Production method of ENiCrMo-3 welding rod
Through vacuum induction smelting, electroslag remelting, diameter forging straight material forging and solid solution treatment, combined with drug skin coating technology, the problem of domestic production of ENiCrMo-3 electrodes is solved, high purity and good tensile performance are achieved, and the Cost and improve productivity.
Patent Information
- Application Number
- CN202411262502.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
The existing ENiCrMo-3 welding rods rely on imports, are expensive and have limited delivery time, and lack domestic solutions.
A reasonable process route design is adopted, including vacuum induction smelting, electroslag remelting, diameter forging straight material forging and solid solution treatment, combined with drug skin covering technology, to ensure the purity, tissue uniformity and surface quality of the welding rod.
The high purity, structure uniformity and good tensile performance of ENiCrMo-3 welding rods are achieved, which solves the problem of domestic production, reduces costs and improves production efficiency.
Smart Images

Figure CN119035873A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material manufacturing, and particularly relates to a production method of an ENiCrMo-3 welding rod. Background Art
[0002] UNS N06625 alloy is a solid solution strengthened nickel-based alloy with excellent high temperature performance, long-lasting performance and corrosion resistance. It is often used in nuclear power, thermal power, chemical industry and other related equipment manufacturing fields. ENiCrMo-3 welding rods are mainly used for welding of this series of nickel-chromium-molybdenum alloys, and the demand is large. The existing ENiCrMo-3 welding rods mainly rely on imports, which are expensive and have limited delivery time. Therefore, the development of the production raw material ENiCrMo-3 welding rod has broad market prospects and is conducive to the localization of ENiCrMo-3 welding rods. Summary of the invention
[0003] In view of the problems in the prior art, the present invention provides a method for producing ENiCrMo-3 welding rods. The method has a reasonable process route design, a fast pace, and high production efficiency. The produced product has high purity, uniform structure, and well-controlled grain size and room temperature tensile properties. At the same time, it has good surface quality and drawing forming performance.
[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:
[0005] A method for producing an ENiCrMo-3 welding rod comprises the following steps:
[0006] Step 1, according to the composition of the metal raw materials, calculate the raw material ratio according to the ENiCrMo-3 target composition, and weigh the metal raw materials respectively according to the ratio relationship; the metal raw materials use return materials or alloy materials; the metal raw materials are cleaned before use to remove surface impurities, and dried to ensure that the raw materials are clean and dry. Among them, the nickel plate is cut into small pieces of (100-150)*(100-150)mm. The removal of surface impurities is to use a drum-type rust remover to remove rust on the nickel plate, pure iron, return materials and alloy materials to eliminate surface oxide scale and attachments; the drying is carried out in a chamber furnace, the drying temperature is 380-450℃, and the drying time is ≥4h;
[0007] Step 2, vacuum induction smelting, metal nickel and metal molybdenum are charged into a furnace, vacuumed for melting and refining, and then metal chromium and nickel niobium are added after melting and refining, and secondary refining is performed after chemical cleaning, and metal aluminum and metal titanium are added after refining is completed, argon gas is filled for refining, sampling and fine-tuning the composition until the composition is qualified, and temperature measurement and steel tapping are obtained to obtain vacuum induction ingots; the temperature of the melting and refining is 1470-1570°C, the time is ≥20min, the temperature of the secondary refining after chemical cleaning is 1480-1580°C, the time is ≥25min, and the pressure of the argon gas is 7000-10000Pa; the temperature of the steel tapping is 1440-1500°C. The whole process of vacuum induction smelting is isolated from the atmosphere, which provides a basis for reducing the gas content of molten steel. High vacuum is drawn during smelting, and the liquid level is in a high vacuum state, which is conducive to the separation of ONH elements in the molten steel. In addition, the refining is divided into two refinings, the first refining removes impurities in the furnace amount, and deoxidizers Al and Ti are added before the secondary refining. The purity of the alloy is improved through step-by-step deoxidation and desulfurization;
