A heat treatment method for preparing high entropy alloy with non-uniform composition and prepared high entropy alloy
Through multi-step heat treatment methods, including solid solution, cold rolling, recrystallization and insulation, the composition inhomogeneity of Ni2CoCrFeTi0.2Al0.1 high-entropy alloy is adjusted, and the problem of unclear impact of heat treatment on alloy performance in the prior art is solved, and the problem of uncertain impact of heat treatment on alloy performance is realized. The diversified mechanical properties are used to fill the gap in heat treatment methods for high-entropy alloys.
Patent Information
- Application Number
- CN202310244503.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-14
AI Technical Summary
At present, the impact of different methods of heat treatment on the alloy performance and microstructure of Ni2CoCrFeTi0.2Al0.1 high-entropy alloys is unclear, especially the experiments related to the annealing of the sample after recrystallization, which leads to the inability to effectively regulate the compositional inhomogeneity and performance of the alloy.
Multi-step heat treatment methods, including solid solution, cold rolling, recrystallization and insulation operations, and experiments are carried out through a high vacuum quenching furnace to eliminate casting defects of the alloy, adjust the composition uniformity and grain structure of the sample, and produce two precipitation phases. , high-entropy alloys that achieve component inhomogeneity.
This method can significantly regulate the compositional inhomogeneity of high-entropy alloys, achieve diversified mechanical properties, fill the gap in heat treatment methods of high-entropy alloys, provide a connection between alloy microstructure and heat treatment methods, and improve the performance of the alloy Performance.
Smart Images

Figure CN116162875B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material preparation, and in particular relates to a heat treatment method for preparing a high entropy alloy with inhomogeneous composition, and also relates to the high entropy alloy prepared by the heat treatment method. Background Art
[0002] CoCrNi-based high entropy alloy is a fcc single-phase solid solution alloy formed by a mixture of multiple elements. Studies have found that due to its unique design concept, its fracture resistance, tensile strength, high temperature resistance, wear resistance and corrosion resistance are better than many traditional alloys. In addition, this alloy is expected to break through the shackles of traditional metal structural materials that are difficult to balance strength and plasticity. At present, there have been many studies on CoCrNi-based high entropy alloys, among which Ni2CoCrFeTi0.2Al0.1 high entropy alloy has attracted widespread attention due to its excellent mechanical properties. Studies have shown that the internal dislocation movement mode of Ni2CoCrFeTi0.2Al0.1 high entropy alloy changes after recrystallization, which may be related to local order. However, the effects of different heat treatment methods on the properties and microstructure of Ni2CoCrFeTi0.2Al0.1 high entropy alloy are still unclear, and there is a lack of experiments on sample annealing after recrystallization. Therefore, it is of great significance to study the effect of sample annealing after recrystallization on the microstructure and properties of high entropy alloys and to design a heat treatment method for preparing Ni2CoCrFeTi0.2Al0.1 high entropy alloys with heterogeneous composition. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a heat treatment method for preparing a Ni2CoCrFeTi0.2Al0.1 high entropy alloy with inhomogeneous composition. The method uses a multi-step heat treatment method to perform solid solution, cold rolling, recrystallization, heat preservation and other experimental operations on the alloy to make the alloy spinodal decomposition and obtain two precipitated phases at the same time, filling the current gap in the heat treatment methods for high entropy alloys and increasing the degree of connection between the heat treatment methods and the alloy microstructure.
[0004] The present invention provides a heat treatment method for preparing a high entropy alloy with heterogeneous composition through the following technical scheme, which comprises the following steps:
[0005] 1) Take Ni2CoCrFeTi0.2Al0.1 high entropy alloy, cut it into block samples, place it in a high vacuum quenching furnace for solid solution, and then quench it with water to room temperature;
[0006] (2) cold rolling the quenched block sample until the thickness is reduced by 70%;
[0007] (3) The cold-rolled sample is placed in a high vacuum quenching furnace for heating and recrystallization, and then water quenched to room temperature;
[0008] (4) Place the product in a high vacuum quenching furnace and heat it again, then quench it with water to room temperature.
