Preparation method of face-centered cubic solid solution layer welding spot containing multi-principal element alloy

By adding nickel and silver elements to the copper substrate and adopting a specific welding process, the face-centered cubic solid solution layer solder joints of multi-main alloys is solved, and the problem of insufficient shear strength of existing gold and tin solder joints is realized, and high-strength solder joints is achieved The preparation of points is suitable for electronic packaging field.

CN119035870AActive Publication Date: 2024-11-29CENT SOUTH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411244195.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing gold-tin solder joints have low shear strength and are difficult to meet industrial needs, which limits their application in the field of electronic packaging.

Method used

By adding nickel and silver elements to the copper substrate and adopting a specific welding process, a multi-main alloy face-centered cubic solid solution layer solder joint is formed to improve the shear strength of the solder joint.

Benefits of technology

This method significantly improves the shear strength of the solder joints to reach 105-107MPa, and has a simple process and low cost, which improves the reliability of the solder joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035870A_ABST
    Figure CN119035870A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a welding spot containing a multi-principal element alloy face-centered cubic solid solution layer. The preparation method comprises the following steps: preparing 58-85% of Cu, 7-20% of Ag and 8-22% of Ni, then sequentially smelting, rolling and cutting to obtain a CuNiAg alloy plate, putting one end of the alloy plate into AuSn20 solder, overlapping another alloy plate on the alloy plate, binding and fixing by using a polytetrafluoroethylene adhesive tape, putting the fixed sample into a hydrogen furnace for brazing for 5 minutes, and then brazing in a muffle furnace for 15 minutes, so as to reduce holes generated during brazing, thereby obtaining the CuNiAg alloy plate. And a balancing weight is placed above a welding spot during brazing in the muffle furnace. According to the method, the thickness of a welding seam can be uniform, holes are few, a multi-principal-element alloy face-centered cubic solid solution layer can be generated near the substrate to relieve stress concentration, and then the strength of a welding spot is improved. The method is simple in process, low in cost and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic welding manufacturing, and relates to a method for preparing a face-centered cubic solid solution layer solder joint containing a multi-principal alloy. Background Art

[0002] With the rapid development of the electronics industry, electronic products are gradually tending towards digitalization and integration, so the performance requirements for electronic components are gradually increasing. As a key link in electronic manufacturing, electronic packaging has a significant impact on the reliability and service life of electronic components. Welding is an important technology for electronic packaging and is widely used in the electronics manufacturing industry, such as microelectronic ceramic cover packaging, insulator welding between metal and ceramic cover, chip mounting, and welding of high-power laser semiconductor chips. Among them, gold-tin eutectic alloy solder has excellent welding performance and is widely used. Especially in recent years, with the introduction of relevant environmental protection policies, the use of traditional lead-based solder has been decreasing, and the demand for gold-tin solder has increased rapidly. Gold-tin eutectic alloy is currently the best solder that can replace high-melting-point lead-based alloys with a melting point of 280℃ to 360℃. Although its application range is greatly limited from the perspective of price and melting point, it is widely used in the electronics manufacturing industry because of its excellent creep and fatigue resistance, good electrical and thermal conductivity, and easy welding and brazing without flux.

[0003] During the gold-tin solder welding process, the liquid gold-tin solder reacts with the substrate and forms intermetallic compounds at the solder / substrate interface. However, due to the hard and brittle characteristics of intermetallic compounds and the stress concentration of intermetallic compounds close to the substrate, cracks are easily generated and extended in the intermetallic compound layer under load. Therefore, a large number of researchers at home and abroad have used a series of methods to improve the strength of solder joints. The existing methods mainly focus on optimizing solder composition, improving welding technology, and improving welding equipment. Solder optimization mainly involves adding alloy elements to the solder. Alloy elements can inhibit the formation and growth of certain intermetallic compounds, thereby reducing the damage of intermetallic compounds to solder joints. The welding process involves changing the welding time and temperature or introducing an external field. These methods can reduce the generation of intermetallic compounds to a certain extent, thereby improving the strength of solder joints.

