 3, the MB degradation rate was 100.0% within 20 minutes.
[0067] Example 4
[0068] The method was adjusted based on Example 1, except that the total molar concentration of metal ions was 2 mmol. The other steps were exactly the same as those in Example 1. In Example 4, the MB degradation efficiency was 95.0% within 20 minutes.
[0069] Example 5
[0070] The method was adjusted based on Example 1, except that the total molar concentration of metal ions was 4 mmol. The other steps were exactly the same as those in Example 1. In Example 5, the MB degradation efficiency was 91.8% within 20 minutes.
[0071] Example 6
[0072] The method was adjusted based on Example 1, except that the molar ratio of CO(NH2)2 to NH4F was 1.2. The other steps were exactly the same as those in Example 1. In Example 6, the MB degradation rate was 100.0% within 20 minutes.
[0073] Example 7
[0074] The method was adjusted based on Example 1, except that the molar ratio of CO(NH2)2 to NH4F was 1.5. The other steps were exactly the same as those in Example 1. In Example 7, the MB degradation rate was 100.0% within 20 minutes.
[0075] Example 8
[0076] The adjustment was made on the basis of Example 1, except that in step 3, the reaction temperature was 90° C. The other steps were exactly the same as those in Example 1. In Example 8, the MB degradation efficiency was 95.4% within 20 minutes.
[0077] Example 9
[0078] The adjustment was made on the basis of Example 1, except that in step 3, the reaction temperature was 140° C. The other steps were exactly the same as those in Example 1. In Example 9, the MB degradation rate was 100.0% within 20 minutes.
[0079] Example 10
[0080] The method is adjusted based on Example 1, except that in step 3, the reaction time is 8 hours. The other steps are exactly the same as those in Example 1. In Example 10, the MB degradation efficiency is 96.2% within 20 minutes.
[0081] Embodiment 11
[0082] The method was adjusted based on Example 1, except that in step 3, the reaction time was 17 hours. The other steps were exactly the same as those in Example 1. In Example 11, the MB degradation efficiency was 94.1% within 20 minutes.
[0083] Comparative Example 1
[0084] An improvement was made on the basis of Example 1, except that the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O was 3:0. The other steps were exactly the same as those of Example 1. The MB degradation efficiency of Comparative Example 1 was 45.7% within 20 minutes.
[0085] Comparative Example 2
[0086] An improvement was made on the basis of Example 1, except that the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O was 0:3. The other steps were exactly the same as those of Example 1. The MB degradation efficiency of Comparative Example 2 was 72.7% within 20 minutes.
[0087] Comparative Example 3
[0088] An improvement was made on the basis of Example 1, except that in step 3, the reaction temperature was 50° C. The other steps were exactly the same as those of Example 1. In Comparative Example 3, the MB degradation efficiency within 20 minutes was less than 70%.
[0089] Comparative Example 4
[0090] An improvement was made on the basis of Example 1, except that in step 3, the reaction temperature was 150° C. The other steps were exactly the same as those of Example 1. In Comparative Example 4, the MB degradation efficiency was 61.1% within 20 minutes.
[0091] Comparative Example 5
[0092] An improvement was made on the basis of Example 1, except that: in step 3, the reaction time was 4 hours. The other steps were exactly the same as those in Example 1. In Comparative Example 5, the MB degradation efficiency was less than 70% within 20 minutes.
[0093] Comparative Example 6
[0094] An improvement was made on the basis of Example 1, except that: in step 3, the reaction time was 20 hours. The other steps were exactly the same as those in Example 1. In Comparative Example 6, the MB degradation efficiency within 20 minutes was less than 70%.
[0095] Comparative Example 7
[0096] An improvement was made on the basis of Example 1, except that in step 2, the total amount of metal substances was 1 mmol. The other steps were exactly the same as those of Example 1. The MB degradation efficiency of Comparative Example 7 was 75.6% within 20 minutes.
[0097] Comparative Example 8
[0098] An improvement was made on the basis of Example 1, except that in step 2, the total amount of metal substances was 6 mmol. The other steps were exactly the same as those of Example 1. In Comparative Example 8, the MB degradation efficiency was less than 70% within 20 minutes.
[0099] By comparing the examples and the comparative examples, it is found that the catalysts prepared in the examples can achieve a degradation rate of MB of more than 85% within 20 minutes, while the maximum degradation rate that the catalysts prepared in the comparative examples can achieve is only 75%.