[0008] Step 3, electroslag remelting: firstly, flatten and grind the vacuum induction ingot to remove surface defects, then weld the induction ingot and the auxiliary electrode together and load them into the electroslag remelting furnace for electroslag remelting to obtain an electroslag ingot, wherein the steady-state melting rate of the electroslag remelting is 4.8-5.8kg / min, and a 6 series nickel-based alloy bottom pad is used instead of a conventional carbon steel bottom pad to avoid the bottom pad melting during arc starting, resulting in increased iron at the bottom of the electroslag ingot;
[0009] Step 4, forging: the steel ingot is homogenized, and then directly forged into a blank (diameter forging straight material) by a radial forging machine to obtain a square billet. The temperature of the homogenization treatment is 1170-1220°C, and the radial forging straight material is formed by two-fire radial forging. The forging temperature is 1150-1200°C, the opening forging temperature is ≥930°C, the final forging temperature is ≥800°C, and the forging elongation is controlled within 1.4. The radial forging regulates the multi-pass large deformation and the intermediate heating system to match the crushed precipitated phase, accelerate the dissolution of the harmful phase, and make the final organization uniformly distributed. Compared with the use of a fast forging machine to forge a square billet (fast forging straight material), the radial forging machine has a fast deformation frequency, the intermediate billet can be hot-cut online, and the forging fire is reduced at the same time, and the overall production rhythm is fast. Compared with the fast forging machine + radial forging machine combined forging into a square billet (fast radial combination), the radial forging straight material reduces the cold material heating and material transportation time, and can be produced continuously.
[0010] Step 5, placing the billet in a walking beam heating furnace for heating, and obtaining a wire rod through preliminary rolling and finish rolling, wherein the diameter of the wire rod is 5.5 mm, the tolerance is within 0.25 mm, the rolling temperature is 1180-1210° C., the starting rolling temperature is ≥1000° C., and the final rolling temperature is ≥870° C.;
[0011] Step 6, the wire is loaded into a ring furnace for solid solution, the solid solution temperature is controlled at 1080-1120 ° C, and after heat preservation, it is cooled in circulating water. After solid solution at this temperature, the grain size of the wire can be controlled at level 3-5, and the tensile strength is controlled at 700-830MPa, which can effectively avoid wire breakage, surface peeling and other problems in the subsequent drawing process. At the same time, the oxide scale on the surface of the wire becomes loose, and after acid pickling and high-pressure water washing, the surface oxide scale can be quickly and efficiently cleaned to ensure the surface quality; the welding core is obtained by drawing, and the chemical composition (wt.%) of the welding core is C≤0.02%, Si≤0.3%, Mn≤0.15%, P≤0.005%, S≤0.01%, Cr 21.5-22.5%, Ni≥58%, Mo 8.5-9.5%, Al 0.1-0.25%, Ti 0.1-0.3%, Nb+Ta 3.4-3.8%, Fe≤0.5%, Cu≤0.05%;
[0012] Step 7, mixing calcium difluoride, potassium feldspar, marble and sodium potassium water glass and grinding them to form a homogeneous fine powder; then adding sodium methyl silicate, aluminum isopropoxide and n-butyl titanate and stirring in a sealed state for 20-30 minutes to obtain a prefabricated powder; the mass ratio of the prefabricated powder is: 7-10 parts of calcium difluoride, 8-15 parts of potassium feldspar, 3-5 parts of marble, 3-5 parts of sodium potassium water glass, 0.5-1 part of sodium methyl silicate, 10-12 parts of aluminum isopropoxide, and 10-15 parts of n-butyl titanate, the grinding temperature is 5-10°C, the grinding pressure is 0.3-0.5MPa, and the stirring speed of the sealed stirring is 300-500r / min; the concentration of the potassium sodium water glass is 44°-45°;
[0013] Step 8, uniformly coating the homogeneous fine powder on the surface of the wire to be coated, using a batten machine for coating treatment, and obtaining an ENiCrMo-3 welding rod after static baking and high-temperature baking, wherein the amount of the homogeneous fine powder added is 50-70% of the wire quality; the atmosphere of the low-temperature baking is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9-10:1, and the temperature of the high-temperature baking is 300-350°C; this step utilizes the liquid properties of potassium sodium water glass and n-butyl titanate to improve the fluidity of the fine powder, thereby ensuring the stability of the uniform distribution, and after static baking, n-butyl titanate and aluminum isopropoxide are in-situ hydrolyzed, and the subsequent high-temperature baking is combined to form a bonding effect with good permeability, thereby ensuring the stability and gap-filling properties of the coating, and having an excellent protective effect on the wire, and the in-situ polycondensation of aluminum hydroxide and titanic acid brought about by the high-temperature baking improves the density of the coating. The material of the coating itself is somewhat similar to that of the wire, and a close connection is formed during the coating, static baking and high-temperature baking processes, reducing the gap between the coating and the wire.
