Preparation method and application of honeycomb-type COF-based composite catalyst material

Honeycomb-type COF is prepared by low-temperature solvent-thermal method and two-step gradient heating method, and sulfur-based semiconductor materials are introduced in combination with in-situ coprecipitation method, which solves the problem that it is difficult to prepare three-dimensional ordered macroporous COF in the prior art. It achieves high-efficiency photocatalytic hydrogen production performance and structural integrity, and improves the utilization efficiency and economic benefits of materials.

CN119034822APending Publication Date: 2024-11-29JIANGSU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411172813.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to prepare honeycomb-type COF catalysts with three-dimensional ordered macroporous structures through the template self-sacrifice method, and it is easy to cause collapse of the pore structure or damage to the chemical structure during the template removal process, limiting the efficiency and sustainability of the material. sex.

Method used

The monodispersed polystyrene ball template was prepared by low-temperature solvent-thermal method, and honeycomb-type COF with mesoporous, micropores and continuous macropores were directly synthesized by a two-step gradient heating method. The sulfur-based semiconductor material was introduced in combination with in situ coprecipitation method. Form a honeycomb-type COF composite catalyst.

Benefits of technology

The structural integrity and efficient photocatalytic hydrogen production performance of honeycomb COF composite catalyst are achieved, the carrier separation and transfer capabilities are improved, the preparation cost and time are reduced, and the photocatalytic hydrogen evolution activity is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034822A_ABST
    Figure CN119034822A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material preparation and hydrogen production, in particular to a preparation method and application of a honeycomb type COF composite catalyst material. According to the invention, a three-dimensional ordered polystyrene sphere template and dimethyl sulfoxide are used as a reaction solvent, and the honeycomb-type COF material with three-dimensional macropores is prepared through two-step heating; and then, preparing the honeycomb type COF composite catalyst by taking the honeycomb type COF material as a carrier and utilizing an in-situ coprecipitation method. The three-dimensional ordered macroporous structure is beneficial to loading the chalcogenide semiconductor nanomaterial on the COF material to realize strong interface bonding, and promotes charge separation and transfer between the honeycomb-type COF and the chalcogenide semiconductor, thereby realizing high-efficiency hydrogen production activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material preparation and hydrogen production, and in particular to a method for preparing a honeycomb COF composite catalyst material and its application, specifically a method for synthesizing a honeycomb COF-based catalyst by an in-situ technique of template self-sacrifice, and in-situ loading of a sulfur-based semiconductor on the honeycomb COF catalyst to prepare a honeycomb COF-based composite catalyst material, which is applied in the technical field of hydrogen production. Background Art

[0002] Hydrogen energy is regarded as an energy source with great prospects. It has attracted much attention due to its environmental protection, economy, high energy density and other characteristics, and has been widely used to deal with global energy crisis and environmental pollution. However, hydrogen energy currently mainly relies on the production of fossil fuels from non-renewable resources. The production process is energy-intensive and has a great impact on the environment, which limits the development of hydrogen (H 2 ) production sustainability and cost-effectiveness. Therefore, exploring a cost-effective method to produce H 2 The technology has urgent needs and potential commercial value.

[0003] So far, many studies have demonstrated that water splitting driven by semiconductor photocatalysts is a promising hydrogen production technology. Among various semiconductor photocatalysts, covalent organic frameworks (COFs) materials are considered to be an excellent candidate material because of their adjustable pore size structure, large specific surface area, and stable structural properties. The ordered pores in COFs materials can not only provide spatial confinement for catalytic active sites, but also provide specific paths for the transport of reaction substrates and products. These unique structural characteristics make COFs materials show great potential in heterogeneous catalytic systems. However, most reported COFs themselves contain only micropores or smaller mesopores (<5nm), which often limit the mass transfer and diffusion of reaction substrates, especially the utilization efficiency of active sites inside the material. Introducing mesoporous or macroporous structures, especially three-dimensional ordered macroporous structures, into COFs is considered to be an effective way to improve the utilization of internal active sites.