[0009] Furthermore, in step (1), the solution temperature of the Ni2CoCrFeTi0.2Al0.1 high entropy alloy is 1200°C and the solution time is 2 hours.
[0010] The solid solution technology can eliminate the casting defects of high entropy alloys and make the internal composition of the sample homogenous.
[0011] Furthermore, in step (2), the number of cold rolling times is 20 times or more.
[0012] Furthermore, in step (3), the recrystallization temperature is 1200° C. and the time is 10 min.
[0013] Furthermore, in step (4), the sample is kept at a temperature of 800° C. for a time of 3-168 h.
[0014] Furthermore, in step (4), the insulation time is 168 hours.
[0015] By using the high entropy alloy Ni2CoCrFeTi0.2Al0.1 to hold the alloy in a heat-insulated state after recrystallization, it is possible to achieve significant fluctuations in composition. Different holding times can produce high entropy alloys with different compositional inhomogeneities.
[0016] Furthermore, the vacuum degree of the high vacuum quenching furnace is 10E-4Pa.
[0017] At the same time, the present invention also provides a high entropy alloy obtained by treating the above-mentioned heat treatment method for preparing a Ni2CoCrFeTi0.2Al0.1 high entropy alloy with uneven composition.
[0018] The present invention has the following beneficial effects:
[0019] The present invention first adopts a solid solution technical solution to the Ni2CoCrFeTi0.2Al0.1 high entropy alloy to eliminate the casting defects of the original alloy and make the internal composition of the sample uniform, and then adopts a cold rolling process to reduce the thickness of the sample by 70%. In this process, cold rolling may change the grain structure inside the alloy, and then through the process of recrystallization annealing and heat preservation, the high entropy alloy is decomposed by amplitude modulation to produce two precipitated phases, and a high entropy alloy with uneven composition is obtained. These high entropy alloys with uneven composition may show different excellent properties. Therefore, the heat treatment preparation method provided by the present invention can realize the diversification of performance such as mechanical properties for high entropy alloys by means of uneven composition. At the same time, the technical solution provided by the present invention also provides a reference for the heat treatment of other high entropy alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 It is the overall heat treatment flow chart of the sample;
[0022] Figure 2 is the sample morphology after rolling;
[0023] Figure 3 It is the step pattern on both sides of the sample cut by ion beam;
[0024] Figure 4 It is the first cut through picture of the sample;
[0025] Figure 5 The sample image is extracted using a tungsten needle;
[0026] Figure 6 It is a cutting sample diagram;
[0027] Figure 7 The first step is to weld the sample to the sample holder;
[0028] Figure 8 It is the final thinning map of the sample;
[0029] Fig. 9 is a STEM image of the sample of Example 1;
[0030] Fig.10 is the energy spectrum image of the sample in Example 1;
[0031] Fig.11 is the sample point scan image;
[0032] Fig.12 is the sample line scan image;
[0033] Fig.13 is the STEM image of the sample of Example 2;
[0034] Fig.14 This is the energy spectrum image of the sample in Example 2;
[0035] Fig.15 is the STEM image of the sample of Example 3;
[0036] Fig.16 This is the energy spectrum image of the sample in Example 3;
[0037] Fig.17 is the STEM image of the sample of Example 4;
[0038] Fig.18 This is the energy spectrum image of the sample in Example 4;
[0039] Fig.19 is the STEM image of the sample of Example 5;
[0040] Fig. 20 This is the energy spectrum image of the sample in Example 5. DETAILED DESCRIPTION
[0041] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0042] Example 1
[0043] (1) Take a Ni2CoCrFeTi0.2Al0.1 alloy ingot and pretreat the alloy: use wire cutting to process a 20*8*4 mm block sample on the initial ingot rod;
[0044] Use 320# and 400# sandpaper to grind off the wire-cut layer on the surface of the sample;
[0045] The sample was placed in the center of a three-zone vertical quenching furnace. The two ends of the tube furnace were connected to an Ar gas cylinder and a molecular pump. After the vacuum reached 10E-4Pa, it was heated to 1200℃ and kept for 2h, and then quenched to room temperature with water.
