Preparation method of high-dispersion sulfuration type hydrogenation catalyst and catalyst
By treating the solution of molybdenum thiotrantonic acid ammonium tungstate and nickel/cobalt salts, a high sulfur content Ni(Co)Mo(W)Sx active phase is formed, which solves the high cost in the existing hydrocracking catalyst vulcanization process. and the problem of instability of active sites, achieving efficient and stable catalytic effects.
Patent Information
- Application Number
- CN202411159882.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The existing sulfurization process of hydrocracking catalysts has problems such as high cost, environmental pollution and unstable catalyst active sites, especially the acid decomposition of molybdenum thiotungstate and surfactant damage to bond during thermal catalytic decomposition. The properties of the agent lead to a decrease in catalyst strength and metal sulfide agglomeration.
By irradiating the solution of molybdenum thiotungstate/ammonium tungstate and nickel/cobalt salt, an amorphous structure is formed and some sulfur ions are stably anchored to the metal site, forming a high sulfur content Ni(Co)Mo(W )Sx active phase avoids passivation of the active site under air atmosphere, and directly obtains a metal vulcanized catalyst, simplifying the preparation process.
A vulcanization hydrogenation catalyst with high dispersion and high active sites is realized, which reduces production difficulty and cost, avoids the passivation and agglomeration of the catalyst in heat treatment, and improves the catalytic effect and stability.
Smart Images

Figure CN119034801A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of oil refining catalysts, and in particular to a preparation method and catalyst of a highly dispersed sulfided hydrogenation catalyst. Background Art
[0002] Hydrocracking of vacuum gas oil (VGO) is one of the most important processes in petroleum refining. Various valuable products such as naphtha, jet fuel and diesel can be obtained through hydrocracking. The catalyst used for hydrocracking is a bifunctional system, in which the metal component usually has the main ability to carry out hydrogenation and dehydrogenation, while the acidic component, such as zeolite, aluminosilicate or γ-Al2O3, has cracking performance. At present, most of the metal active components of industrial hydrocracking catalysts exist in the form of oxides. In actual use, the active metal oxides on the catalyst need to be converted into sulfides. Therefore, the catalyst needs to be sulfurized or pre-sulfurized before use.
[0003] Conventional catalyst sulfurization methods use "in-situ" sulfurization, which has many disadvantages in terms of cost, safety, activity, and selectivity. Therefore, the ex-situ presulfurization technology, which is simple, efficient, pollution-free, and low-cost, has become the development trend of hydrocracking preparation technology in recent years. At present, the "ex-situ" presulfurization technology is roughly divided into two technical routes: one is to complete the presulfurization of the catalyst in a special presulfurization device in the presence of hydrogen and hydrogen sulfide or an easily decomposable organic sulfurizing agent, and then passivate it with oxygen-containing gas to make a non-spontaneous presulfurized catalyst. The second is to directly impregnate thiomolybdenum / tungstate + cobalt / nickel salt, and then heat it with inert gas to prepare a sulfurized catalyst loaded with metal sulfide.
[0004] CN85107953 discloses a method for treating a hydrogenation catalyst, which mainly comprises firstly treating a hydrocracking catalyst by impregnating elemental sulfur and a plurality of organic polysulfides dissolved and diluted with petroleum solvent at 50-150°C, then treating the catalyst in a hydrogen-free atmosphere at a temperature below 275°C, sulfiding the active metal oxide, and finally activating the catalyst at a temperature above 275°C in the presence of hydrogen. US6417134 discloses an ex-situ presulfurization method for a hydroprocessing catalyst, which is characterized in that the catalyst is firstly treated by impregnating the catalyst with elemental sulfur, organic sulfide, organic polysulfide, olefin-containing oil, and olefin-containing components diluted with a solvent at a temperature of 300°C, then treating the catalyst with hydrogen at a temperature of 250-600°C, and finally passivating the catalyst with an oxygen-containing gas. The above method belongs to the first technical route of ex-situ sulfurization, which is to presulfurize the existing oxidized catalyst, which not only requires an additional set of sulfurization equipment, but also causes serious environmental pollution during the sulfurization process.
