Method for improving electromagnetic wave absorption performance of hollow copper selenide box
Through template directional in-situ selenization/sulfation reaction and S-doping adjustment, the structure and performance of the selenized copper box are optimized, and the problem of insufficient electromagnetic wave absorption performance of existing copper selenized materials is solved, achieving a more efficient electromagnetic wave absorption effect.
Patent Information
- Application Number
- CN202310616012.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-29
AI Technical Summary
The electromagnetic wave absorption performance of existing copper selenide materials still needs to be further improved, especially in the GHz frequency range, where there is insufficient electromagnetic wave absorption performance.
Through the template-oriented in-situ selenization/vulcanization reaction, Cu2O microcubes are converted into Cu2-xSe hollow copper selenized box, and its morphology, composition, heterogeneous interface, defect level and conductivity are adjusted through S doping to optimize its Electromagnetic wave absorption performance.
The electromagnetic wave absorption performance of hollow selenized copper boxes is significantly improved, the microwave absorption characteristics of wide band and thin thickness are improved, and more efficient electromagnetic wave absorption, RL strength and effective absorption band are achieved.
Smart Images

Figure CN119038500A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wireless communications, and in particular to a method for improving the electromagnetic wave absorption performance of a hollow copper selenide box. Background Art
[0002] The rapid development of 5G electronic devices in wireless communications and military applications has prompted researchers to develop electromagnetic wave absorbing materials in the GHz frequency range. However, challenges remain due to their limited EMW (electromagnetic wave) attenuation mechanism. To this end, people continue to work hard to improve their electromagnetic response capabilities and optimize impedance matching, including the careful design of parameters such as morphology, defect level, electronic conductivity, composition characteristics, and interface structure.
[0003] Copper selenide is a p-type semiconductor with high earth abundance. Due to their complex structure and valence states (such as Cu 0.87 Se, CuSe, Cu3Se2, Cu 1.8 Se, Cu2Se, CuSe2, etc.) lead to some unique optical and electrical properties, which make it widely used in many fields such as sensors, solar cells, electronic switches, etc., and a lot of work has been invested in the synthesis of copper selenide crystals with different morphologies such as nanoparticles, nanowires and nanotubes.
[0004] However, the electromagnetic wave absorption performance of the copper selenide materials prepared so far still needs to be further improved. Summary of the invention
[0005] The purpose of the present invention is to provide a method for improving the electromagnetic wave absorption performance of a hollow copper selenide box, which can significantly improve the electromagnetic wave absorption performance of the copper selenide box.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for improving the electromagnetic wave absorption performance of a hollow copper selenide box, comprising the following steps:
[0008] Se powder, Na2S and alkali solution are mixed and subjected to hydrothermal reaction to obtain a selenium-sulfur solution;
[0009] Cu2O cubic powder and water are mixed, and the obtained suspension is mixed with a selenium-sulfur solution to perform a selenization-sulfurization reaction to obtain a S-doped hollow copper selenide box.
[0010] Preferably, the usage ratio of the Se powder to the alkali solution is (2.12-6.35) mmol:50 mL; and the concentration of the alkali solution is 10 mol / L.
[0011] Preferably, the temperature of the hydrothermal reaction is 120° C. and the time is 4 hours.
[0012] Preferably, the method for preparing the Cu2O cubic powder comprises: mixing copper salt, alkali, glucose and water, and reducing them to obtain Cu2O cubic powder.
[0013] Preferably, the copper salt includes copper sulfate, and the alkali includes sodium hydroxide; the mass ratio of the copper salt, the alkali and the glucose is 7.5:3.6:4.2.
[0014] Preferably, the reduction temperature is 70° C. and the time is 30 min.
[0015] Preferably, in the selenium-sulfur solution, S 2- with Se 2- The molar ratio is (0.2-5):1 and not 5:1.
[0016] Preferably, in the selenium-sulfur solution, S 2- with Se 2- The molar ratio is 1:5 or 3:3.