[0014] It can be seen from the above description that the present invention has the following advantages:
[0015] 1. The ENiCrMo-3 welding rod prepared by the present invention has high purity, uniform structure, good control of grain size and tensile properties, and good surface quality and drawing forming performance, which is conducive to the localization of ENiCrMo-3 welding rods and solves the problem that ENiCrMo-3 welding rods are imported from abroad, are expensive, and have limited delivery time.
[0016] 2. The present invention adopts a high-purity smelting method (vacuum induction + protective atmosphere electroslag remelting special smelting). Control the induction refining temperature and time to remove harmful elements; control the steady-state melting rate of electroslag to ensure shrinkage compensation; use a 6-series nickel-based alloy bottom pad to solve the problem of increased iron content at the bottom of the electroslag. The wire produced by the high-purity smelting method has less non-metallic inclusions and the gas content is controlled at a low level.
[0017] 3. The present invention adopts the forging blanking method of radial forging straight materials, the deformation pass distribution is reasonable, the square billet structure is uniform, continuous production can be achieved, the transfer rhythm is fast, and the production efficiency is high.
[0018] 4. The present invention adopts solid solution treatment to control the temperature, so as to adjust the grain size to level 3-5 and the tensile strength to between 700-830 MPa, and the subsequent pickling and drawing forming effects are excellent.
[0019] 5. The coating of the present invention contains n-butyl titanate and potassium sodium water glass, which has good fluidity in the precursor state, not only forms a close connection with the wire, but also can play a good protective role on the wire, and at the same time has the functions of improving the mechanical properties of the weld, stabilizing arc combustion, Baohua weld and reducing welding slag. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a photograph of the solid solution grain size of the wire prepared in Example 1 of the present invention;
[0021] Figure 2 is a photograph of the solid solution grain size of the wire prepared in Example 2 of the present invention;
[0022] Figure 3 This is a photograph of the solid solution grain size of the wire prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0023] Combination Figures 1 to 3 The embodiments of the present invention are described in detail, but no limitation is imposed on the claims of the present invention.
[0024] Example 1
[0025] A method for producing an ENiCrMo-3 welding rod comprises the following steps:
[0026] Step 1, according to the composition of the metal raw materials, calculate the raw material ratio according to the ENiCrMo-3 target composition, and weigh the metal raw materials respectively according to the ratio relationship; the metal raw materials use return materials or alloy materials; the metal raw materials are cleaned before use to remove surface impurities, and dried to ensure that the raw materials are clean and dry. Among them, the nickel plate is cut into small pieces of 100*100mm after slitting. The removal of surface impurities is to use a drum-type rust remover to remove rust on the nickel plate, pure iron, return materials and alloy materials to eliminate surface oxide scale and attachments; the drying is carried out in a chamber furnace, the drying temperature is 380°C, and the drying time is 4h;
