Low-temperature sintering preparation process of fine-grain molybdenum alloy

By employing hydrothermal and spark plasma sintering techniques, the problem of uneven second-phase dispersion in molybdenum alloys was solved, enabling low-temperature sintering of fine-grained molybdenum alloys. This improved the uniformity and stability of the material, reduced production costs, and enhanced mechanical properties.

CN119035564APending Publication Date: 2024-11-29HUAIBEI NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127723.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing molybdenum alloy preparation processes, the second phase cannot be uniformly dispersed, resulting in coarse grains, unstable performance, and complex preparation processes with high costs and low material utilization.

Method used

MoO3 and ZrC precursors were prepared by hydrothermal method. Low-temperature sintering was achieved by liquid-liquid doping and spark plasma sintering technology, which ensured uniform dispersion of the second phase, shortened the sintering time, avoided local aggregation, and simplified the preparation process.

Benefits of technology

This study improved the uniformity and stability of fine-grained molybdenum alloys, reduced production costs, increased material utilization and mechanical properties, and shortened the preparation cycle.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a low-temperature sintering preparation process of a fine-grain molybdenum alloy, which comprises the following steps: respectively preparing a MoO3 precursor and a ZrC precursor by adopting a hydrothermal method, mixing and fully stirring two types of turbid liquid subjected to hydrothermal treatment in a liquid-liquid doping manner, and filtering and freeze-drying to obtain a micron-sized MoO3 precursor and a nano-sized ZrC precursor. The molybdenum alloy prepared through the technology can be sintered at the low temperature to obtain fine grains, compared with a traditional high-temperature sintering technology, spark plasma sintering is low in temperature and short in time, energy consumption can be reduced, the economical efficiency and sustainability of preparation can be improved, meanwhile, MoO3 and ZrC precursors can be evenly dispersed in an aqueous solution through liquid-liquid doping, and therefore the performance of the molybdenum alloy is improved. The second phase in the fine-grain molybdenum alloy is uniformly distributed, the consistency and stability of the material performance are further improved, in addition, the prepared molybdenum alloy has the small grain size which is usually in the nanometer level to the micrometer level, and the overall mechanical property of the material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of a fine-grained molybdenum alloy, in particular to a low-temperature sintering preparation process of the fine-grained molybdenum alloy. Background Art

[0002] Molybdenum alloy is a material with excellent mechanical properties and thermal stability. It is widely used in aerospace, engineering machinery, electronic devices and other fields. Traditional molybdenum alloy materials have problems such as coarse grains and unstable mechanical properties, which limit their application in high temperature environments. In order to overcome these problems, researchers have proposed a preparation process for fine-grained molybdenum alloys.

[0003] However, the current preparation process of fine-grained molybdenum alloy has the following disadvantages: in the existing preparation process of molybdenum alloy, the second phase cannot be evenly dispersed in the molybdenum alloy, and the high sintering temperature and long holding time of the molybdenum alloy cause the grains of the molybdenum alloy to be relatively coarse, thereby affecting the consistency and stability of the performance of the molybdenum alloy; in the existing preparation process of molybdenum alloy, the second phase cannot be evenly dispersed in the matrix, and local aggregation is prone to occur, resulting in the uniformity and stability of the prepared molybdenum alloy being affected. In addition, the existing methods for adding the second phase are limited, and generally require powder mixing, drying and ball milling and other processes, which increase some equipment and operating cost investment, increase the waste and loss of raw materials, reduce the utilization rate of materials, and thereby increase production costs; in the existing preparation process of molybdenum alloy, the sintering temperature and cycle of the second phase-reinforced molybdenum alloy block are high, resulting in coarse molybdenum alloy grains and low quality. Summary of the invention

[0004] The purpose of the present invention is to solve the problems in the existing preparation process of molybdenum alloy, that the second phase cannot be evenly dispersed in the molybdenum alloy, the molybdenum alloy has a high sintering temperature and a long holding time, resulting in coarse grains of the molybdenum alloy, thereby affecting the consistency and stability of the performance of the molybdenum alloy; in the existing preparation process of molybdenum alloy, the second phase cannot be evenly dispersed in the matrix, and local aggregation is prone to occur, resulting in the uniformity and stability of the prepared molybdenum alloy being affected. In addition, the existing methods for adding the second phase are limited, and generally powder mixing, drying and ball milling processes are required, which increase the investment in some equipment and operating costs, increase the waste and loss of raw materials, reduce the utilization rate of materials, and thereby increase production costs; in the existing preparation process of molybdenum alloy, the sintering temperature and cycle of the second phase-reinforced molybdenum alloy block are high, resulting in coarse grains and low quality of the molybdenum alloy, and thus a low-temperature sintering preparation process for fine-grained molybdenum alloy is proposed.