[0017] Preferably, the molar ratio of the Cu2O cubic powder to the Se powder is 3.47:(2.12-6.35).
[0018] Preferably, the temperature of the selenization-sulfurization reaction is room temperature and the time is 5 hours.
[0019] The present invention provides a method for improving the electromagnetic wave absorption performance of a hollow selenide copper box. The present invention uses a Cu2O cube as a sacrificial template, and through a template-directed in-situ selenization / sulfurization reaction, a wet chemical method is used to successfully convert the Cu2O microcube into Cu 2-x Se hollow copper selenide box, through S doping adjustment engineering, optimizes the morphology, composition, heterogeneous interface, defect level, conductivity and EMW absorption performance of the hollow copper selenide box, regulates the structure, component and complex dielectric constant of the hollow copper selenide box, improves the EMW absorption performance of the hollow copper selenide box through ion substitution and hollow cube structure, optimizes the microwave absorption characteristics from the perspective of wide band, thin thickness and strong absorption, and further improves the EMW absorption performance of the hollow copper selenide box.
[0020] The results of the embodiment show that the S-doped hollow copper selenide box prepared by the method of the present invention has a high L The strength and EAB of S1 / paraffin-40wt% have obvious advantages, and the RLmin of S2 / paraffin-40wt% is -46.3dB at 2.7mm, and the RLmin of S2 / paraffin-40wt% is -44.5dB at 1.9mm. The S doping regulation engineering mentioned in the present invention is expected to be extended to other sulfide / selenide materials and be widely used. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD patterns of S-doped copper selenide boxes (S1-S3) with different sulfur contents (a) and standard diffraction spectra of CuSe, CuS and Cu7S4 (b);
[0022] Figure 2 The middle is Cu doped with different S contents 2-x The morphology of Se boxes (S1-S3) (ac) and EDSmapping spectra of S1-S3 and the corresponding element statistics (df);
[0023] Figure 3 Specific surface area and pore size distribution diagram of S1-S3;
[0024] Figure 4 is the complex dielectric constant (ab) of T5, S1, S2 and S3 when the filling amount is 40wt% and the ε" of the composite materials of T5, S1, S2 and S3 and paraffin C and ε" P Plot of variation with frequency (cd);
[0025] Figure 5 The three-dimensional reflection loss diagram (a1, b1, c1) of S1, S2, S3 and paraffin composite materials; the two-dimensional reflection loss diagram (a2, b2, c2) of S1, S2, S3 and paraffin composite materials and the effective bandwidth / reflection loss-thickness histogram (a3, b3, c3) of S1, S2, S3 and paraffin composite materials. DETAILED DESCRIPTION
[0026] The present invention provides a method for improving the electromagnetic wave absorption performance of a hollow copper selenide box, comprising the following steps:
[0027] Se powder, Na2S and alkali solution are mixed and subjected to hydrothermal reaction to obtain a selenium-sulfur solution;
[0028] Cu2O cubic powder and water are mixed, and the obtained suspension is mixed with a selenium-sulfur solution to perform a selenization-sulfurization reaction to obtain a S-doped hollow copper selenide box.
[0029] In the present invention, unless otherwise specified, the required reagents are commercially available products well known in the art.
[0030] The invention mixes Se powder, Na2S and alkali solution, and performs hydrothermal reaction to obtain a selenium-sulfur solution.
[0031] In the present invention, the usage ratio of the Se powder to the alkali solution is preferably (2.12-6.35) mmol:50 mL, more preferably 6.35 mmol:50 mL; the concentration of the alkali solution is preferably 10 mol / L; and the alkali in the alkali solution is preferably sodium hydroxide.
[0032] In the present invention, the Na2S is preferably used in the form of Na2S·9H2O; the amount of Na2S preferably satisfies the required S in the selenium-sulfur solution. 2- with Se 2- The molar ratio is sufficient.
[0033] The present invention has no special limitation on the process of mixing the Se powder, Na2S and alkali solution, and the materials can be mixed uniformly according to the process well known in the art.