[0004] The preparation of three-dimensional ordered macroporous materials often adopts the template method. First, spherical silica (SiO 2 ) or polystyrene balls (PS) as hard templates, the material will grow in the gaps of the templates, and then the templates are removed by heat treatment or acid-base etching. 2 It can be used as a template for preparing honeycomb COF, but this requires SiO 2The template is etched to obtain three-dimensional interconnected macroporous channels. However, in the process of removing the template, high temperature treatment or acid-base etching will inevitably lead to the collapse of the COF pore structure or the destruction of the chemical structure. The synthesis of COF needs to be carried out in an organic solvent. Most solvents for synthesizing COF, such as dioxane, N,N-dimethylacetamide (DMAC) and mesitylene, will cause the PS template to dissolve directly at room temperature and cannot form a three-dimensional ordered macroporous structure. Therefore, it is very challenging to explore a method for constructing a honeycomb COF with a three-dimensional ordered macroporous structure by template self-sacrifice, which has not been realized so far. The present invention proposes a method for synthesizing a honeycomb COF with an in-situ technique of template self-sacrifice. PS is used as a template, and the PS template self-sacrifice method is used to synthesize a honeycomb COF by selecting a COF solvent and gradient heating. This method does not require secondary heat treatment or acid-base etching to remove the template, ensures the integrity of the honeycomb COF structure with macropores, and saves the time and cost of removing the template. Based on the above background, the present invention synthesizes a honeycomb COF with a template self-sacrificing in-situ technology, and uses the honeycomb COF material as a carrier. By virtue of the ordered nanopores and high stability of the honeycomb COF material, a sulfur-based semiconductor is in-situ loaded thereon to construct a honeycomb COF composite catalyst material. The prepared honeycomb COF composite catalyst material exhibits excellent photocatalytic hydrogen production performance. Summary of the invention

[0005] The present invention provides a method for synthesizing a honeycomb COF-based composite catalyst with a three-dimensional macroporous structure by an in-situ technique of template self-sacrifice, wherein the separation and transfer capabilities of carriers are enhanced by in-situ loading of sulfur-based semiconductor materials on the honeycomb COF, thereby improving the performance of photocatalytic water decomposition to produce hydrogen.

[0006] The present invention prepares monodisperse colloidal polystyrene spheres by a low-temperature solvothermal method, and assembles a three-dimensional ordered polystyrene sphere template after a long period of low-speed centrifugation. Further, a honeycomb COF having mesoporous, microporous and continuous macroporous structures is directly prepared by a two-step gradient heating. Finally, a honeycomb COF-based composite photocatalyst is prepared by introducing a sulfur-based semiconductor material into the honeycomb COF structure by an in-situ coprecipitation method. This type of catalyst exhibits excellent photocatalytic hydrogen production activity.

[0007] The present invention achieves the above technical objectives through the following technical solutions.

[0008] A method for preparing a honeycomb COF catalyst co-precipitated S-series semiconductor material by a template self-sacrificial method, comprising the following steps:

[0009] 1. Preparation of monodisperse polystyrene spheres: styrene was washed with sodium hydroxide (NaOH) solution and deionized water in turn; then, the washed styrene was added to a three-necked round-bottom flask containing polyvinylpyrrolidone (PVP) aqueous solution; 2 After bubbling for 15-30 min, stir in an oil bath at 50-100 °C for 10-60 min under magnetic stirring; then, 2 S 2 O 8 The aqueous solution is added into the above three-necked flask to initiate the polymerization reaction of styrene. After continuous stirring for 10-30 hours (preferably 24 hours), the mixture is cooled to room temperature to obtain a milky product which is monodisperse colloidal polystyrene spheres.

[0010] 2. Preparation of three-dimensional ordered polystyrene sphere template: The monodispersed polystyrene spheres in step 1 are placed in a centrifuge tube for ultrasonic treatment to form a uniform emulsion, and then centrifuged at a speed of 1-3 krpm. The obtained precipitate is dried at 30-60°C overnight, and after natural cooling, the three-dimensional ordered polystyrene sphere template is collected.