[0005] The object of the present invention can be achieved by the following technical scheme: a low-temperature sintering preparation process of a fine-grained molybdenum alloy, wherein a hydrothermal method is used to prepare MoO3 and ZrC precursors respectively, the two suspensions after hydrothermal treatment are mixed and fully stirred by liquid-liquid doping, and micron-grade MoO3 and nano-grade ZrC precursors are obtained by filtration and freeze-drying. The low-temperature sintering preparation process comprises the following steps: Step 1: according to the proportion of the second phase, that is, the mass ratio of zirconium carbide to the alloy in the finished product is 0.1-1.2%, ammonium tetramolybdate is weighed and added to an aqueous solution with a pH value of 1, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction to obtain solution A; zirconium nitrate and starch are weighed and dissolved in 100 ml of deionized water, wherein the amount of zirconium nitrate corresponds to the molar amount of zirconium carbide, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction to obtain solution B; solution A and solution B are mixed, and magnetically stirred for 20 minutes to obtain solution C; Step 2: Filter solution C, freeze the filtrate in a refrigerator, and then put it into a freeze dryer and dry it in a vacuum environment at -50°C for 24 hours. Grind and sieve the powder to obtain precursors of zirconium carbide and molybdenum trioxide; Step 3: calcining the mixed powder obtained in step 2, keeping the mixture warm after calcination, and then cooling the mixture with the furnace to obtain a mixed powder of zirconium carbide precursor and molybdenum trioxide; Step 4: performing two-stage reduction on the mixed powder obtained in step 3 to obtain carbide precursor doped molybdenum powder after reduction; Step 5: The composite powder is subjected to spark plasma sintering and kept warm. After the spark plasma sintering is completed, the sample is cooled along with the furnace to obtain a molybdenum alloy block.

[0006] A further technical improvement of the present invention is that the temperature of the hydrothermal reaction when preparing solution A in step 1 is controlled at 180-230° C. and the time is controlled at 16-24 h.

[0007] A further technical improvement of the present invention is that when preparing solution B in step 1, the temperature of the hydrothermal reaction is controlled at 180-230° C. and the time is controlled at 16-24 h.

[0008] A further technical improvement of the present invention is that the molar ratio of zirconium element to carbon element in zirconium nitrate and starch in step 1 is controlled at 1:5 or 1:6 or 1:7 or 1:8.

[0009] The further technical improvement of the present invention is that the freezing time of the filtrate in step 2 is controlled within 10-15 hours, and the vacuum degree of the vacuum environment of the freeze dryer is ≤5Pa.

[0010] The further technical improvement of the present invention is that: in step 3, the temperature of calcining the mixed powder is controlled at 450-600°C, and the insulation time is controlled at 1-2h.

[0011] The further technical improvement of the present invention is that: in step 4, the first stage reduction temperature is 400-550°C, and the second stage reduction temperature is 900°C-1050°C.

[0012] The further technical improvement of the present invention is that in step five, the sintering temperature is controlled at 1450-1650° C., the heating rate is controlled at 80-120° C. / min, and the sintering pressure is controlled at 45-55 MPa.

[0013] A further technical improvement of the present invention is that the insulation time in step 5 is controlled within 10-15 minutes, and the vacuum degree during insulation is less than 0.05 Pa.