[0004] However, despite a series of methods to optimize the composition, morphology and distribution of intermetallic compounds, the welded joints still show relatively low shear strength. The reason is that no matter how the process is optimized, the hard and brittle nature of the intermetallic compounds produced at the welding interface will not change. Therefore, the strength of the solder joints prepared by gold-tin solder is difficult to significantly improve and meet industrial needs, which seriously restricts the application of gold-tin solder in the field of electronic packaging.

[0005] The existing method for preparing solder joints containing multi-principal alloy face-centered cubic solid solution layers is to prepare a substrate by preparing copper, nickel, and silver metals with equal atomic ratios through arc melting and rolling, and then weld them together using gold-tin solder at a welding temperature of 350°C. The shear strength of the solder joint can reach 81MPa. In addition, when a substrate with a copper-nickel atomic ratio of 4:1 prepared by arc melting is used and AuSn29 is used for welding, a solder joint with a multi-principal alloy face-centered cubic solid solution layer can also be obtained, and the shear strength of the solder joint is about 93MPa. Summary of the invention

[0006] On the basis of the prior art, the present invention further optimizes the components of the substrate and cooperates with the welding process to explore a product with higher solder joint shear strength.

[0007] The present invention adds a certain amount of nickel, silver and other elements into the copper substrate, and after a period of welding, the obtained solder joint contains a multi-principal alloy face-centered cubic solid solution layer, and its shear strength is improved. The method has simple process and low cost, and can improve the reliability of the solder joint.

[0008] The present invention provides a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer, comprising the following steps:

[0009] Step 1 Ingredients

[0010] According to the atomic ratio; Cu: 58-85%, Ag: 7-20%, Ni: 8-22%, preferably Cu: 80-82%, Ag: 10-12%, Ni: 8-9%, more preferably Cu: 81%, Ag: 11%, Ni: 8%, Cu, Ni, Ag;

[0011] Step 2: Melting

[0012] Put the prepared metal materials into a smelting furnace for smelting to obtain ingots;

[0013] Step 3: Extrusion

[0014] The ingot is extruded, with a single deformation of 10-15%, into a plate with a thickness of 1 to 1.5 mm; Step 4 Cutting

[0015] Cutting the plate obtained in step 3 to obtain metal strips of set size;

[0016] Step 5: Pre-treatment before welding

[0017] Grinding, polishing and cleaning to obtain a metal strip with a clean surface and no impurities; placing AuSn20 solder of a set size on one side of the metal strip, and then overlapping another metal strip on it, binding and fixing them to obtain a sample to be welded;

[0018] Step 6: Soldering

[0019] The sample to be welded obtained in step 5 is placed in a hydrogen furnace for welding, the welding temperature is 350-360°C, and the welding time is 5-8min; then the sample welded in the hydrogen furnace is placed in a muffle furnace for welding for 15-20min, and the temperature of the muffle furnace is 330-350°C.

[0020] As a preferred embodiment, the present invention provides a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer, wherein the melting furnace is an arc melting furnace.

[0021] The present invention provides a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer.

[0022] Put the prepared metal material into a quartz tube, pass argon into the quartz tube, and then evacuate it to a vacuum, repeat at least 3 times to expel the air, and then seal the quartz tube containing the metal material; after sealing, the quartz tube contains argon;

[0023] Turn on the induction heating power supply, ensure that the cooling system operates normally, modulate the current to 180A, then put the quartz tube containing the sample into the center of the induction coil, and increase the current to 240A after the metal sample is burned red, and the metal sample can be melted; after smelting for 3 minutes, bury the sample end of the quartz tube in the sand to cool naturally, and take out the sample after cooling; obtain the ingot. Of course, its smelting process can also be used in the present invention, but different smelting processes have a certain effect on the strength of the final weld. For example, put the prepared metal material into an arc melting furnace, first turn on the mechanical pump to extract the vacuum, and then introduce argon gas. After repeating the operation at least 2 times, start the arc, and after starting the arc, turn the current to 300A and smelt for 15 seconds. To ensure uniform smelting, use a robotic arm to turn the sample over and repeat the operation 5 times. After smelting, cool it in the furnace to obtain a button ingot. During the specific operation of arc melting, evacuate the furnace until the pressure in the furnace drops to less than or equal to 10000Pa, then open the argon valve and inject argon until the pressure in the furnace is slightly negative (the reading on the meter is -0.02-0, unit MPa)

[0024] The present invention discloses a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer. In step 4, the plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0025] The present invention provides a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer. In step 5, the metal strip is polished with 800#, 1200#, 1500# and 2000# sandpaper to remove the surface oxide film, and after the polishing is completed, the metal strip is polished and ultrasonically cleaned to obtain a metal strip with a clean surface and no impurities. Preferably, the surface roughness of the metal strip with a clean surface and no impurities is Ra=0.7-0.9μm.