[0011] 3. Preparation of honeycomb COF photocatalyst: The aldehyde precursor was added to the dimethyl sulfoxide solution, and then the three-dimensional ordered polystyrene sphere template was immersed in the above solution for 10-60 min. The aldehyde precursor solution was evenly infiltrated into the template by vacuum degassing. N 2 Then, a dimethyl sulfoxide solution containing an amine precursor was added and stirred at N 2 The temperature is increased in two steps under the atmosphere, and the total reaction time is 1-5 days. The precipitate is washed by centrifugation with an organic solvent, and dried in a vacuum oven at 50-100° C. for 6-18 hours to obtain a honeycomb COF photocatalyst.

[0012] 4. Preparation of honeycomb COF composite photocatalyst: The honeycomb COF photocatalyst prepared in step 3 was dispersed in an aqueous solution and subjected to ultrasonic treatment. Then, a metal source was added and stirred at room temperature for 1-3 h. Then, a sulfur source (Na 2 S˙9H 2 O aqueous solution), stirred for 5-10 hours, allowed to stand for 10-20 hours, washed by centrifugation with deionized water, and dried in vacuo at 50-100°C to obtain a honeycomb COF-based composite catalyst.

[0013] Furthermore, in step 1, the concentration of the NaOH solution is 10 wt.%, the concentration of the PVP aqueous solution is 1-10 g / L, and the K 2 S 2 O 8 The concentration of the aqueous solution is 5-30g / L, and the washed styrene, PVP aqueous solution and K 2 S 2 O8 The volume ratio of the aqueous solution is 1:1-10:0.1-1, and the stirring rate in the polymerization step is maintained at 100-500 rpm.

[0014] In the step 2, the ultrasonic treatment time is 10-50 min, the temperature of the ultrasonic machine is maintained below 30° C., and the ultrasonic frequency is maintained at 40-60 KHz.

[0015] In step 3, the molar ratio of the aldehyde precursor to the amine precursor is 1 to 3:1, preferably 1.5:1, the mass ratio of the three-dimensional ordered polystyrene sphere template to the amine precursor is 15-30:1, N 2 The first step of heating under atmosphere is maintained at 30-70°C, the heating rate is 1-5°C / min, and the reaction is performed for 4-8h. The second step of heating is maintained at 80-150°C, the heating rate is 1-5°C / min, and the organic solvent used for centrifugation is at least one of acetone, tetrahydrofuran, methanol, chloroform, N,N-dimethylacetamide, dioxane, and dichloromethane.

[0016] The metal source in step 4 refers to Zn(NO 3 ) 2 6H 2 O.Cd(NO 3 ) 2 4H 2 O and InCl 3 4H 2 O, at least one of the metal sources and Na 2 S˙9H 2 The molar ratio of O is 1:1-3, Na 2 S˙9H 2 The concentration of the O aqueous solution is 10.4 g / L, and the mass ratio of the added amount of the honeycomb COF and the metal source is 0.1-1:1.

[0017] In step 3 of the above preparation method, the aldehyde precursor is one of the following structures, and its structural formula is as follows:

[0018]

[0019] The amino precursor is one of the following structures, and its structural formula is as follows:

[0020]

[0021] The principle of preparing the honeycomb COF photocatalyst by the template self-sacrificing method of the present invention is:

[0022] Using three-dimensional ordered polystyrene sphere templates and dimethyl sulfoxide as the reaction solvent, a honeycomb COF material with three-dimensional macropores was prepared by two steps of heating. Then, the honeycomb COF material was used as a carrier to prepare the honeycomb COF composite catalyst by in-situ coprecipitation. The three-dimensional ordered macroporous structure is conducive to the strong interface bonding of sulfur-based semiconductor nanomaterials loaded on COF materials, promoting the charge separation and transfer between honeycomb COF and sulfur-based semiconductors, thereby achieving efficient hydrogen production activity.