[0005] CN102836736A discloses a method for preparing a sulfidation type hydrogenation catalyst, which comprises the following steps: uniformly mixing a carrier precursor, thiomolybdate and / or thiotungstate, a nickel salt and / or a cobalt salt, adding a binder and kneading, forming, and then drying at 100-130°C and calcining at 500-600°C under the protection of an inert gas. However, it is inevitable that the acid decomposition characteristics of thiomolybdate / tungstate break the performance of the binder (molybdenum / tungstate salts are alkaline salts and react with each other in the presence of an aluminum binder); and in the subsequent thermal catalytic decomposition process, the decomposed alkaline gas generated during the decomposition process of thiomolybdate / tungstate (such as ammonium tetrathiomolybdate) and the surfactant used also break the Al bridge bond of the binder, resulting in a decrease in the catalyst strength; in addition, during the pyrolysis process, the thiometallic salt inevitably causes the metal sulfide to agglomerate with the evaporation effect, which becomes more and more obvious with the heating time, which leads to a reduction in the exposed boundary active sites.
[0006] In order to solve the above problems, a sulfided hydrogenation catalyst with a simple preparation process and highly dispersed active sites is urgently needed. Summary of the invention
[0007] The present invention provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst and a catalyst. The thiomolybdenum / tungstate ammonium salt and the nickel / cobalt salt are decomposed by light to form an amorphous structure. The photon excitation and reduction reaction enable part of the sulfur ions to be stably anchored on the metal site to form a Ni(Co)Mo(W)S with a high sulfur content at the boundary. x The active phase makes it difficult for the active sites of the catalyst to be passivated even when exposed to air atmosphere during post-treatment, which reduces the difficulty of production and ensures the catalytic effect.
[0008] The present invention provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst, comprising the following steps:
[0009] Step 1, preparing a solution A of thiomolybdate or thiotungstate, and preparing a solution B of nickel salt or cobalt salt;
[0010] Taking a hydrocracking carrier component, mixing the powder of the hydrocracking carrier component with a solvent and slurrying the mixture to obtain a slurry C;
[0011] Step 2: at room temperature, passing solution A and solution B into slurry C, and adding a sacrificial reagent to obtain a total slurry, and isolating the total slurry from air; wherein the sacrificial reagent accounts for 1%-10% of the volume of the total slurry;
[0012] Stirring the total slurry, and simultaneously performing light treatment on the total slurry, wherein the light source used in the light treatment emits light with a wavelength of λ≤620nm, and the light treatment time is 5h-20h;
[0013] Step 3: filtering, washing, and first drying the material obtained after the light treatment, and kneading it with a binder to form it; and drying and calcining it for a second time under an inert atmosphere to obtain a highly dispersed sulfurized hydrogenation catalyst.
[0014] In one embodiment, the light source used for the light treatment includes one or more of sunlight, LED, xenon lamp, mercury lamp, and X-ray lamp.
[0015] In one embodiment, the sacrificial agent includes a mixture of one or more of methanol, ethanol, triethylamine, triethanolamine, and acetonitrile.
[0016] In one embodiment, the thiomolybdate or thiotungstate is selected from ammonium salt and tetraalkylamine salt; the nickel salt or cobalt salt is selected from chloride and nitrate.
[0017] In one embodiment, 1L of solution A contains 5g-100g of Mo and / or W; 100mL of solution B contains 1g-40g of Ni and / or Co.
[0018] In one embodiment, the hydrocracking support component includes at least one or more acidic cracking components selected from molecular sieves and amorphous silica-alumina.
[0019] In one embodiment, the molecular sieve includes one or more combinations of Y molecular sieve, β molecular sieve, ZSM-5, and SAPO molecular sieve; the mass fraction of the acidic cracking component in the hydrocracking carrier component is 5-50%; and each of the acidic cracking components includes alumina with a mass fraction of 5-40%.
[0020] In one embodiment, in the step 1, the solvent includes water, and the slurry ratio of the powder of the hydrocracking carrier component and the solvent is (1 g: 5 mL) - (1 g: 10 ml).
[0021] In one embodiment, in step three,
[0022] The first drying condition is 60°C-110°C, vacuum drying for 5h-20h;
[0023] Under an inert atmosphere, the second drying condition is 80-150°C for 2h-5h, and the roasting condition is 500°C-850°C for 4-10h;
[0024] Wherein, the binder comprises peptized small-pore alumina.
[0025] The present application also provides a highly dispersed sulfurized hydrogenation catalyst having a Ni(Co)Mo(W)S x The active phase has a size less than 20 nanometers.