[0027] Step 2, vacuum induction smelting, charging metal nickel and metal molybdenum into a furnace, vacuumizing and melting and refining, then adding metal chromium and nickel niobium after melting and refining, and refining again after chemical cleaning, adding metal aluminum and metal titanium after refining, refining with argon gas, sampling and fine-tuning the composition until the composition is qualified, measuring the temperature and tapping to obtain a vacuum induction ingot; the temperature of the melting and refining is 1470-1570°C, the time is 20min, the temperature of the secondary refining after chemical cleaning is 1480-1580°C, the time is 25min, the pressure of the argon gas is 7000-10000Pa; the tapping temperature is 1440°C;
[0028] Step 3, electroslag remelting: firstly, flatten and grind the vacuum induction ingot to remove surface defects, then weld the induction ingot and the auxiliary electrode together and load them into the electroslag remelting furnace for electroslag remelting to obtain an electroslag ingot, wherein the steady-state melting rate of the electroslag remelting is 5.0-5.8kg / min;
[0029] Step 4, forging: homogenizing the electroslag ingot and then forging to obtain a square billet, wherein the homogenizing temperature is 1170-1220° C., the forging adopts two-fire fine forging, the forging temperature is 1150-1200° C., the start forging temperature is 957-1027° C., the final forging temperature is 886-898° C., and the forging elongation is controlled within 1.35;
[0030] Step 5, placing the billet in a walking beam heating furnace for heating, and obtaining a wire rod through preliminary rolling and finish rolling, wherein the diameter of the wire rod is 5.5 mm, the tolerance is within 0.25 mm, the rolling temperature is 1180-1210° C., the starting rolling temperature is ≥1005° C., and the final rolling temperature is ≥900° C.;
[0031] Step 6, the wire is placed in a ring furnace for solid solution, heated and kept at 1000°C, then cooled in circulating water, pickled with acid, rinsed with high-pressure water, the surface oxide scale is cleaned, and the welding core is obtained by drawing;
[0032] Step 7, mixing calcium difluoride, potassium feldspar, marble and sodium potassium water glass and grinding them to form a homogeneous fine powder; then adding sodium methyl silicate, aluminum isopropoxide and n-butyl titanate and stirring in a sealed manner for 20 minutes to obtain a prefabricated powder; the mass ratio of the prefabricated powder is: 7 parts of calcium difluoride, 8 parts of potassium feldspar, 3 parts of marble, 3 parts of sodium potassium water glass, 0.5 parts of sodium methyl silicate, 10 parts of aluminum isopropoxide, and 10 parts of n-butyl titanate, the grinding temperature is 5°C, the grinding pressure is 0.3MPa, and the stirring speed of the sealed stirring is 300r / min; the concentration of the potassium sodium water glass is 44°;
[0033] Step 8, evenly coating the homogeneous fine powder on the surface of the welding core, using a batten machine to wrap it, and obtaining the ENiCrMo-3 welding rod after static baking and high-temperature baking. The amount of the homogeneous fine powder added is 50% of the wire quality; the atmosphere of the low-temperature baking is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the temperature of the high-temperature baking is 300°C.
[0034] The ENiCrMo-3 prepared in this embodiment has a fast production rhythm and high production efficiency, and the produced wire has high purity, uniform structure, and good control of grain size and room temperature tensile properties, and has good surface quality and drawing forming performance; the prepared welding rod has less spatter, easy arc re-striking, simple slag removal, excellent slag, beautiful weld formation and no pores during welding.