[0023] Compared with the prior art, the present invention has the following beneficial technical effects:

[0024] (1) In the process of preparing the honeycomb COF photocatalyst, the present invention can directly prepare a three-dimensional ordered macroporous covalent organic framework material by selecting a suitable reaction solvent and a two-step heating method, without calcining the polystyrene sphere template or dissolving it in a specific solvent. There is currently no report on the preparation of porous COF catalysts by self-sacrificing templates.

[0025] (2) The present invention utilizes the macroporous structure of the honeycomb COF to effectively load sulfur-based semiconductors, effectively improving the separation and transmission capabilities of electron-hole pairs in the composite catalytic system, thereby enhancing the photocatalytic hydrogen evolution capability of the honeycomb COF composite photocatalyst.

[0026] (3) The template self-sacrificial preparation method of the present invention can not only ensure the structural integrity of the honeycomb COF, but also save the cost and time of the reaction and improve the economic benefits of the synthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a scanning electron microscope image of the polystyrene sphere template of the present invention;

[0028] Figure 2 This is the XRD pattern of the honeycomb COF prepared in Example 1 of the present invention;

[0029] Figure 3 This is the thermogravimetric diagram of the honeycomb COF prepared in Example 1 of the present invention;

[0030] Figure 4 Scanning (left) and transmission (right) electron micrographs of the honeycomb COF prepared in Example 1 of the present invention;

[0031] Figure 5 In prepared in Example 1 of the present invention 2 S 3 / Transmission electron microscopy image of honeycomb COF. DETAILED DESCRIPTION

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.

[0033] Evaluation of the photocatalytic activity of the photocatalyst prepared in the present invention:

[0034] Photocatalytic hydrogen evolution performance test: The photocatalytic hydrogen evolution performance of different samples is measured by the rate at which the photocatalyst produces hydrogen under the irradiation of LED-420nm single-wave light source. The detection device is a GC-2014 gas chromatograph manufactured by Shimadzu Corporation of Japan. The specific operation is as follows: A 100mL three-necked flask is used as the reaction container, and a certain amount of the sample to be tested is weighed and ultrasonically dispersed into 80mL of a solution containing 10% (Vol) lactic acid as a hole sacrificial agent. The bottle stopper is wrapped with a multi-layer sealing film to ensure the airtightness of the reaction bottle, and the air guide tubes at both ends are passed through high-purity N in a long-in and short-out manner. 2 , and keep it for 15 minutes to remove the impurity gas in the reactor. At room temperature, place it under the LED-420nm single-wave light source and stir it continuously during the illumination process. Online detection is performed every 1 hour to determine the amount of gas generated, and finally H 2 The yield.

[0035] Embodiment 1:

[0036] (1) Preparation of monodisperse colloidal polystyrene spheres:

[0037] First, 70 mL of styrene was thoroughly washed with 20 mL of 10 wt.% NaOH solution and deionized water in order to remove the stabilizer. Then, 65 mL of the washed styrene was added to a 1 L three-necked round-bottom flask and 500 mL of an aqueous solution containing 2.5 g of PVP was added. 2 After bubbling for 15 min, the mixture was stirred in an oil bath at 60 °C for 30 min under magnetic stirring. 2 S 2 O 8 The aqueous solution of 1,4-dihydro-1-nitropropene was quickly added to the three-necked round-bottom flask to initiate the polymerization of styrene. After continuous stirring for 24 hours, the mixture was cooled and the obtained milky product was monodisperse colloidal polystyrene spheres. It is worth noting that the stirring rate in the polymerization step was 400 rpm, because a higher stirring rate would lead to the agglomeration of monodisperse colloidal polystyrene spheres.

[0038] The preparation methods of five polystyrene balls with different particle sizes are shown in the following table:

[0039] Styrene (mL) PVP(g) <![CDATA[K 2 S 2 O 8 (g)]]> Temperature(℃) Average diameter(nm) 65 2.5 1 75 270 65 2.5 1 94 190 65 2.5 1 60 340 59 0.6 0.2 75 400 59 0 0.2 87 470

[0040] In this Example 1, monodisperse colloidal polystyrene spheres with a diameter of 340 nm were selected for subsequent experiments.