[0026] The beneficial effects of the present invention include at least:
[0027] The invention provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst, wherein thio molybdenum / ammonium tungstate salt and nickel / cobalt salt are dissolved in water containing a sacrificial reagent. During light irradiation, nickel / cobalt ions catalyze the decomposition of thio molybdenum / ammonium tungstate to form amorphous Mo(W)S3 and Ni(Co)-S. Meanwhile, photons excite the valence band (S) of Mo(W)S3. 2- Group) electrons transition to the conduction band (:Mo(W) 6+ group), Mo(W) is reduced to tetravalent to form amorphous Mo(W)S2 species, and holes (active S·) are formed in the valence band. After the sacrificial reagent is oxidized, part of S is converted to S2 2- The Ni(Co)Mo(W)Sx active phase is anchored on the metal site in the form of a high sulfur content boundary Ni(Co)Mo(W)Sx active phase. The high sulfur boundary sulfur formed can avoid the problem of passivation of the active site when the catalyst intermediate is exposed to the air atmosphere during the subsequent extrusion process. In addition, the carrier precursor has a strong dispersing ability and can disperse the Ni(Co)Mo(W)Sx active phase very well, so that the edge sites of the catalytically active molybdenum / tungsten sulfide formed are fully exposed, thereby improving the catalytic effect.
[0028] Secondly, during the preparation process, the catalyst of the present invention does not need to go through a metal oxidation state, and can directly obtain a metal sulfide state with catalytic activity, which is convenient for production. That is, when used, it does not need to be activated in the vessel or pre-sulfurized outside the vessel, which reduces production equipment and production time, and reduces production costs.
[0029] The present invention also provides a highly dispersed sulfurized hydrogenation catalyst, which directly obtains the sulfide of the metal without going through the oxide state of the metal. Compared with the oxide catalyst, the pre-sulfurized catalyst does not need to be sulfurized before and during use, which can save start-up time and reduce production costs. Secondly, the catalyst of the present application does not need to be sulfurized in an oxidized state, and does not need to impregnate a sulfurizing agent onto a carrier, and a sulfurized catalyst can be directly prepared. The preparation process is simple, and the current catalyst sulfurization process for fixed bed hydrogenation can be simplified. The present application uses a mild self-decomposition method, and the dispersion of the active component molybdenum sulfide / tungsten on the obtained catalyst is relatively high compared with the current technology, that is, under high-temperature sulfurization of hydrogen / hydrogen sulfide or organic sulfur, the catalyst does not need to be air passivated, there is no risk of spontaneous combustion, and the size of the active phase is less than 20 nanometers.
[0030] Abstract of the drawings
[0031] Figure 1 is a SEM image of a carrier precursor in one embodiment of the present application;
[0032] Figure 2 It is a NiMoS type catalyst intermediate in one embodiment of the present application;
[0033] Figure 3 This is an electron binding energy spectrum of the cobalt element in the catalyst intermediate obtained in one embodiment of the present application;
[0034] Figure 4 This is the electron binding energy spectrum of the molybdenum element in the catalyst intermediate obtained in one embodiment of the present application;
[0035] Figure 5 This is an electron binding energy spectrum of sulfur element in the catalyst intermediate obtained in one embodiment of the present application. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.
[0037] The embodiments of the present application provide a highly dispersed sulfurized hydrogenation catalyst and a preparation method thereof, which are described in detail below.
[0038] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order. Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.
[0039] The present application provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst.
[0040] Step 1, preparing a solution A of thiomolybdate or thiotungstate, and preparing a solution B of nickel salt or cobalt salt;
[0041] Taking a hydrocracking carrier component, mixing the powder of the hydrocracking carrier component with a solvent and slurrying the mixture to obtain a slurry C;
[0042] Step 2: at room temperature, passing solution A and solution B into slurry C, and adding a sacrificial reagent to obtain a total slurry, and isolating the total slurry from air; wherein the sacrificial reagent accounts for 1%-10% of the volume of the total slurry;
[0043] Stirring the total slurry, and simultaneously performing light treatment on the total slurry, wherein the light source used in the light treatment emits light with a wavelength of λ≤620nm, and the light treatment time is 5h-20h;
[0044] Step 3: filtering, washing, and first drying the material obtained after the light treatment, and kneading it with a binder to form it; and drying and calcining it for a second time under an inert atmosphere to obtain a highly dispersed sulfurized hydrogenation catalyst.
[0045] Wherein, the thiomolybdate or thiotungstate is selected from ammonium salt and tetraalkylamine salt; the nickel salt or cobalt salt is selected from chloride and nitrate;
[0046] Preferably, the thiomolybdate includes tetrathiomolybdenum, hexadecyltrimethylammonium tetrathiomolybdate, ammonium polythiomolybdate ([NH4]2Mo3S 13 ) or more; the thiotungstate comprises ammonium tetrathiotungstate.