[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) In the present invention, the preparation process adopts a hydrothermal method. The fine-grained molybdenum alloy prepared in this way can be sintered at a relatively low temperature to obtain relatively fine grains. Compared with the traditional high-temperature sintering process, the spark plasma sintering has a low temperature and a short time, which can reduce energy consumption and improve the economy and sustainability of the preparation. At the same time, liquid-liquid doping can make MoO3 and ZrC precursors evenly dispersed in the aqueous solution, which can achieve uniform distribution of fine-grained molybdenum alloy, thereby improving the consistency and stability of the material's performance. In addition, the fine-grained molybdenum alloy prepared by the hydrothermal method has a smaller grain size, usually at the nanometer to micrometer level, which can improve the overall mechanical properties of the material; (2) In the present invention, the preparation process adopts a liquid-liquid doping method to add the second phase material into the matrix material in liquid form. On the one hand, the second phase material is evenly dispersed in the matrix. Since the liquid can flow freely in the matrix, the second phase material can be fully mixed and dispersed during the doping process to avoid local agglomeration, thereby improving the dispersion of the second phase material in the matrix, thereby enhancing the uniformity and stability of the prepared alloy. On the other hand, it is convenient to adjust the operating conditions in the liquid-liquid doping process, such as temperature, concentration, etc., so as to achieve precise control of the amount of the second phase material added, and can flexibly adjust the content and distribution of the second phase material as needed. In addition, compared with other methods for adding the second phase material, the liquid-liquid doping method has a lower preparation cost and does not require powder mixing, drying and ball milling processes, which can save some equipment and operating costs. At the same time, it can reduce the waste and loss of the second phase material, improve material utilization, and reduce production costs. (3) In the present invention, the preparation process obtains a second phase reinforced molybdenum alloy block by spark plasma sintering of a carbide precursor doped with molybdenum powder. By using spark plasma sintering technology, on the one hand, high-speed sealed sintering can be achieved at a lower temperature, the sintering speed can be increased, and the sintering cycle can be shortened, thereby improving the efficiency of the process for preparing fine-grained molybdenum alloys. On the other hand, rapid heating and cooling can be achieved, and heat can be transferred through high-temperature plasma to make the temperature inside the sample uniform, resulting in a uniform grain distribution, making the grain size of the molybdenum alloy after sintering smaller, so as to achieve the purpose of fine grains, thereby improving the quality of the prepared fine-grained molybdenum alloy. DETAILED DESCRIPTION

[0015] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1

[0016] A low temperature sintering preparation process for a fine-grained molybdenum alloy, the low temperature sintering preparation process comprising the following steps: Step 1: According to the proportion of the second phase, that is, the mass ratio of zirconium carbide to the alloy in the finished product is 0.5%, ammonium tetramolybdate is weighed and added to an aqueous solution with a pH value of 1, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction, the hydrothermal reaction temperature is 200°C, and the time is 18 hours to obtain solution A; zirconium nitrate and starch are weighed and dissolved in 100 ml of deionized water, wherein the amount of zirconium nitrate corresponds to the molar amount of zirconium carbide, the molar ratio of zirconium element to carbon element is 1:6, magnetically stirred for 30 minutes, placed in a hydrothermal reactor for hydrothermal reaction, the hydrothermal reaction temperature is 200°C, and the time is 18 hours to obtain solution B; solution A and solution B are mixed, and magnetically stirred for 20 minutes to obtain solution C; Step 2: Filter solution C, freeze the filtrate in a refrigerator for 12 hours, put it in a freeze dryer, dry it at -50°C and a vacuum degree of 4 Pa ​​for 24 hours, grind and sieve the powder to obtain precursors of zirconium carbide and molybdenum trioxide; Step 3: calcining the mixed powder obtained in step 2 at a temperature of 500° C. for 1.5 hours, and then cooling with the furnace to obtain a mixed powder of zirconium carbide precursor and molybdenum trioxide; Step 4: subjecting the mixed powder obtained in step 3 to two-stage reduction, wherein the first stage reduction temperature is 450° C. and the second stage reduction temperature is 1000° C., to obtain carbide precursor doped molybdenum powder after reduction; Step 5: The composite powder is subjected to spark plasma sintering at a sintering temperature of 1400°C, a sintering heating rate of 90°C / min, a sintering pressure of 50Mpa, and is kept warm for 12 minutes. The vacuum degree is 0.03Pa. After the spark plasma sintering is completed, the sample is cooled with the furnace to obtain a molybdenum alloy block. Embodiment 2