[0041] (2) Preparation of three-dimensional ordered polystyrene sphere template:

[0042] The monodisperse polystyrene spheres were placed in a 50 ml centrifuge tube for ultrasonic treatment to form a uniform emulsion, which was then centrifuged at 2 krpm for 12 hours. The obtained precipitate was dried at 50°C overnight, and after natural cooling, the three-dimensional ordered polystyrene sphere template was collected.

[0043] (3) Preparation of honeycomb COF catalyst:

[0044] Honeycomb COF was prepared by template self-sacrificing in-situ technology. First, 2,4,6-trihydroxybenzene-1,3,5-tricarbaldehyde (Tp, 0.13 mmol) was dissolved in 5 mL of dimethyl sulfoxide solution. Then, 1 g of polystyrene sphere template was immersed in the above solution for 30 minutes and then vacuum degassed for 10 minutes to allow the precursor solution to evenly penetrate into the template. N 2 , and then 2 ml of dimethyl sulfoxide solution containing 4,4',4"-(1,3,5-triazine-2,4,6-triyl)triphenylamine (Tta, 0.07 mmol) was added. Finally, a two-step gradient temperature increase was performed, maintaining at 60°C for 3 hours, and then the temperature was increased to 120°C and reacted for 3 days. The precipitate was washed several times with methanol and N,N-dimethylformamide, and vacuum dried at 70°C overnight. A honeycomb COF photocatalyst was obtained.

[0045] (4)In 2 S 3 / Preparation of honeycomb COF composite photocatalyst:

[0046] In situ co-precipitation strategy was used to obtain 2 S 3 / honeycomb COF. 40 mg of honeycomb COF was dispersed in 150 ml of deionized water and ultrasonicated for 15 minutes. Then 0.258 g InCl 3 4H 2 O, stirred at room temperature for 1 h, and then added 0.415 g Na 2 S˙9H 2 O in 40 mL aqueous solution and stirred for 8 h. After standing for 12 h, it was centrifugally washed with deionized water 6 times and dried in a vacuum oven at 70 °C to obtain In 2 S 3 / honeycomb COF composite photocatalyst.

[0047] (5) Using a 100 mL three-necked flask as a reaction vessel, take In (4) 2 S 30.005 g of honeycomb COF photocatalyst was ultrasonically dispersed into 80 mL of a solution containing 10% (Vol) lactic acid as a hole sacrificial agent. The bottle stopper was wrapped with a multi-layer sealing film to ensure the airtightness of the reaction bottle. The air guide tubes at both ends were connected to high-purity N in a long-in and short-out manner. 2 , and keep it for 15 minutes to remove the impurity gas in the reactor. At room temperature, place it under the LED-420nm single-wave light source and continue stirring during the illumination process. Online detection is performed every 1 hour to determine the amount of gas generated, and finally the 3-hour H 2 The yield was 68.9 mmol / g.

[0048] Embodiment 2:

[0049] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (1) of embodiment 1, the size of the monodisperse colloidal polystyrene spheres is adjusted by changing the amount of PVP to 0.6 g PVP, and K 2 S 2 O 8 Adjust to 0.2g.

[0050] Embodiment 3:

[0051] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (1) of embodiment 1, the size of the monodisperse colloidal polystyrene spheres is adjusted by changing the temperature of the oil bath to 75°C.

[0052] Embodiment 4:

[0053] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (2) of embodiment 1, the arrangement of the three-dimensional ordered polystyrene spheres is adjusted by changing the centrifugal speed to 1.5 krpm.

[0054] Embodiment 5:

[0055] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (2) of embodiment 1, the arrangement of the three-dimensional ordered polystyrene spheres is adjusted by changing the centrifugation time to 15 h.

[0056] Embodiment 6:

[0057] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the aldehyde monomer to 2,4-dihydroxybenzene-1,3,5-tricarbaldehyde.

[0058] Embodiment 7:

[0059] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the aldehyde monomer to 2-hydroxybenzene-1,3,5-tricarbaldehyde.