[0047] The sacrificial agent includes a mixture of one or more of methanol, ethanol, triethylamine, triethanolamine, and acetonitrile.
[0048] The light source used for the light treatment may be sunlight, any one or more combinations of LED, xenon lamp, mercury lamp and X-ray lamp.
[0049] The highly dispersed sulfurized hydrogenation catalyst comprises Ni(Co)Mo(W)S x The active phase has a size less than 20 nanometers.
[0050] It should be noted that the boundary high sulfur content Ni(Co)Mo(W)S x The active phase is different in the reaction system of different metal salts. For example, when solution A is Mo salt and solution B is Ni salt, the active phase is NiMoS x ; When solution A is W salt and solution B is Ni salt, the active phase is NiWS x When solution A is a mixed solution of Mo salt and W salt, and solution B is a mixed solution of Ni salt and Co salt, the active phase is Ni(Co)Mo(W)S x .
[0051] It should be noted that the thiomolybdate, thiotungstate, nickel salt, cobalt salt, alcohol, ethanol, triethylamine, triethanolamine, acetonitrile, Y molecular sieve, β molecular sieve, ZSM-5, SAPO molecular sieve, and alumina used in the examples of the present application were all purchased commercially;
[0052] The TEM scanning electron microscope, X-ray photoelectron spectrometer, etc. used in structural testing are all conventional testing instrument models.
[0053] The present application provides a method for preparing a highly dispersed sulfided hydrogenation catalyst, and the details are shown in the following examples.
[0054] Example 1-1
[0055] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0056] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20g of nickel;
[0057] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0058] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethanolamine is added while stirring to obtain a total slurry; irradiation is performed using a 100 W xenon lamp (a 300 W xenon lamp can be used, which is controlled to 100 W by adjusting the flow) for 5 hours;
[0059] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiMoSx, which is dried in a vacuum oven at 60° C. for 6 hours;
[0060] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0061] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiMoS type catalyst.
[0062] Example 1-2
[0063] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0064] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 200mL of cobalt chloride solution (i.e., solution B), wherein solution B contains 20.08g of cobalt;
[0065] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0066] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethanolamine is added while stirring to obtain a total slurry; irradiation is performed for 5 hours using a 100 W xenon lamp (a 300 W xenon lamp can be used, controlled by flow adjustment);
[0067] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed CoMoSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0068] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0069] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a CoMoS type catalyst.
[0070] Examples 1-3
[0071] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0072] Step 1: prepare 2000 mL of ammonium tetrathiotungstate solution (i.e., solution A), wherein solution A contains 50 g of tungsten; prepare 100 mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20 g of nickel;
[0073] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0074] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethanolamine is added while stirring to obtain a total slurry; irradiation is performed for 5 hours using a 100 W xenon lamp (a 300 W xenon lamp can be used, controlled by flow adjustment);
[0075] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiWSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0076] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0077] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiWSx catalyst.
[0078] Example 2-1
[0079] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0080] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 200mL of cobalt chloride solution (i.e., solution B), wherein solution B contains 20.08g of cobalt;
[0081] Weigh 20 g of USY molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0082] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethylamine is added while stirring to obtain a total slurry; 100 W LED light is used for 10 hours;
[0083] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed CoMoSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0084] The catalyst intermediate is placed in a kneader, and a binder is added to form an extrudable paste, which is then extruded into strips; wherein the binder is prepared by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0085] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a CoMoS type catalyst.
[0086] Example 2-2
[0087] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0088] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20g of nickel;
[0089] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0090] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethylamine is added while stirring to obtain a total slurry; 100 W LED light is used for 10 hours;
[0091] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiMoSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0092] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0093] In a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiMoS type catalyst.
[0094] Example 3
[0095] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0096] Step 1: prepare 2000 mL of ammonium tetrathiotungstate solution (i.e., solution A), wherein solution A contains 50 g of tungsten; prepare 100 mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20 g of nickel;
[0097] Weigh 20 g of β molecular sieve dry powder, 200 g of amorphous silica-alumina dry powder and 120 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0098] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 400 mL of triethylamine is added while stirring to obtain a total slurry; 300 W xenon lamp is used for 5 hours;
[0099] Step 3: Filter and wash the material obtained after the light treatment, and the pH of the washing residual liquid is less than 8. The filter cake is a catalyst intermediate for depositing highly dispersed NiWSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0100] The catalyst intermediate is placed in a kneader, and a binder is added to form an extrudable paste, which is then extruded into strips; wherein the binder is prepared by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0101] In a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiWS type catalyst.