[0035] Example 2
[0036] A method for producing an ENiCrMo-3 welding rod comprises the following steps:
[0037] Step 1, according to the composition of the metal raw materials, calculate the raw material ratio according to the ENiCrMo-3 target composition, and weigh the metal raw materials respectively according to the ratio relationship; the metal raw materials use return materials or alloy materials; the metal raw materials are cleaned before use to remove surface impurities, and dried to ensure that the raw materials are clean and dry. Among them, the nickel plate is cut into small pieces of 150*150mm. The removal of surface impurities is to use a drum-type rust remover to remove rust on the nickel plate, pure iron, return materials and alloy materials to eliminate surface oxide scale and attachments; the drying is carried out in a chamber furnace, the drying temperature is 450°C, and the drying time is 4.5h;
[0038] Step 2, vacuum induction smelting, charging metal nickel and metal molybdenum into a furnace, vacuumizing and melting and refining, then adding metal chromium and nickel niobium after melting and refining, and refining again after chemical cleaning, adding metal aluminum and metal titanium after refining, refining with argon gas, sampling and fine-tuning the composition until the composition is qualified, measuring the temperature and tapping to obtain a vacuum induction ingot; the temperature of the melting and refining is 1470-1570°C, the time is 40min, the temperature of the secondary refining after chemical cleaning is 1480-1580°C, the time is 30min, the pressure of the argon gas is 7000-10000Pa; the tapping temperature is 1500°C;
[0039] Step 3, electroslag remelting: firstly, flatten and grind the vacuum induction ingot to remove surface defects, then weld the induction ingot and the auxiliary electrode together and load them into the electroslag remelting furnace for electroslag remelting to obtain an electroslag ingot, wherein the steady-state melting rate of the electroslag remelting is 5.1-5.8 kg / min;
[0040] Step 4, forging: homogenizing the electroslag ingot and then forging to obtain a square billet, wherein the homogenizing temperature is 1185-1215° C., the forging adopts two-fire fine forging, the forging temperature is 1165-1195° C., the start forging temperature is 977-1016° C., the final forging temperature is 887-901° C., and the forging elongation is controlled within 1.34;
[0041] Step 5, placing the billet in a walking beam heating furnace for heating, and obtaining a wire rod through preliminary rolling and finish rolling, wherein the diameter of the wire rod is 5.5 mm, the tolerance is within 0.25 mm, the rolling temperature is 1185-1215° C., the start rolling temperature is ≥1005° C., and the final rolling temperature is ≥900° C.;
[0042] Step 6, the wire is placed in a ring furnace for solid solution, heated and kept at 1000°C, then cooled in circulating water, pickled with acid, rinsed with high-pressure water, the surface oxide scale is cleaned, and the welding core is obtained by drawing;
[0043] Step 7, mixing calcium difluoride, potassium feldspar, marble and sodium potassium water glass and grinding them to form a homogeneous fine powder; then adding sodium methyl silicate, aluminum isopropoxide and n-butyl titanate and stirring in a sealed state for 20-30 minutes to obtain a prefabricated powder; the mass ratio of the prefabricated powder is: 10 parts of calcium difluoride, 15 parts of potassium feldspar, 5 parts of marble, 5 parts of sodium potassium water glass, 1 part of sodium methyl silicate, 12 parts of aluminum isopropoxide, and 15 parts of n-butyl titanate, the grinding temperature is 10°C, the grinding pressure is 0.5MPa, and the stirring speed of the sealed stirring is 300-500r / min; the concentration of the potassium sodium water glass is 45°;
[0044] Step 8, evenly coating the homogeneous fine powder on the surface of the welding core, using a batten machine for coating treatment, and obtaining the ENiCrMo-3 welding rod after static baking and high-temperature baking. The amount of the homogeneous fine powder added is 70% of the wire quality; the atmosphere of the low-temperature baking is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10:1, and the temperature of the high-temperature baking is 350°C.
[0045] The ENiCrMo-3 prepared in this embodiment has a fast production rhythm and high production efficiency, and the produced wire has high purity, uniform structure, and good control of grain size and room temperature tensile properties, and has good surface quality and drawing forming performance; the prepared welding rod has less spatter, easy arc re-striking, simple slag removal, excellent slag, beautiful weld formation and no pores during welding.