[0060] Embodiment 8:

[0061] The method and steps of this embodiment are consistent with those of embodiment 1, except that only in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the aldehyde monomer to 1,3,5-benzenetricarboxaldehyde.

[0062] Embodiment 9:

[0063] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the amino monomer to p-phenylenediamine.

[0064] Embodiment 10:

[0065] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the amino monomer to 2,5-diaminepyridine.

[0066] Embodiment 11:

[0067] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (3) of embodiment 1, the honeycomb COF structure is adjusted by changing the amino monomer to 5,5-diamino-2,2-bipyridine.

[0068] Embodiment 12:

[0069] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (4) of embodiment 1, the composite photocatalyst prepared by changing the sulfur source is changed to 0.262 g Zn(NO 3 ) 2 6H 2 O.

[0070] Embodiment 13:

[0071] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (4) of embodiment 1, the composite photocatalyst prepared by changing the sulfur source is changed to 0.271 g Cd(NO 3 ) 2 ˙4H 2 O.

[0072] Embodiment 14:

[0073] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (4) of embodiment 1, the composite photocatalyst prepared by changing the sulfur source is changed to 0.129 g InCl 3 ˙4H 2 O and 0.131g Zn(NO 3 ) 2 ˙6H 2 O.

[0074] Embodiment 15:

[0075] The method and steps of this embodiment are consistent with those of embodiment 1, except that in step (4) of embodiment 1, the composite photocatalyst prepared by changing the sulfur source is changed to 0.129 g InCl 3 ˙4H 2 O and 0.135g Cd(NO 3 ) 2 ˙4H 2 O.

[0076] Comparative Example 1:

[0077] (1)In 2 S 3 Preparation of nanomaterial photocatalysts:

[0078] In was prepared by precipitation method. 2 S 3 Nanomaterials. Add 0.258g InCl in 150mL deionized water. 3 ˙4H 2 O, stirred at room temperature for 1 h, and then added 0.415 g Na 2 S˙9H 2 O in 40 mL aqueous solution and stirred for 8 h. After standing for 12 h, the precipitate was washed six times by centrifugation with deionized water and dried overnight at 70 °C. 2 S 3 Photocatalyst.

[0079] (2) Using a 100 mL three-necked flask as a reaction vessel, take In (1) 2 S 3 0.005 g of the photocatalyst was ultrasonically dispersed into 80 mL of a solution containing 10% (Vol) lactic acid as a hole sacrificial agent. The bottle stopper was wrapped with a multi-layer sealing film to ensure the airtightness of the reaction bottle. The air guide tubes at both ends were connected to high-purity N in a long-in and short-out manner. 2 , and keep it for 15 minutes to remove the impurity gas in the reactor. At room temperature, place it under the LED-420nm single-wave light source and continue stirring during the illumination process. Online detection is performed every 1 hour to determine the amount of gas generated, and finally the 3-hour H2 The yield was 12.9 mmol / g.

[0080] Comparative Example 2:

[0081] (1) Preparation of Bulk-COF Catalyst:

[0082] First, 2,4,6-trihydroxybenzene-1,3,5-tricarbaldehyde (Tp, 0.13 mmol) was dissolved in 5 mL of dimethyl sulfoxide solution. 2 , then 2 ml of dimethyl sulfoxide solution containing 4,4',4"-(1,3,5-triazine-2,4,6-triyl)triphenylamine (Tta, 0.07 mmol) was added. Finally, a two-step gradient temperature increase was performed, maintaining at 60°C for 3 hours, and then the temperature was increased to 120°C and reacted for 3 days. The precipitate was washed several times with methanol and N,N-dimethylformamide, and vacuum dried at 70°C overnight. Bulk-COF photocatalyst was obtained.

[0083] (2)In 2 S 3 Preparation of Bulk-COF Photocatalyst:

[0084] In situ co-precipitation strategy was used to obtain 2 S 3 / Bulk-COF. 40 mg of Bulk-COF was dispersed in 150 ml of deionized water and ultrasonicated for 15 minutes. Then 0.258 g of InCl 3 4H 2 O, stirred at room temperature for 1 h, and then added 0.415 g Na 2 9H 2 O in 40 mL aqueous solution and stirred for 8 h. After standing for 12 h, it was centrifugally washed with deionized water 6 times and dried in a vacuum oven at 70 °C to obtain In 2 S 3 / Bulk-COF composite photocatalyst.