[0100] Taking the catalyst prepared in Example 3 as an example, this example is characterized. Figure 2 It can be seen that the FeCoNi in situ grown on NF is in the shape of nano needles. At the same time, EDS element mapping and EDS spectrum can prove that Fe, Co, Ni, and O elements exist on NF and are evenly distributed, indicating that FeCoNi oxide has been successfully grown on NF. Figure 3 It can be seen that by comparing with the standard card, it is found that the in-situ grown FeCoNi-NF may have Fe 0.5 Ni 0.5 Two spinel structures: Co2O4 and NiCo2O4. Figure 4 It shows that the metal elements in FeCoNi-NF have multiple valence states (divalent and trivalent), and these metal ions can quickly transform between different oxidation states, promoting electron transfer in redox reactions. The catalysts prepared in other examples also showed the same structure as Example 3 after the above test.
[0101] The performance of the embodiments of the present invention is compared with other catalysts in the prior art. Ni-NF catalyst, CoNi-NF catalyst, FeNi-NF catalyst and FeCoNi-NF catalyst of the present invention are prepared by the prior art. The degradation effect of each catalyst on PLA is compared under the conditions of [PLA] = 1 g / L, [PMS] = 5 mM, pH = 7.6, T = 25 ° C. Figure 5 As shown in A, among the catalysts, the FeCoNi-NF catalyst of the present invention has the best conductivity, which is due to the presence of multivalent metal ions inside the FeCoNi-NF. The migration of these multivalent metal ions promotes its conductivity and electron transfer rate; Figure 5As shown in B, under the same conditions, the FeCoNi-NF catalyst of the present invention has the best degradation efficiency for PLA.
[0102] 2. Effect of degradation conditions on catalyst degradation effect
[0103] Example 12
[0104] Taking the catalyst prepared in Example 3 as an example, the degradation conditions were further studied. The catalyst prepared in Example 3 was subjected to a degradation experiment under the conditions of pH=7.6, [PMS]=5mmol / L, [PLA]=1g / L, T=25°C (0.2mol / L borate buffer, 100ml), and a FeCoNi-NF catalyst with a length×width×height of 2cm×3cm×1mm was added. The PLA degradation rate was 79.1% within two hours.
[0105] Embodiment 13
[0106] An improvement was made on the basis of Example 12, except that the pH value was 3. Other conditions were exactly the same as those of Example 12. The degradation rate of PLA within 2 hours was 99.2%.
[0107] Embodiment 14
[0108] An improvement was made on the basis of Example 12, except that the pH value was 5. Other conditions were exactly the same as those of Example 12. The degradation rate of PLA within 2 hours was 88.4%.
[0109] Embodiment 15
[0110] An improvement was made on the basis of Example 12, except that the concentration of PMS was 10 mM, and the other steps were exactly the same as those of Example 2. The degradation rate of PLA within 2 h was 90.4%.
[0111] Example 16
[0112] Improvements were made on the basis of Example 12, except that the pH value was 11. The other conditions were exactly the same as those of Example 12. The degradation rate of PLA within 2 hours was 23.5%. At the same time, further research revealed that under the condition of only changing the pH value, when the pH value was in the range of 8 to 10, the degradation rate of PLA within 2 hours was able to stabilize at more than 70%; and when the pH value reached or exceeded 11, the degradation rate began to decrease, but under this condition, the catalyst still had the effect of activating persulfate to degrade PLA.
[0113] Comparative Example 9
[0114] An improvement was made on the basis of Example 12, except that in step 6, the PMS concentration was 0 mM, and the other steps were exactly the same as those of Example 2. The PLA degradation rate within 2 h was 7.6%.
[0115] Comparative Example 10
[0116] An improvement was made on the basis of Example 12, except that in step 6, the PMS concentration was 2 mM, and the other steps were exactly the same as those of Example 2. The PLA degradation rate within 2 h was 55.6%.
[0117] Comparative Example 11
[0118] An improvement was made on the basis of Example 12, except that the concentration of PLA was 2 g / L, and the other steps were exactly the same as those of Example 2. The degradation rate of PLA within 2 h was 50.1%.
[0119] Comparative Example 12
[0120] An improvement was made on the basis of Example 12, except that the concentration of PLA was 5 g / L, and the other steps were exactly the same as those of Example 2. The degradation rate of PLA within 2 h was 34.5%.