[0102] Example 4
[0103] Provided is a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0104] Step 1, prepare 2000mL of 10v% acetonitrile solution of ammonium polysulfide molybdate (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein the slurry contains 20g of nickel;
[0105] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0106] Step 2: At room temperature, solution A and solution B are introduced into slurry C while stirring; irradiation is performed using a 300W xenon lamp for 8 hours;
[0107] Step 3: Filter and wash the material obtained after the light treatment, and the pH of the washing residual liquid is less than 8. The filter cake is a catalyst intermediate for depositing highly dispersed NiWSx, which is dried in a vacuum oven at 60°C for 6 hours;
[0108] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0109] In a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to prepare a NiMoS type catalyst.
[0110] Example 5
[0111] This embodiment provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0112] Step 1: prepare 1000 mL of ammonium tetrathiotungstate solution (i.e., solution A), wherein solution A contains 20 g of tungsten; prepare 100 mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 5 g of nickel;
[0113] Weigh 20 g of USY molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0114] Step 2: At room temperature, solution A and solution B were passed into slurry C, and 200 mL of triethylamine was added while stirring to obtain a total slurry; 300 W xenon lamp was used for 5 hours;
[0115] Step 3: Filter and wash the material obtained after the light treatment, and the pH of the washing residual liquid is less than 8. The filter cake is a catalyst intermediate for depositing highly dispersed NiWSx, which is dried in a vacuum oven at 60° C. for 6 hours;
[0116] The catalyst intermediate is placed in a kneader, and then a binder is added to form a paste for extrusion, and the extrusion is formed; wherein the binder is prepared by peptizing 18g nitric acid and 160g small-pore pseudo-boehmite.
[0117] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiWS catalyst.
[0118] Example 6
[0119] This embodiment provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0120] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20g of nickel;
[0121] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0122] Step 2: At 27°C, solution A and solution B are introduced into slurry C, and 200 mL of triethanolamine is added while stirring to obtain a total slurry; the slurry is illuminated with sunlight for 10 hours;
[0123] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiMoSx, which is dried in a vacuum oven at 60° C. for 6 hours;
[0124] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0125] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiMoS type catalyst.
[0126] Example 7
[0127] This embodiment provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0128] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20g of nickel;
[0129] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0130] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of triethanolamine is added while stirring to obtain a total slurry; a 100 W mercury lamp is used for illumination for 5 hours;
[0131] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiMoSx, which is dried in a vacuum oven at 60° C. for 6 hours;
[0132] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0133] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiMoS type catalyst.
[0134] Example 8
[0135] This embodiment provides a method for preparing a highly dispersed sulfurized hydrogenation catalyst:
[0136] Step 1, prepare 2000mL of ammonium tetrathiomolybdate solution (i.e., solution A), wherein solution A contains 26.11g of molybdenum; prepare 100mL of nickel nitrate solution (i.e., solution B), wherein solution B contains 20g of nickel;
[0137] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry C);
[0138] Step 2: At room temperature, solution A and solution B are passed into slurry C, and 200 mL of ethanol is added while stirring to obtain a total slurry; irradiation is performed using a 100 W xenon lamp (a 300 W xenon lamp can be used, controlled by flow adjustment) for 5 hours;
[0139] Step 3: Filter and wash the material obtained after the light treatment, wash the remaining liquid to pH <8, and the filter cake is a catalyst intermediate for depositing highly dispersed NiMoSx, which is dried in a vacuum oven at 60° C. for 6 hours;
[0140] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0141] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiMoS type catalyst.
[0142] Comparative Example 1
[0143] A preparation method of a sulfidation type hydrogenation catalyst:
[0144] Prepare 2000 mL of ammonium tetrathiomolybdate solution (solution A), the slurry contains 26.11 g of molybdenum; prepare 100 mL of nickel nitrate solution (solution B), the slurry contains 20 g of nickel;
[0145] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (i.e., slurry CC);
[0146] At room temperature, solution A and solution B were passed into slurry C, and 200 mL of triethanolamine was added while stirring; 100 W LED light was used for 5 hours;
[0147] The obtained slurry was filtered and washed, and the pH of the washing residual liquid was less than 8; the filtered mother liquor was collected, and the mother liquor contained 16.43g of molybdenum and 11.22g of nickel that was not deposited.