[0046] Example 3
[0047] A method for producing an ENiCrMo-3 welding rod comprises the following steps:
[0048] Step 1, according to the composition of the metal raw materials, calculate the raw material ratio according to the ENiCrMo-3 target composition, and weigh the metal raw materials respectively according to the ratio relationship; the metal raw materials use return materials or alloy materials; the metal raw materials are cleaned before use to remove surface impurities, and dried to ensure that the raw materials are clean and dry. Among them, the nickel plate is cut into small pieces of 150*150mm after slitting. The removal of surface impurities is to use a drum-type rust remover to remove rust on the nickel plate, pure iron, return materials and alloy materials to eliminate surface oxide scale and attachments; the drying is carried out in a chamber furnace, the drying temperature is 400℃, and the drying time is 4h;
[0049] Step 2, vacuum induction smelting, charging metal nickel and metal molybdenum into a furnace, vacuumizing and melting and refining, then adding metal chromium and nickel niobium after melting and refining, and refining again after chemical cleaning, adding metal aluminum and metal titanium after refining, refining with argon gas, sampling and fine-tuning the composition until the composition is qualified, measuring the temperature and tapping to obtain a vacuum induction ingot; the melting and refining temperature is 1480-1560°C, the time is 30min, the secondary refining temperature after chemical cleaning is 1480-1560°C, the time is 35min, the pressure of the argon gas is 8000-10000Pa; the tapping temperature is 1488°C;
[0050] Step 3, electroslag remelting: firstly, flatten and grind the vacuum induction ingot to remove surface defects, then weld the induction ingot and the auxiliary electrode together and load them into the electroslag remelting furnace for electroslag remelting to obtain an electroslag ingot, wherein the steady-state melting rate of the electroslag remelting is 5.0-5.7 kg / min;
[0051] Step 4, forging: homogenizing the electroslag ingot and then forging to obtain a square billet, wherein the homogenizing temperature is 1185-1215° C., the forging adopts two-fire fine forging, the forging temperature is 1165-1195° C., the start forging temperature is ≥957° C., the final forging temperature is ≥881° C., and the forging elongation is controlled within 1.4;
[0052] Step 5, placing the billet in a walking beam heating furnace for heating, and obtaining a wire rod through preliminary rolling and finish rolling, wherein the diameter of the wire rod is 5.5 mm, the tolerance is within 0.25 mm, the rolling temperature is 1185-1215° C., the start rolling temperature is ≥1061° C., and the final rolling temperature is ≥935° C.;
[0053] Step 6: Place the wire into a ring furnace for solid solution, heat and keep it at 1000°C, cool it in circulating water, pickle it with acid, rinse it with high-pressure water, clean the surface oxide skin, and draw it to obtain the welding core.
[0054] Step 7, mixing calcium difluoride, potassium feldspar, marble and sodium potassium water glass and grinding them to form a homogeneous fine powder; then adding sodium methyl silicate, aluminum isopropoxide and n-butyl titanate and stirring them in a sealed state for 25 minutes to obtain a prefabricated powder; the mass ratio of the prefabricated powder is: 8 parts of calcium difluoride, 12 parts of potassium feldspar, 4 parts of marble, 4 parts of sodium potassium water glass, 0.8 parts of sodium methyl silicate, 11 parts of aluminum isopropoxide, and 13 parts of n-butyl titanate, the grinding temperature is 8°C, the grinding pressure is 0.4MPa, and the stirring speed of the sealed stirring is 300-500r / min; the concentration of the potassium sodium water glass is 45°;
[0055] Step 8, uniformly coating the homogeneous fine powder on the surface of the wire to be coated, using a batten machine for coating treatment, and obtaining the ENiCrMo-3 welding rod after static baking and high-temperature baking. The amount of the homogeneous fine powder added is 60% of the wire quality; the atmosphere of the low-temperature baking is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the temperature of the high-temperature baking is 330°C.
[0056] The ENiCrMo-3 welding rod prepared in this embodiment has a fast production rhythm and high production efficiency, and the produced wire has high purity, uniform structure, and good control of grain size and room temperature tensile properties, and has good surface quality and drawing forming performance; the prepared welding rod has less spatter, easy arc re-striking, simple slag removal, excellent slag, beautiful weld formation and no pores during welding.
[0057] Performance Testing
[0058] The wires in Examples 1-3 were used as samples for testing, and the results are as follows:
[0059] The chemical composition of the wires of Examples 1-3 is shown below:
[0060]
[0061]
[0062] The non-metallic inclusions of the wires of Examples 1-3 are shown in the following table:
[0063]
[0064] The solid solution grain sizes of the wires of Examples 1-3 are as follows:
[0065] The solid solution grain size of the wire of Example 1 is as follows: Figure 1 As shown, it reaches level 4.5.
[0066] The solid solution grain size of the wire of Example 2 is as follows: Figure 2 As shown, reach level 5.
[0067] The solid solution grain size of the wire of Example 3 is as follows: Figure 3 As shown, reach level 5.