[0026] The present invention provides a method for preparing a weld containing a multi-principal alloy face-centered cubic solid solution layer. In step 5, a polytetrafluoroethylene tape is used to bind and fix the welded sample to obtain a welded sample. This ensures that the weld size is uniform, the holes are few, and the weld is not prone to dislocation.

[0027] The present invention discloses a method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer. When welding is performed in step 6, a metal block is applied above the solder joint to reduce holes. When the size of the metal strip is 33 mm×5 mm and the size of the AuSn20 solder is 3 mm×5 mm, the mass of the applied metal block is 70-80 g. When applied in industry, the mass of the applied metal block can be adjusted according to actual conditions.

[0028] When welding in a hydrogen furnace, a certain amount of hydrogen is introduced to ensure that the substrate and solder are not oxidized during the welding process, thereby ensuring that the liquid solder has high fluidity, can wet the substrate well, and ensure the welding quality. When welding in a muffle furnace later, a counterweight block of the same temperature can be added to reduce holes without affecting the interface product.

[0029] The process designed by the present invention is suitable for preparing high-strength solder joints. The strength of the solder joints prepared is higher than that of similar technologies and the cost is lower.

[0030] The present invention adds a certain amount of alloy elements such as Ni and Ag to the substrate to obtain a solder joint having a face-centered cubic solid solution layer containing a multi-principal alloy, and the shear strength of the solder joint is improved. The advantages of the present invention are:

[0031] 1. The composition of the cast substrate is uniform and there is no segregation.

[0032] 2. The weld thickness is uniform and there are few holes, which reduces the impact of holes on joint strength.

[0033] 3. The obtained solder joint has a multi-principal alloy face-centered cubic solid solution layer near the substrate. The solid solution layer can relieve stress concentration through plastic deformation, thereby improving the strength of the solder joint. After optimization, the shear strength of the obtained solder joint can reach 105-107MPa.

[0034] 4. The process is simple and the obtained product has excellent performance; the production process of the present invention is simple and does not require complex welding equipment. At the same time, the performance of the product obtained by the present invention is better than that of the product obtained by the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a schematic diagram of a process flow of a face-centered cubic solid solution layer containing multiple principal element alloys.

[0036] Figure 2 This is the macroscopic morphology of the plate obtained after ingot extrusion in Example 1.

[0037] Figure 3 This is a SEM image of the substrate obtained in Example 1.

[0038] Figure 4 This is the macroscopic morphology of the welding sample obtained in Example 1.

[0039] Figure 5 This is the EBSD test result of the solder joint in Example 1.

[0040] Figure 6 This is the SEM test result of the solder joint in Example 1.

[0041] Figure 7 This is the XRD test result of the solder joint in Example 1.

[0042] Figure 8 The tensile test results of the welding samples in Example 1 are shown in FIG.

[0043] Fig. 9 This is the SEM test result of the solder joint in Example 2.

[0044] Fig.10 The following are the test results of the tensile test of the welding sample in Example 2.

[0045] Fig.11 This is the SEM test result of the solder joint in Example 3.

[0046] Fig.12 The following are the test results of the tensile test of the welding sample in Example 3. DETAILED DESCRIPTION

[0047] Example 1

[0048] 1) Using an electronic balance, prepare the metal raw materials of Cu, Ni and Ag according to the atomic ratio: Cu: 81%, Ag: 11%, Ni: 8%;

[0049] 2) Melting and Casting: Place the prepared metal material into a quartz tube and perform a gas washing operation first: introduce argon into the quartz tube, then evacuate it to a vacuum, repeat three times to expel the air, and after the last gas washing is completed, introduce a certain amount of argon into the quartz tube and close the argon valve, and use a mixture of propane and oxygen to seal the quartz tube with a certain amount of argon. Turn on the induction heating power supply, ensure the normal operation of the cooling system, modulate the current to 180A, and then place the quartz tube containing the sample in the center of the induction coil. After the metal sample is burned to red, increase the current to 240A, and the metal sample can be melted. After 3 minutes of smelting, bury the sample end of the quartz tube in the sand to cool naturally, and take out the sample after cooling.