[0046] Use 320# and 400# sandpaper to polish the sample in turn;
[0047] (2) After more than 20 cold rollings, the thickness is uniformly reduced by 70% from 3.7 mm to 1.11 mm. The morphology after rolling is as follows: Figure 2 As shown;
[0048] (3) Place it in the center of a three-zone vertical quenching furnace, connect an Ar gas cylinder and a molecular pump to both ends of the tube furnace, and after the vacuum reaches 10E-4Pa, heat it to 1200℃ and keep it for 10min for recrystallization, and then quench it with water to room temperature;
[0049] Use 320# and 400# sandpaper to polish the sample surface in turn;
[0050] (4) The sample was placed at the center of a three-zone vertical quenching furnace. The two ends of the tube furnace were connected to an Ar gas cylinder and a molecular pump. After the vacuum reached 10E-4Pa, the sample was heated to 800℃ and kept for 168h, and then quenched with water to room temperature.
[0051] The samples were processed into 1*1*0.5mm sheet samples by wire cutting;
[0052] The sample was polished with 400#, 800#, 1200#, 2000#, 3000#, 5000# and 7000# sandpaper in sequence. The final thickness of the sample was 70μm, and it was polished flat with a mechanical polisher.
[0053] The specific process flow chart is as follows Figure 1 shown.
[0054] Test the prepared samples:
[0055] Using the focused ion beam system, after adjusting the sample stage to the concentric height, first find a suitable scratch-free area of the sample in the electron beam window, turn the sample stage to 52° and use the ion beam (30kV 93pA) to assist deposition. The final C protective layer thickness is about 1μm.
[0056] Use an ion beam (30kV 21nA) to cut the sample. The ion source is Si. The sample stage is tilted 52°. Step-shaped pits are cut on both sides of the sample. The sample surface is about 10μm away from the deepest part of the pit, and the upper pit is slightly larger than the lower pit (to facilitate sample extraction). Figure 3 shown; from Figure 3 It can be seen that stepped pits have been cut into both sides of the sample;
[0057] The sample was initially thinned to a thickness of 1 μm using an ion beam current of 2.8 nA and an ion source of Si.
[0058] Then tilt the sample stage to 7° and draw a U-shaped pattern to make the sample completely clean without adhesion. After cutting, cut off the left side and hang on the right side. Figure 4 Shown is the first cut through image of the sample;
[0059] Tilt the sample stage to 0°, move the tungsten needle to the same height as the sample, flush with the upper surface of the sample, and use an ion beam (30kV93pA) to deposit C for welding; Figure 5 Shown is a sample image extracted by a tungsten needle;
[0060] Set the ion beam current to 5.8 nA, the ion source to Si, cut off the hanging connection on the right side of the sample, and withdraw the tungsten needle; Figure 6 Shown is a diagram of a cut sample;
[0061] Move the sample stage to find the ABC sample holder in the electron beam window, and move the tungsten needle to carry the sample to contact the target position of the sample holder;
[0062] Use ion beam (30kV 93pA) and Pt dep to weld the sample stage and sample holder firmly, and then use Si ion source to cut off the welding point between the sample and the tungsten needle; Figure 7 The figure shows welding the sample to the sample holder;
[0063] The sample stage is tilted to 52°, the ion source is Si, and the sample is thinned step by step by continuously changing the beam current of the ion beam until the thickness of the sample is 70nm; Figure 8 This is the final image of the sample after thinning;
[0064] The extracted samples were placed in a HF5000 spherical aberration corrected transmission electron microscope, and the morphology of the sample precipitation phase was observed by STEM mode; Fig. 9 The STEM image of the sample is shown. Fig. 9 It can be clearly seen from the image in that the composition of the prepared high entropy alloy is not uniform; the energy spectrum information of the sample is obtained using a HF5000 spherical aberration corrected transmission electron microscope; Fig.10 Shown is the energy spectrum image of the sample; Fig.11 Scan the image for the sample point; Fig.12 It is a line scan image of the sample. From the energy spectrum image, it can be seen that the diameter of the uneven spheres of the alloy is greater than 50nm, and the unevenness is very obvious.