[0068] The welds welded by the welding rods of Examples 1-3 were tested, and the results are as follows:
[0069]
[0070] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for producing an ENiCrMo-3 welding rod, comprising the following steps: Step 1, according to the composition of the metal raw materials, the raw material ratio is calculated according to the ENiCrMo-3 target composition, and the metal raw materials are weighed respectively according to the ratio relationship; Step 2, vacuum induction smelting, loading metal nickel and metal molybdenum into a furnace, vacuumizing and melting and refining, then adding metal chromium and nickel niobium after melting and refining, and refining again after chemical clarification, adding metal aluminum and metal titanium after refining, refining with argon, sampling and fine-tuning the composition until the composition is qualified, measuring the temperature and tapping the steel to obtain a vacuum induction ingot; Step 3, electroslag remelting: firstly, flatten and grind the vacuum induction ingot to remove surface defects, then weld the induction ingot and the auxiliary electrode together and load them into the electroslag remelting furnace for electroslag remelting to obtain an electroslag ingot; Step 4, forging: homogenizing the electroslag ingot, and then forging it to obtain a square billet; Step 5, placing the billet in a walking beam heating furnace for heating, and obtaining wire rod through initial rolling and finish rolling; Step 6, placing the wire into a ring furnace for solid solution, cooling it in circulating water after heat preservation, and washing it with acid solution and high-pressure water to clean the surface oxide scale to obtain a welding core; Step 7, mixing and grinding calcium difluoride, potassium feldspar, marble and sodium potassium water glass to form a homogeneous fine powder; then adding sodium methyl silicate, aluminum isopropoxide and n-butyl titanate and stirring in a sealed manner for 20-30 minutes to obtain a prefabricated powder; Step 8, evenly coating the homogeneous fine powder on the surface of the wire to be coated, using a batten machine to coat it, and obtaining the ENiCrMo-3 welding rod through static baking and high-temperature baking.
2. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The metal raw material in step 1 is recycled material or alloy material.
3. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The temperature of the smelting and refining in step 2 is 1470-1570°C, and the time is ≥20min. The temperature of the secondary refining after smelting and refining is 1480-1580°C, and the time is ≥25min. The pressure of the argon filling is 7000-10000Pa; the temperature of the steel tapping is 1440-1500°C.
4. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The steady-state melting rate of the electroslag remelting in step 3 is 4.8-5.8 kg / min.
5. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The temperature of the homogenization treatment in step 4 is 1170-1220°C, the forging adopts two-diameter forging straight material, the forging temperature is 1150-1200°C, the start forging temperature is ≥930°C, the final forging temperature is ≥800°C, and the forging elongation is controlled within 1.
4.
6. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The diameter of the wire in step 5 is 5.5 mm, with a tolerance within 0.25 mm. The rolling temperature is 1180-1210° C., the starting rolling temperature is ≥1000° C., and the final rolling temperature is ≥870° C.
7. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The heating temperature in step 6 is 1080-1120°C.
8. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The chemical composition (wt.%) of the welding core in step 6 is: C≤0.02%, Si≤0.3%, Mn≤0.15%, P≤0.005%, S≤0.01%, Cr21.5-22.5%, Ni≥58%, Mo 8.5-9.5%, Al 0.1-0.25%, Ti 0.1-0.3%, Nb+Ta 3.4-3.8%, Fe≤0.5%, Cu≤0.05%.
9. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The mass ratio of the prefabricated powder in step 7 is: 7-10 parts of calcium difluoride, 8-15 parts of potassium feldspar, 3-5 parts of marble, 3-5 parts of sodium potassium water glass, 0.5-1 part of sodium methyl silicate, 10-12 parts of aluminum isopropoxide, and 10-15 parts of n-butyl titanate. The grinding temperature is 5-10° C., the grinding pressure is 0.3-0.5 MPa, and the stirring speed of the sealed stirring is 300-500 r / min; the concentration of the potassium sodium water glass is 44°-45°.
10. The method for producing the ENiCrMo-3 welding rod according to claim 1, characterized in that: The amount of the homogeneous fine powder added in step 8 is 50-70% of the wire quality; the atmosphere of the low-temperature baking is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9-10:1, and the temperature of the high-temperature baking is 300-350°C.