[0017] A low temperature sintering preparation process for a fine-grained molybdenum alloy, the low temperature sintering preparation process comprising the following steps: Step 1: According to the proportion of the second phase, that is, the mass ratio of zirconium carbide to the alloy in the finished product is 1%, ammonium tetramolybdate is weighed and added to an aqueous solution with a pH value of 1, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction at a temperature of 220°C for 20 hours to obtain solution A; zirconium nitrate and starch are weighed and dissolved in 100 ml of deionized water, wherein the amount of zirconium nitrate corresponds to the molar amount of zirconium carbide, and the molar ratio of zirconium element to carbon element is 1:8, magnetically stirred for 30 minutes, placed in a hydrothermal reactor for hydrothermal reaction at a temperature of 220°C for 20 hours to obtain solution B; solution A and solution B are mixed, and magnetically stirred for 20 minutes to obtain solution C; Step 2: Filter solution C, freeze the filtrate in a refrigerator for 14 hours, put it in a freeze dryer, dry it at -50°C and a vacuum degree of 3.5 Pa for 24 hours, grind and sieve the powder to obtain precursors of zirconium carbide and molybdenum trioxide; Step 3: calcining the mixed powder obtained in step 2 at a temperature of 550° C. for 1.5 hours, and then cooling the mixture with the furnace to obtain a mixed powder of zirconium carbide precursor and molybdenum trioxide; Step 4: subjecting the mixed powder obtained in step 3 to two-stage reduction, wherein the first stage reduction temperature is 500° C. and the second stage reduction temperature is 950° C., to obtain carbide precursor doped molybdenum powder after reduction; Step 5: The composite powder is subjected to spark plasma sintering at a sintering temperature of 1500°C, a sintering heating rate of 100°C / min, a sintering pressure of 50Mpa, and is kept warm for 14 minutes. The vacuum degree is 0.02Pa. After the spark plasma sintering is completed, the sample is cooled with the furnace to obtain a molybdenum alloy block.

[0018] Working principle: This preparation process prepares MoO3 and ZrC precursors respectively by hydrothermal method, mixes the two suspensions after hydrothermal treatment by liquid-liquid doping and fully stirs them, and obtains micron-sized MoO3 and nano-sized ZrC precursors by filtration and freeze-drying.

[0019] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A low-temperature sintering preparation process for fine-grained molybdenum alloy, wherein MoO3 and ZrC precursors are prepared by hydrothermal method, the two suspensions after hydrothermal treatment are mixed and stirred by liquid-liquid doping, and micron-grade MoO3 and nano-grade ZrC precursors are obtained by filtration and freeze drying, wherein: The low temperature sintering preparation process comprises the following steps: Step 1: according to the proportion of the second phase, that is, the mass ratio of zirconium carbide to the alloy in the finished product is 0.1-1.2%, ammonium tetramolybdate is weighed and added to an aqueous solution with a pH value of 1, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction to obtain solution A; zirconium nitrate and starch are weighed and dissolved in 100 ml of deionized water, wherein the amount of zirconium nitrate corresponds to the molar amount of zirconium carbide, magnetically stirred for 30 minutes, and placed in a hydrothermal reactor for hydrothermal reaction to obtain solution B; solution A and solution B are mixed, and magnetically stirred for 20 minutes to obtain solution C; Step 2: Filter solution C, freeze the filtrate in a refrigerator, and then put it into a freeze dryer and dry it in a vacuum environment at -50°C for 24 hours. Grind and sieve the powder to obtain precursors of zirconium carbide and molybdenum trioxide; Step 3: calcining the mixed powder obtained in step 2, keeping the mixture warm after calcination, and then cooling the mixture with the furnace to obtain a mixed powder of zirconium carbide precursor and molybdenum trioxide; Step 4: performing two-stage reduction on the mixed powder obtained in step 3 to obtain carbide precursor doped molybdenum powder after reduction; Step 5: The composite powder is subjected to spark plasma sintering and kept warm. After the spark plasma sintering is completed, the sample is cooled along with the furnace to obtain a molybdenum alloy block.

2. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: When preparing solution A in step 1, the temperature of the hydrothermal reaction is controlled at 180-230° C. and the time is controlled at 16-24 h.

3. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: When preparing solution B in step 1, the temperature of the hydrothermal reaction is controlled at 180-230° C. and the time is controlled at 16-24 h.

4. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: In step 1, the molar ratio of zirconium element to carbon element in zirconium nitrate and starch is controlled at 1:5 or 1:6 or 1:7 or 1:

8.

5. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: In step 2, the freezing time of the filtrate is controlled at 10-15 hours, and the vacuum degree of the vacuum environment of the freeze dryer is ≤5Pa.

6. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: In step 3, the calcination temperature of the mixed powder is controlled at 450-600°C, and the insulation time is controlled at 1-2h.

7. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: In step 4, the first stage reduction temperature is 400-550°C, and the second stage reduction temperature is 900°C-1050°C.

8. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 7, characterized in that: In step 5, the sintering temperature is controlled at 1450-1650° C., the heating rate is controlled at 80-120° C. / min, and the sintering pressure is controlled at 45-55 MPa.

9. The low temperature sintering process for preparing a fine-grained molybdenum alloy according to claim 1, characterized in that: In step 5, the insulation time is controlled at 10-15 minutes, and the vacuum degree during insulation is less than 0.05Pa.