[0148] The filter cake is a catalyst intermediate of deposited highly dispersed NiMoSx, which is dried in a vacuum oven at 60°C for 6 hours; the catalyst intermediate is placed in a kneader, and a binder made of 18g nitric acid and 160g small-pore pseudo-boehmite peptization is added to make a paste that can be extruded, and extruded into strips. In a nitrogen atmosphere, the molded catalyst is dried at 110°C for 4 hours and calcined at 550°C for 4 hours to obtain NiMoS type catalyst-3.
[0149] By observing the state of the solution, it can be seen from the comparison between Example 1 and Comparative Example 1 that the catalytic degradation of molybdenum salt requires ultraviolet light with a lower wavelength. Example 1 uses a xenon lamp, which can excite a large amount of ultraviolet light, while the LED in Comparative Example 1 cannot provide a large amount of ultraviolet light with a lower wavelength. Under the same irradiation time, the light sources are different and different light intensities are used for irradiation. The LED cannot completely decompose the molybdenum salt and deposit it in situ on the carrier powder. Some of it still exists in the form of aqueous solution, and the reaction mass is a brown heterogeneous solution; compared with Example 2, extending the irradiation time can basically achieve the effect of 5 hours of irradiation in Example 1.
[0150] Comparative Example 2
[0151] Prepare 2000mL of ammonium tetrathiotungstate solution (solution A), the slurry contains 50g of tungsten; prepare 100mL of nickel nitrate solution (solution B), the slurry contains 20g of nickel;
[0152] Weigh 20 g of β molecular sieve dry powder, 200 g of amorphous silica-alumina dry powder and 120 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, and stir and slurry (slurry C);
[0153] The A and B slurries were added to C, and 400 mL of triethylamine was added and stirred; the mixture was stirred for 5 hours without applying light; no reaction effect was observed, and the reaction was continued for 10 hours, but still no change occurred;
[0154] The obtained slurry was filtered and washed, and the pH of the washing residue was less than 8; the filter cake was a catalyst intermediate of deposited highly dispersed NiWSx, which was dried in a vacuum oven at 60°C for 6 hours;
[0155] The catalyst intermediate is placed in a kneader, and then a binder is added to make a paste that can be extruded into strips, and then extruded into strips; wherein the binder is made by peptizing 18g of nitric acid and 160g of small-pore pseudo-boehmite.
[0156] Under a nitrogen atmosphere, the molded catalyst was dried at 110° C. for 4 hours and calcined at 550° C. for 4 hours to obtain a NiWS catalyst.
[0157] Comparative Example 2 is compared with Example 3. No light is applied, the catalyst intermediate has no obvious color change, and there is basically no nickel / tungsten deposition (that is, the W salt and the Ni salt are not decomposed, and no active components are deposited on the carrier). ICP (ion pair chromatography) measured that the catalyst obtained in Comparative Example 2 has 1247.1 ppm nickel and 422.7 ppm tungsten. After the total slurry is allowed to stand, the material presents the original brown transparent clear solution (different from the black heterogeneous solution after the light reaction is completed).
[0158] Comparative Example 3
[0159] Prepare 2000mL of tetrathiomolybdenum / ammonium tungstate composite solution (solution A), the slurry contains 18.05g of molybdenum and 25g of tungsten; prepare 100mL of nickel nitrate / cobalt composite solution (solution B), the slurry contains 10g of nickel and 10.04g of cobalt;
[0160] Weigh 20 g of β molecular sieve dry powder, 250 g of amorphous silica-alumina dry powder and 70 g of macroporous pseudo-boehmite, add them into a sealed glass jar containing 2000 mL of water, stir and slurry (slurry C);
[0161] Solution A and solution B are added to slurry C without adding any sacrificial reagent such as triethanolamine or triethylamine; irradiation is performed using a 300W xenon lamp for 5 hours;
[0162] The obtained slurry is filtered and washed, and the pH of the washing residual liquid is less than 8; the filtered mother liquid is collected;
[0163] The filter cake was dried in a vacuum oven at 60°C for 6 hours; the catalyst intermediate was placed in a kneader, and 18g of nitric acid and 160g of a binder made of small-pore pseudo-boehmite peptized were added to make a paste that can be extruded, and extruded into strips. In a nitrogen atmosphere, the molded catalyst was dried at 110°C for 4 hours and calcined at 550°C for 4 hours to obtain CoNiMoWS x Type catalyst.
[0164] Through detection and observation, it can be seen that the mother liquor is still brown, indicating that some metal salts are not deposited. ICP measured that the mother liquor contained 7.16g of molybdenum, 4.96g of nickel, 18.31g of tungsten and 2.11g of cobalt that were not deposited.