[0121] The present invention further studies the degradation system. Based on the degradation system of Example 12, the FeCoNi-NF catalyst is added to different degradation systems to observe the degradation effect on PLA. Figure 6 In A, PLA means that the buffer contains only PLA (concentration is 1g / L); PMS / PLA means that the buffer contains PMS (concentration is 5mmol / L) and PLA (concentration is 1g / L); FeCoNi-NF / PLA means that the buffer contains FeCoNi-NF and PLA (concentration is 1g / L); PMS / FeCoNi-NF / PLA means that the buffer contains PMS (concentration is 5mmol / L), FeCoNi-NF and PLA (concentration is 1g / L). Figure 6 A It can be seen that when only PLA exists in the buffer, the degradation process does not occur and the concentration of PLA remains unchanged; after PMS and FeCoNi-NF are added separately, the degradation efficiency of PLA is improved, which shows that the use of PMS and FeCoNi-NF alone has a certain degradation effect on PLA, and the degradation effect of PMS on PLA is better than that of FeCoNi-NF; when PMS and FeCoNi-NF exist in the system at the same time, the degradation effect of PLA is greatly improved, which shows that under the same conditions, the FeCoNi-NF / PMS system has the best effect of degrading PLA. Figure 6B is the effect of repeatedly using FeCoNi-NF to activate PMS to degrade PLA. Figure 6 B shows that after the FeCoNi-NF catalyst of the present invention was reused for 5 times to activate PMS to degrade PLA, its degradation rate was only reduced by 8%, indicating that the catalyst of the present invention has good reusability.
[0122] 3. Verification of the catalyst degradation mechanism of the present invention
[0123] Under the reaction conditions of [PLA] = 1 g / L, [MeOH] = 0.5 M, [TBA] = 0.5 M, [PMS] = 5 mM, pH = 7.6, and T = 25 °C, the degradation mechanism of PLA by FeCoNi-NF / PMS system was investigated.
[0124] Figure 7 A is the effect of free radical quencher on the degradation of PLA in FeCoNi-NF / PMS system. It can be seen that the free radical quencher has no effect on the degradation of PLA in FeCoNi-NF / PMS system, indicating that its degradation process is a non-free radical process.
[0125] Figure 7 B is the EPR spectrum of DMPO in different reaction systems. As shown in the figure, since 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) loses electrons to the oxidant in the PMS activation system to produce 5,5-dimethyl-2-pyrrolidone-n-oxyl (DMPOX), the peak intensity of DMPOX in the FeCoNi-NF / PMS / PLA system is weakened compared with the peak intensity in the FeCoNi-NF / PMS system. This indicates that DMPO and PLA have a competitive electron donation process, which weakens the peak intensity of DMPOX. This can further prove that the degradation process of PLA in the FeCoNi-NF / PMS system is a process dominated by a non-free radical mechanism.
[0126] IV. Practical Application
[0127] 1. SO4 in industrial wastewater 2- 、HCO3 - 、NO3 - and Cl - Effects on activated PMS and PLA degradation
[0128] The present invention studies the common SO4 2- 、HCO3 - 、NO3 - and Cl -Effects on the degradation of activated PMS and PLA (wherein the concentration of each anion is 200 mM). Taking the catalyst prepared in Example 3 as an example, the degradation conditions of Example 12 were used for degradation treatment. SO4 was added separately to the degradation system of Example 12. 2- 、HCO3 - 、NO3 - and Cl - , where the mass ratio of each anion to PLA: SO4 2- / PLA=28.4、HCO3 - / PLA=16.8、NO3 - / PLA=17.0 and Cl - / PLA=11.7, the result is as follows Figure 8 As shown, the degradation effects were then compared and found to be:
[0129] (1)Cl - The presence of has a significant inhibitory effect on the degradation of PLA, and the degradation efficiency has dropped significantly, down to 50.7%;
[0130] (2)HCO3 - It also has the same - Similar inhibitory effect, but HCO3 - The inhibitory effect is more obvious in HCO3 - Under the influence of background, the PLA degradation efficiency decreased to 37.8%;
[0131] (3) However, the difference is that SO4, which was originally predicted to have an inhibitory effect 2- and NO3 - The degradation effect of PLA was different in SO4 2- and NO3 - There was no significant decrease in the presence of SO4 2- and NO3 - The degradation efficiency of PLA remained unchanged after addition, indicating that SO4 2- and NO3 - There was no negative effect on the degradation process at a concentration of 200 mM.