[0050] 3) Extrusion The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of about 1.25 mm.

[0051] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0052] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities, and the surface roughness is Ra = 0.8μm. Place AuSn20 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0053] 6) Welding The sample to be welded obtained in step 5 is placed in a hydrogen furnace for welding at a welding temperature of 350°C and a welding time of 5 minutes. The sample welded in the hydrogen furnace is then placed in a muffle furnace for welding for 15 minutes at a temperature of 350°C. During welding, a 75g metal block is applied above the weld point to reduce holes.

[0054] 7) Product performance. The obtained solder joints have few holes, uniform weld size, and contain a face-centered cubic solid solution layer composed of four alloy elements, Au, Sn, Cu, and Ag, near the substrate. The solder joint shear strength is high, up to 106.6MPa.

[0055] Example 2

[0056] 1) Using an electronic balance, prepare the metal raw materials of Cu, Ni and Ag according to the atomic ratio: Cu: 71%, Ag: 7%, Ni: 22%;

[0057] 2) Melting and Casting: Put the prepared metal materials into the arc melting furnace, first start the mechanical pump to draw vacuum, then introduce argon, repeat the operation 3 times, turn on the molecular pump, draw vacuum until the furnace pressure drops to less than or equal to 10000Pa, then open the argon valve and flush argon until the pressure in the furnace is slightly negative (the reading on the meter is -0.02-0, unit MPa); start the arc, after starting the arc, turn the current to 300A, melt for 15 seconds, and use a mechanical arm to turn the sample over and repeat the operation 5 times to ensure uniform melting. After the melting is completed, cool it with the furnace to obtain a button ingot.

[0058] 3) Extrusion The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of 1.25 mm.

[0059] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0060] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities, and the surface roughness is Ra = 0.8μm. Place AuSn20 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0061] 6) Welding The sample to be welded obtained in step 5 is placed in a hydrogen furnace for welding at a welding temperature of 350°C and a welding time of 5 minutes. The sample welded in the hydrogen furnace is then placed in a muffle furnace for welding for 15 minutes at a temperature of 350°C. During welding, a 75g metal block is applied above the weld point to reduce holes.

[0062] 7) The obtained welds have few holes, uniform weld size, and high shear strength of about 76MPa.

[0063] Example 3

[0064] 1) Using an electronic balance, prepare the metal raw materials of Cu, Ni and Ag according to the atomic ratio: Cu: 61%, Ag: 20%, Ni: 19%;

[0065] 2) Melting and Casting: Put the prepared metal materials into the arc melting furnace, first start the mechanical pump to draw vacuum, then introduce argon, repeat the operation 3 times, turn on the molecular pump, draw vacuum until the furnace pressure drops to less than or equal to 10000Pa, then open the argon valve and flush argon until the pressure in the furnace is slightly negative (the reading on the meter is -0.02-0, unit MPa); start the arc, after starting the arc, turn the current to 300A, melt for 15 seconds, and use a mechanical arm to turn the sample over and repeat the operation 5 times to ensure uniform melting. After the melting is completed, cool it with the furnace to obtain a button ingot.

[0066] 3) Extrusion The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of 1.25 mm.

[0067] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0068] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities, and the surface roughness is Ra = 0.8μm. Place AuSn20 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0069] 6) Welding The sample to be welded obtained in step 5 is placed in a hydrogen furnace for welding at a welding temperature of 350°C and a welding time of 5 minutes. The sample welded in the hydrogen furnace is then placed in a muffle furnace for welding for 15 minutes at a temperature of 350°C. During welding, a 75g metal block is applied above the weld point to reduce holes.

[0070] 7) Product performance: The welds obtained have few holes, uniform weld size, high strength, and a shear strength of approximately 89MPa.