[0165] The filter cake is a deposited highly dispersed CoNiMoWS x Composite catalyst intermediates.
[0166] It should be noted that in Comparative Example 3, no sacrificial reagent was applied, and part of the hydrogenation site precursor (ie, molybdenum / tungsten metal salt) was still present in the water without deposition.
[0167] In the coexistence of solution A and solution B, the ions are described as Co\Ni2MoS4 and Co\Ni2WS4. Under light conditions, the decomposition rate of Co\Ni2MoS4 is lower than the decomposition rate of Co\Ni2WS4. Since there is no sacrificial reagent to provide electrons to annihilate conduction band holes, most of the valence band electrons can only return to the ground state from the excited state, so that the valence state of molybdenum and tungsten is still 6. + Therefore, the amount of molybdenum deposited by the catalyst obtained in Comparative Example 3 is much greater than the amount of tungsten deposited.
[0168] The present application provides a highly dispersed sulfided hydrogenation catalyst, which is obtained by the method of any of the above embodiments.
[0169] Specifically, the electron microscope image of the carrier precursor is shown in the attached Figure 1 As shown, it is a scanning electron microscope image of the β molecular sieve body of Example 1, in which highly dispersed active sites are not formed;
[0170] Specifically, the intermediate of the catalyst is shown in the attached specification. Figure 2 , Figure 2 TEM scanning electron microscope image of the NiMoSx catalyst intermediate of Example 1;
[0171] Specifically, Figure 3 , Figure 4 , Figure 5 The catalyst CoMoS of Example 1-2 x The electron binding energy spectrum of cobalt, sulfur and molybdenum in the intermediates; it can be seen that cobalt / nickel metal promotes the decomposition of molybdenum / tungsten salts, and cobalt / nickel competes for sulfur at the boundary of molybdenum / tungsten, forming a part of Ni(Co)-S-Mo(W) bond; in the process of forming molybdenum / tungsten sulfide under light, the formation of Ni(Co)-S-Mo(W) bond causes part of S to be vacated to form S2 2- Form exists (see Figure 4 ), in addition, the influence of the Mo(W) electron energy state on Ni(Co)S in the Ni(Co)-S-Mo(W) bond causes the cobalt 2p orbital to shift to a lower binding energy (compared with the cobalt sulfide sample), which demonstrates the strong chemical force of the bond.
[0172] The catalyst of the present application forms highly dispersed hydrogenation sites in advance through light irradiation. Compared with the prior art that forms hydrogenation sites during the final high-temperature calcination process, the advantage is that in addition to having high dispersion and high activity, it also avoids the influence of metal salts on the carrier strength in advance. The carrier strength is an important measurement indicator for whether the catalyst in the refining industry can operate stably for many years and avoid losses caused by sudden shutdown.
[0173] Catalyst performance evaluation test
[0174] Catalysts from different embodiments and comparative examples (Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1, Comparative Example 2, Comparative Example 3) were taken as samples. The test was carried out on a 200ml small hydrogenation device. The properties of the raw oil used are shown in Table 1.
[0175] The operating conditions are as follows: hydrogen partial pressure 15.0 MPa, hydrogen to oil volume ratio 1500:1, liquid hourly volume space velocity 0.9 h -1 .
[0176] Commercial catalysts are listed in Table 2;
[0177] The test results of the catalytic activity of the catalyst are shown in Table 3.
[0178] Table 1 Properties of the evaluation stock oil
[0179]
[0180]
[0181] Table 2 Physical and chemical properties of commercial hydrocracking catalysts
[0182] project unit data <![CDATA[WO3]]> wt% 24.15 NiO wt% 7.58 <![CDATA[Al2O3]]> wt% 44.98 <![CDATA[SiO2]]> wt% 21.32 Kong Rong cm3 / g 0.357 Specific surface area m2 / g 181.97 Diameter*Length mm*cm 2.38*3-8 Bulk density g / cm3 0.928 Crushing strength N / cm 226 shape Cylindrical Bar
[0183] Table 3 Reaction conditions and evaluation results of catalysts of Examples and Comparative Examples
[0184]
[0185] According to Table 3, it can be seen from the comparison of Example 1-1, Example 2-1, Example 3 and Comparative Example 2 that the catalytic degradation of molybdenum and tungsten salts requires ultraviolet light with a lower wavelength, and the xenon lamp can excite a large amount of ultraviolet light (Example 1 and Example 3), while the LED requires a long time of irradiation to react (Comparative Example 2, Example 2-2), and the amount of ultraviolet light with a lower wavelength required by the LED is small. Comparative Example 2 did not undergo a photocatalytic decomposition reaction, and the active sites formed were insufficient, and it had almost no reaction catalytic ability, and was inferior to commercial catalysts. This shows that the edge sites of molybdenum / tungsten sulfide with catalytic activity formed by light irradiation are fully exposed, which greatly improves the catalytic effect of the catalyst, and the obtained catalyst is more stable than the existing catalyst that has been oxidized and sulfided;
[0186] By comparing Example 1-1, Example 1-2, and Example 1-3, it can be seen that the four metal salts can be well loaded on the carrier under photocatalysis, achieving a good catalytic effect, and the diesel yield is much higher than that of commercial catalysts. The cetane number of the oil obtained by catalysis in the examples of the present application is also higher than that of the oil obtained by catalysis with commercial catalysts, and the tail oil yield is much lower than that of commercial catalysts.