[0132] 2. Impact of the degradation effect on target pollutants in the context of natural organic matter
[0133] The present invention further studies the effect of degradation of target pollutants in the context of natural organic matter. Humic acid (HA) is a representative NOM. Taking the catalyst prepared in Example 3 as an example, the degradation conditions of Example 12 are used for degradation treatment. Humic acid (HA) is added to the degradation system of Example 12. Fig. 9As shown in the figure, the amount of humic acid added gradually increased from 0. When the concentration of HA in the degradation system was low (less than 100 mg / L), the degradation efficiency of PLA was significantly improved. This also shows that low concentrations of HA will promote the process of FeCoNi-NF activating PMS to degrade PLA. However, with the gradual increase in HA concentration, the degradation efficiency of PLA began to fluctuate. When the concentration of HA in the degradation system was 200 mg / L, the degradation efficiency of PLA was 81.9%, which was lower than that without adding HA. Fig. 9 As shown in the figure, the degradation efficiency of PLA did not decrease significantly, and the overall fluctuation was very stable. It can be seen that high concentration of HA will not inhibit the degradation of PLA, while low concentration of HA will promote FeCoNi-NF to activate PMS to degrade PLA.
[0134] 3. Effects in actual environmental applications
[0135] In order to further evaluate the potential of the catalyst FeCoNi-NF in practical environmental applications, the present invention also conducted catalytic experiments in tap water and river water (the river water was filtered water from Fuxi River in Zigong City). The results are as follows: Fig.10 As shown. It is noteworthy that the degradation of PLA was not inhibited, and the degradation efficiency was even faster than that in the buffer solution (pH = 7.6). Similarly, PLA was degraded using the degradation system of Example 12, except that the borate buffer was replaced with tap water and river water, respectively. Within 2 hours, the PLA removal rate reached 81.0% (tap water) and 88.9% (river water).
[0136] In summary, the above three situations all indicate that the catalyst prepared by the present invention can be applied in actual environments. The catalyst can efficiently degrade pollutants in the context of high inorganic ions and high natural organic pollutants, and can also maintain high degradation performance in actual water environments.
[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing an in-situ grown FeCoNi catalyst, characterized in that: The specific steps include: Step 1: Clean the surface of nickel foam; Step 2: Dissolve Co(NO3)2·6H2O and Fe(NO3)3·9H2O in 35 mL of water and stir to form a uniform solution; wherein the molar ratio of Co(NO3)2·6H2O to Fe(NO3)3·9H2O is 0.5 to 2.2, and the total amount of metal ions is 2 to 4 mmol; Step 3: Add CO(NH2)2 and NH4F to the solution obtained in step 2, stir evenly, immerse the nickel foam treated in step 1, and keep it at 90-140°C for 8-17h; wherein the molar ratio of CO(NH2)2 to NH4F is 1-1.5; Step 4: washing the nickel foam after the reaction in step 3 with water, and drying at 50-70° C. for 10-14 hours to obtain a nickel foam precursor; Step 5: calcine the nickel foam precursor at 300-400° C. for 2-4 hours to obtain a FeCoNi catalyst.
2. The preparation method according to claim 1, characterized in that: In step 1, the surface of the nickel foam is ultrasonically cleaned with HCl, acetone, ethanol and ultrapure water in sequence.
3. The preparation method according to claim 1, characterized in that: In step 3, the reaction temperature is 120° C. and the reaction time is 12 h.
4. The preparation method according to claim 1, characterized in that: In step 4, drying was performed at 60°C for 12 h.
5. The preparation method according to claim 1, characterized in that: In step 5, calcination was carried out at 350°C for 3h.
6. The preparation method according to claim 1, characterized in that: In step 5, the heating rate was 5°C / min, and calcination was performed under an air atmosphere.
7. An application of an in-situ grown FeCoNi catalyst, characterized in that: The FeCoNi catalyst prepared by any preparation method described in claims 1 to 6 is used to activate persulfate to degrade plastics.
8. The use according to claim 7, characterized in that: The persulfate is peroxymonosulfate.
9. The use according to claim 7, characterized in that: The size of the plastic is less than or equal to 5 mm.
10. The use according to claim 7, characterized in that: The pH value during the degradation process is 3-11.
Citation Information
Cited By
Rare earth assisted Fe-MnNi supported desulfurization catalyst, preparation method and application