[0071] Comparative Example 1

[0072] 1) Use an electronic balance to prepare Cu, Ni and Ag according to the atomic ratio of Cu:Ni:Ag=1:1:1;

[0073] 2) Melting and Casting: Place the prepared metal materials into the arc melting furnace, first turn on the mechanical pump to draw vacuum, then introduce argon gas, repeat the operation 3 times, then turn on the molecular pump to draw the furnace to a vacuum degree of 10 -5 , and then open the argon valve to -0.02. After the arc is started, the current is turned to 300A and the melting is performed for 15 seconds. To ensure uniform melting, the sample is turned over by a robot arm and the operation is repeated 5 times. After the melting is completed, the sample is cooled in the furnace to obtain a button ingot.

[0074] 3) Extrusion The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of 1.25 mm.

[0075] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0076] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities. Place AuSn20 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0077] 6) Welding: The sample to be welded obtained in step 5 is placed in an argon furnace for welding at a welding temperature of 350° C. and a welding time of 20 min.

[0078] 7) Product performance. The obtained solder joints have few holes, uniform weld size, and contain a face-centered cubic solid solution layer composed of five alloy elements, Au, Sn, Cu, Ni, and Ag, near the substrate, but the shear strength of the solder joint is 81MPa.

[0079] Comparative Example 2

[0080] Preparation of face-centered cubic solid solution layer solder joints containing four alloy elements Au, Sn, Cu and Ni

[0081] 1) Use an electronic balance to mix Cu and Ni according to the atomic ratio of Cu:Ni=4:1;

[0082] 2) Melting and Casting: Place the prepared metal materials into the arc melting furnace, first turn on the mechanical pump to draw vacuum, then introduce argon gas, repeat the operation 3 times, then turn on the molecular pump to draw the furnace to a vacuum degree of 10 -5 , and then open the argon valve to -0.02. After the arc is started, the current is turned to 300A and the melting is performed for 15 seconds. To ensure uniform melting, the sample is turned over by a robot arm and the operation is repeated 5 times. After the melting is completed, the sample is cooled in the furnace to obtain a button ingot.

[0083] 3) Extrusion: The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of 1 to 1.5 mm.

[0084] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0085] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities. Place AuSn29 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0086] 6) Welding: The sample to be welded obtained in step 5 is placed in an argon furnace for welding at a temperature of 350° C. and a welding time of 20 min. During welding, a 75 g metal block is applied above the welding point to reduce holes.

[0087] 7) Product performance. The obtained solder joints have few holes, uniform weld size, and contain a face-centered cubic solid solution layer composed of four alloy elements: Au, Sn, Cu, and Ni near the substrate. The solder joint strength is 93MPa.

[0088] Comparative Example 3

[0089] 1) Use an electronic balance to prepare Cu and Ni according to the atomic ratio of Cu:Ni=2:3;

[0090] 2) Melting and Casting: Place the prepared metal material into a quartz tube and perform a gas washing operation first: introduce argon into the quartz tube, then evacuate it to a vacuum, repeat three times to expel the air, and after the last gas washing is completed, introduce a certain amount of argon into the quartz tube and close the argon valve, and use a mixture of propane and oxygen to seal the quartz tube with a certain amount of argon. Turn on the induction heating power supply, ensure the normal operation of the cooling system, modulate the current to 180A, and then place the quartz tube containing the sample in the center of the induction coil. After the metal sample is burned to red, increase the current to 240A, and the metal sample can be melted. After 3 minutes of smelting, bury the sample end of the quartz tube in the sand to cool naturally, and take out the sample after cooling.

[0091] 3) Extrusion: The smelted button ingot is extruded, with a single deformation of about 15%, and is extruded into a plate with a thickness of 1 to 1.5 mm.

[0092] 4) Cutting The plate obtained in step 3 is cut into metal strips of 33 mm×5 mm.

[0093] 5) Pre-welding treatment: Use 800#, 1200#, 1500# and 2000# sandpaper to grind the metal strip obtained in step 4 to remove the surface oxide film, polish it after grinding, and ultrasonically clean it to obtain a metal strip with a clean surface and no impurities. Place AuSn29 solder with a size of 3mm×5mm on one side of the metal strip, and then overlap another metal strip on it, and use polytetrafluoroethylene tape to bind and fix it to obtain a sample to be welded.