[0085] (3) Using a 100 mL three-necked flask as a reaction vessel, take In (2) 2 S 3 0.005 g of Bulk-COF photocatalyst was ultrasonically dispersed into 80 mL of a solution containing 10% (Vol) lactic acid as a hole sacrificial agent. The bottle stopper was wrapped with a multi-layer sealing film to ensure the airtightness of the reaction bottle. The air guide tubes at both ends were connected to high-purity N in a long-in and short-out manner. 2, and keep it for 15 minutes to remove the impurity gas in the reactor. At room temperature, place it under the LED-420nm single-wave light source and continue stirring during the illumination process. Online detection is performed every 1 hour to determine the amount of gas generated, and finally the 3-hour H 2 The yield was 39 mmol / g.

[0086] like Figure 1 Shown is a scanning electron micrograph of a polystyrene sphere template, showing smooth spheres with a diameter of 340 nm and neatly arranged.

[0087] Figure 2 The X-ray diffraction pattern of the honeycomb COF. The XRD pattern shows the crystallinity of the honeycomb COF. The peaks at 5.7, 9.6 and 14.9° correspond to the plane reflections of (100), (110) and (210), respectively, and the broad peak appearing at a higher 2θ value (~26.5°) is attributed to the (001) plane reflection, which is caused by the π-π stacking between continuous layers. This proves the successful preparation of the honeycomb COF.

[0088] Figure 3 The thermogravimetric diagram of honeycomb COF. The first level of weight loss (<100°C) is due to the evaporation of a small amount of methanol solvent molecules or water in the air, the second level of weight loss (100-200°C) is due to the evaporation of a small amount of high boiling point solvent molecules or the loss of surface functional groups, and the third level of weight loss (≥200°C) is due to the decomposition of bulk materials. This shows that the honeycomb COF material has good thermal stability.

[0089] Figure 4 Scanning and transmission electron micrographs of honeycomb COFs show the ordered macroporous structure of the honeycomb COF material.

[0090] Figure 5 ForIn 2 S 3 Transmission electron microscopy image of a honeycomb COF. It shows that In grown in the ordered macroporous structure of the honeycomb COF material 2 S 3 Nanomaterials. This illustrates the successful preparation of the composite catalyst.

[0091] Table 1 Hydrogen production performance of the photocatalytic materials provided in the embodiments of the present invention.

[0092]

[0093]

[0094] The preferred embodiments of the present invention are described in detail above, but the protection scope of the present invention is not limited thereto, and any modification, equivalent replacement and improvement made by any technician familiar with the technical field within the technical scope disclosed by the present invention shall be included in the protection scope of the invention.

Claims

1. A method for preparing a honeycomb COF-based composite catalyst material, characterized in that: (1) Preparation of honeycomb COF photocatalyst: an aldehyde precursor is added to a dimethyl sulfoxide solution, and then a three-dimensional ordered polystyrene sphere template is immersed in the dimethyl sulfoxide solution, and a vacuum degassing treatment is performed to allow the aldehyde precursor solution to evenly penetrate into the template; N2 is introduced, and then a dimethyl sulfoxide solution containing an amine precursor is added, and a two-step gradient temperature increase is performed under a N2 atmosphere, and the total reaction time is 1-5 days; the precipitate is washed by centrifugation with an organic solvent, and the obtained precipitate is dried to obtain a honeycomb COF photocatalyst; (2) Preparation of honeycomb COF composite photocatalyst: The honeycomb COF photocatalyst prepared in step 3 was dispersed in an aqueous solution and ultrasonically treated, and then a metal source was added and stirred at room temperature for 1-3 h. Then, a sulfur source Na2S˙9H2O aqueous solution was added and stirred for 5-10 h. The mixture was allowed to stand for 10-20 h, and washed by centrifugation with deionized water. The mixture was dried in a vacuum oven at 50-100°C to obtain a honeycomb COF-based composite catalyst.