[0065] Example 2
[0066] In step (4), the holding time is 3 hours, and the rest is the same as in Example 1. The STEM image is shown in the attached Fig.13 The energy spectrum images of the six elements of the Ni2CoCrFeTi0.2Al0.1 high entropy alloy are shown in the attached figure. Fig.14 As shown. Fig.13 and Fig.14 It can be clearly seen from the image that the composition of the prepared high entropy alloy is not uniform, among which, Fig.14 The average value of the uneven spherical diameter is 12 nm.
[0067] Example 3
[0068] In step (4), the holding time is 6 hours, and the rest is the same as in Example 1. The STEM image is shown in the attached Fig.15 The energy spectrum images of the six elements of the Ni2CoCrFeTi0.2Al0.1 high entropy alloy are shown in the attached figure. Fig.16 As shown. Fig.15 and Fig.16 It can be clearly seen from the image that the composition of the prepared high entropy alloy is not uniform, among which, Fig.16 The average value of the uneven spherical diameter is 19 nm.
[0069] Example 4
[0070] In step (4), the holding time is 12 h, and the rest is the same as in Example 1. The STEM image is shown in the attached Fig.17 The energy spectrum images of the six elements of the Ni2CoCrFeTi0.2Al0.1 high entropy alloy are shown in the attached figure. Fig.18 As shown. Fig.17 and Fig.18 It can be clearly seen from the image that the composition of the prepared high entropy alloy is not uniform, among which, Fig.18 The average value of the non-uniform spherical diameter is 25 nm.
[0071] Example 5
[0072] In step (4), the holding time is 48 hours, and the rest is the same as in Example 1. The STEM image is shown in the attached Fig.19 The energy spectrum images of the six elements of the Ni2CoCrFeTi0.2Al0.1 high entropy alloy are shown in the attached figure. Fig. 20 As shown. Fig.19 and Fig. 20 It can be clearly seen from the image that the composition of the prepared high entropy alloy is not uniform, among which, Fig. 20 The average value of the non-uniform spherical diameter is 47.5 nm.
[0073] From the STEM images and energy spectra of the above embodiments, it can be clearly seen that the composition of the prepared high entropy alloy is inhomogeneous, and as the holding time increases, the average value of the inhomogeneous spherical diameter also increases. Therefore, the present invention can obtain high entropy alloys with different composition inhomogeneities by adopting the technical solution of holding annealing after recrystallization of the high entropy alloy and controlling different holding times.
[0074] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A Ni2CoCrFeTi 0.2 Al 0.1 A heat treatment method for a high entropy alloy, characterized in that: The following steps are involved: (1) Take Ni2CoCrFeTi 0.2 Al 0.1 The high entropy alloy is cut into block samples, placed in a high vacuum quenching furnace for solid solution, and then water quenched to room temperature; the solid solution temperature is 1200°C and the time is 2h; (2) cold rolling the quenched block sample until the thickness is reduced by 70%; (3) placing the cold-rolled sample in a high vacuum quenching furnace for heating and recrystallization, and then quenching it with water to room temperature; the heating and recrystallization temperature is 1200° C. and the time is 10 min; (4) placing the product in a high vacuum quenching furnace for heating and heat preservation again, and then quenching it with water to room temperature, wherein the heating and heat preservation temperature is 800° C. and the time is 3-168 h.
2. The heat treatment method according to claim 1, characterized in that In step (2), the cold rolling is performed by using a rolling mill for 20 times or more.
3. The heat treatment method according to claim 1, characterized in that: In the step (4), the heating and insulation time is 168 hours.
4. The heat treatment method according to claim 1, characterized in that: The vacuum degree of the high vacuum quenching furnace is 10E - 4 Pa.
Citation Information
Cited By
2500MPa-grade ultrahigh-strength high-entropy alloy and preparation method thereof