[0094] 6) Welding: The sample to be welded obtained in step 5 is placed in an argon furnace for welding at a welding temperature of 350° C. and a welding time of 10 min.

[0095] 7) Product performance. The obtained solder joints have few holes, uniform weld size, and contain a face-centered cubic solid solution layer composed of four alloy elements: Au, Sn, Cu, and Ni near the substrate. The solder joint strength is 62MPa.

[0096] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer, characterized in that: The steps include: Step 1 Ingredients According to the atomic ratio: Cu: 58-85%, Ag: 7-20%, Ni: 8-22%, Cu, Ni, Ag are matched; Step 2: Melting Put the prepared metal materials into a smelting furnace for smelting to obtain ingots; Step 3: Extrusion The ingot is extruded, with a single deformation of 10-15%, into a plate with a thickness of 1-1.5 mm; Step 4: Cutting Cutting the plate obtained in step 3 to obtain metal strips of set size; Step 5: Pre-treatment before welding Grinding, polishing and cleaning to obtain a metal strip with a clean surface and no impurities; placing AuSn20 solder of a set size on one side of the metal strip, and then overlapping another metal strip on it, binding and fixing them to obtain a sample to be welded; Step 6: Soldering The sample to be welded obtained in step 5 is placed in a hydrogen furnace for welding, the welding temperature is 350-360°C, and the welding time is 5-8min; then the sample welded in the hydrogen furnace is placed in a muffle furnace for welding for 15-20min, and the temperature of the muffle furnace is 330-350°C.

2. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: In step one, Cu, Ni and Ag are matched according to the atomic ratio: Cu: 80-82%, Ag: 10-12%, Ni: 8-9%.

3. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 2, characterized in that: In step 1, Cu, Ni and Ag are prepared according to the atomic ratio of Cu: 81%, Ag: 11% and Ni: 8%.

4. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: Put the prepared metal material into a quartz tube, pass argon into the quartz tube, and then evacuate it, repeat at least 3 times to expel the air, and then seal the quartz tube containing the metal material; after sealing, the quartz tube contains argon; turn on the induction heating power supply to ensure the normal operation of the cooling system, modulate the current to 180A, and then put the quartz tube containing the sample into the center of the induction coil, and increase the current to 240A after the metal sample is burned to red, and the metal sample can be melted; after smelting for 3 minutes, bury the sample end of the quartz tube in the sand to cool naturally, and take out the sample after cooling is completed; obtain an ingot.

5. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: Put the prepared metal materials into the arc melting furnace, first turn on the mechanical pump to draw vacuum, then introduce argon, repeat the operation at least 2 times, start the arc, turn the current to 300A after arc starting, and melt for 15 seconds. To ensure uniform melting, use a mechanical arm to turn the sample over and repeat the operation 5 times; after melting, cool with the furnace to obtain button ingots; when vacuuming, evacuate until the furnace pressure drops to less than or equal to 1000Pa, and when filling with argon, fill it until the pressure in the furnace is slightly negative, at which time the reading on the meter is -0.02-0, unit MPa.

6. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: In step 5, the surface roughness of the clean metal strip without impurities is Ra=0.7-0.9 μm.

7. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: In step five, the metal strip is sanded with 800#, 1200#, 1500# and 2000# sandpaper to remove the surface oxide film, and then polished and ultrasonically cleaned to obtain a metal strip with a clean surface and no impurities.

8. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: In step 5, the sample to be welded is bound and fixed with polytetrafluoroethylene tape, which can ensure that the weld size is uniform, there are few holes, and it is not easy to move during welding.

9. The method for preparing a solder joint containing a multi-principal alloy face-centered cubic solid solution layer according to claim 1, characterized in that: During soldering in step six, a metal block is applied above the solder joint to reduce voids. When the size of the metal strip is 33 mm×5 mm and the size of the AuSn20 solder is 3 mm×5 mm, the mass of the applied metal block is 70-80 g.

Citation Information

Patent Citations

  • Preparing method of AuSn20 brazing filler metal for improving braze performance

    CN107234371A

  • Solder joint of Cu-Ni alloyed substrate and lead-free solder and preparation method thereof

    CN109175573A

  • Substrate for use in joining element

    CN1509499A

  • Au-Sn ALLOY SOLDER

    JP2012200788A