2. The method for preparing a honeycomb COF-based composite catalyst material according to claim 1, characterized in that: In step (1), the three-dimensional ordered polystyrene sphere template is immersed in a dimethyl sulfoxide solution for 10-60 minutes, and the obtained precipitate is dried in a vacuum oven at 50-100°C for 6-18 hours; the molar ratio of the aldehyde precursor to the amine precursor is 1 to 3:1, and the mass ratio of the three-dimensional ordered polystyrene sphere template to the amine precursor is 15-30:

1. The first step of heating under N2 atmosphere is maintained at 30-70°C, the heating rate is 1-5°C / min, and the reaction is carried out for 4-8 hours. The second step of heating is maintained at 80-150°C, the heating rate is 1-5°C / min, and the organic solvent used for centrifugation is at least one of acetone, tetrahydrofuran, methanol, chloroform, N,N-dimethylacetamide, dioxane, and dichloromethane.

3. The method for preparing a honeycomb COF-based composite catalyst material according to claim 2, characterized in that: The molar ratio of the aldehyde precursor to the amine precursor is 1.5:1; the aldehyde precursor is one of the following structures, and its structural formula is as follows: The amine precursor is one of the following structures, and its structural formula is as follows:

4. The method for preparing a honeycomb COF-based composite catalyst material according to claim 1, characterized in that: In step (2), the metal source refers to at least one of Zn(NO3)2 6H2O, Cd(NO3)2 4H2O and InCl3 4H2O, the molar ratio of the metal source to Na2S˙9H2O is 1:1-3, the concentration of the Na2S˙9H2O aqueous solution is 10.4 g / L, and the mass ratio of the added amount of the honeycomb COF to the metal source is 0.1-1:

1.

5. The method for preparing a honeycomb COF-based composite catalyst material according to claim 1, characterized in that: The preparation method of the three-dimensional ordered polystyrene sphere template is as follows: styrene is washed with sodium hydroxide solution and deionized water in sequence; then, the washed styrene is added to a three-necked round-bottom flask containing a polyvinyl pyrrolidone aqueous solution; after bubbling with N2 for 15-30 minutes, it is stirred in an oil bath at 50-100°C for 10-60 minutes under magnetic stirring; subsequently, an aqueous solution containing K2S2O8 is added to the above three-necked flask to initiate a styrene polymerization reaction, and after continuous stirring for 10-30 hours, it is cooled to room temperature, and the obtained milky product is monodisperse colloidal polystyrene spheres; the monodisperse polystyrene spheres are placed in a centrifuge tube for ultrasonic treatment to form a uniform emulsion, and then centrifuged at a speed of 1-3krpm, and the obtained precipitate is dried overnight at 30-60°C, and after natural cooling, the three-dimensional ordered polystyrene sphere template is collected.

6. The method for preparing a honeycomb COF-based composite catalyst material according to claim 5, characterized in that: The concentration of NaOH solution is 10wt.%, the concentration of PVP aqueous solution is 1-10g / L, the concentration of K2S2O8 aqueous solution is 5-30g / L, the volume ratio of the added washed styrene, PVP aqueous solution and K2S2O8 aqueous solution is 1:1~10:0.1~1, the stirring rate in the polymerization step is maintained at 100-500rpm, and stirring is continued for 24h; the ultrasonic treatment time is 10-50min, the ultrasonic machine temperature is maintained below 30°C, and the ultrasonic frequency is maintained at 40-60KHz.

7. Use of the honeycomb COF-based composite catalyst material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: As a catalyst for photocatalytic decomposition of water to produce hydrogen.

Citation Information

Cited By

  • Pressure response type high-conjugation covalent organic framework self-lubricating nanosheet and application thereof

    CN121873602A

  • Pressure-responsive high-conjugated covalent organic framework self-lubricating nanosheet and application thereof

    CN121873602B