[0187] By comparing Example 5, Example 6, Example 7 and Example 8, it can be seen that within the appropriate range of metal salts, the catalyst of the present application can be obtained by replacing different light sources and sacrificial agents, that is, the catalyst preparation conditions of the present application are simple and have broad market prospects;
[0188] Comparative Example 3 is a comparison without a sacrificial reagent. Under the irradiation of the maximum light source, it is shown that the stability of tetrathiomolybdate is different from that of the corresponding tetrathiotungstate. The lack of a sacrificial reagent to provide electrons to annihilate valence band holes results in a low loading rate of the metal salt and a low catalytic effect of the catalyst.
[0189] The above is a detailed introduction to a highly dispersed sulfided hydrogenation catalyst and a preparation method thereof provided in the examples of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present application.
Claims
1. A method for preparing a highly dispersed sulfided hydrogenation catalyst, characterized in that: The steps include: Step 1, preparing a solution A of thiomolybdate or thiotungstate, and preparing a solution B of nickel salt or cobalt salt; Taking a hydrocracking carrier component, mixing the powder of the hydrocracking carrier component with a solvent and slurrying the mixture to obtain a slurry C; Step 2: at room temperature, passing solution A and solution B into slurry C, and adding a sacrificial reagent to obtain a total slurry, and isolating the total slurry from air; wherein the sacrificial reagent accounts for 1%-10% of the volume of the total slurry; Stirring the total slurry, and simultaneously performing light treatment on the total slurry, wherein the light source used in the light treatment emits light with a wavelength of λ≤620nm, and the light treatment time is 5h-20h; Step 3: filtering, washing, and first drying the material obtained after the light treatment, and kneading it with a binder to form it; and drying and calcining it for a second time under an inert atmosphere to obtain a highly dispersed sulfurized hydrogenation catalyst.
2. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: The light source used in the light treatment includes one or more of sunlight, LED, xenon lamp, mercury lamp, and X-ray lamp.
3. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: The sacrificial agent includes a mixture of one or more of methanol, ethanol, triethylamine, triethanolamine, and acetonitrile.
4. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: The thiomolybdate or thiotungstate is selected from ammonium salt and tetraalkylamine salt; the nickel salt or cobalt salt is selected from chloride and nitrate.
5. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to any one of claims 4, characterized in that: 1L of solution A contains 5g-100g of Mo and / or W; 100mL of solution B contains 1g-40g of Ni and / or Co.
6. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: The hydrocracking carrier component at least includes one or more acidic cracking components selected from molecular sieves and amorphous silica-alumina.
7. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 6, characterized in that: The molecular sieve comprises one or more combinations of Y molecular sieve, β molecular sieve, ZSM-5 and SAPO molecular sieve; the mass fraction of the acidic cracking component in the hydrocracking carrier component is 5-50%; each of the acidic cracking components comprises 5-40% alumina.
8. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: In the step 1, the solvent includes water, and the slurry ratio of the powder of the hydrocracking carrier component and the solvent is (1 g: 5 mL) - (1 g: 10 ml).
9. The method for preparing a highly dispersed sulfided hydrogenation catalyst according to claim 1, characterized in that: In the step three, The first drying condition is 60°C-110°C, vacuum drying for 5h-20h; Under an inert atmosphere, the second drying condition is 80-150°C for 2h-5h, and the roasting condition is 500°C-850°C for 4-10h; Wherein, the binder comprises peptized small-pore alumina.
10. A highly dispersed sulfided hydrogenation catalyst, characterized in that: The highly dispersed sulfided hydrogenation catalyst comprises Ni(Co)Mo(W)S x The active phase has a size less than 20 nanometers.