[0034] In the present invention, the temperature of the hydrothermal reaction is preferably 120°C, and the time is preferably 4 hours. During the hydrothermal reaction, Se reacts with the alkali solution to form Se 2- , Se is converted into 2 / 3Na2Se and 1 / 3Na2SeO3.
[0035] After the hydrothermal reaction is completed, the system is preferably cooled naturally to room temperature, the excess Se powder is filtered to separate, and the liquid material is collected, i.e., the alkaline selenium-sulfur solution (containing Se 2- 、SeO3 2- and S 2- three ions).
[0036] In the present invention, in the selenium-sulfur solution, S 2- with Se 2- The molar ratio of is preferably (0.2-5):1 and not 5:1, more preferably 1:5 or 3:3; the corresponding molar ratio of Se powder to Na2S is preferably (2.12-6.35):(1.41-7.05), more preferably 6.35:4.22.
[0037] After obtaining the selenium-sulfur solution, the present invention mixes Cu2O cubic powder and water, mixes the obtained suspension with the selenium-sulfur solution, performs selenization-sulfurization reaction, and obtains the S-doped hollow selenized copper box.
[0038] In the present invention, the method for preparing the Cu2O cubic powder preferably comprises: mixing copper salt, alkali, glucose and water, and reducing them to obtain the Cu2O cubic powder.
[0039] In the present invention, the copper salt preferably includes copper sulfate, more preferably copper sulfate pentahydrate; the alkali preferably includes sodium hydroxide.
[0040] In the present invention, the mass ratio of the copper salt, the base and the glucose is preferably 7.5:3.6:4.2.
[0041] The present invention preferably dissolves the copper salt in part of the water, and under the set reduction temperature condition, the copper salt is completely dissolved by stirring, the alkali is dissolved in the remaining water, the obtained alkali solution is added to the copper salt solution, and the stirring is continued for 5 minutes before adding glucose to carry out reduction.
[0042] In the present invention, the reduction temperature is preferably 70° C., and the time is preferably 30 min; and the reduction is preferably carried out under stirring conditions.
[0043] After the reduction is completed, the present invention preferably collects the obtained product by centrifugation, filters the excess liquid, washes the product with deionized water, and vacuum dries it at 50° C. for 12 h to obtain Cu2O cubic powder.
[0044] The present invention has no special limitation on the usage ratio of the Cu2O cubic powder and water, as long as the Cu2O cubic powder is fully dispersed and suspended; in an embodiment of the present invention, specifically 3.47 mmol Cu2O cubic powder is stirred and dispersed in 400 mL deionized water.
[0045] In the present invention, the molar ratio of the Cu2O cubic powder to the Se powder is preferably 3.47:(2.12-10.58), and more preferably 3.47:6.35.
[0046] In the present invention, the temperature of the selenization-sulfurization reaction is preferably room temperature, and the time is preferably 5 hours; the selenization-sulfurization reaction is preferably carried out under stirring conditions; the present invention has no special limitation on the stirring, and the reaction can be carried out smoothly according to the process well known in the art. In the process of the selenization-sulfurization reaction, the Cu2O cube acts as a sacrificial template, and the Na2Se in the selenium-sulfur solution plays the role of selenizing Cu2O to form copper selenide, while S 2- Doping penetration in Cu 2-x In the Se lattice, when the amount of S added is large, the excess S combines with Cu2O to form Cu 2-x S (copper sulfide).
[0047] After the selenization-sulfurization reaction is completed, the present invention preferably collects the product by suction filtration, then washes it with deionized water, and then vacuum dries the obtained product to obtain an S-doped hollow selenized copper box. The present invention has no particular limitation on the suction filtration and vacuum drying, and can be carried out according to processes well known in the art.
[0048] In the present invention, S not only participates in the regulation process in the form of a dopant, but also can control the S concentration to form a new phase. The S-induced new phase formation process is more prominent in the coordination of morphology, composition, heterogeneous interface, defect level and conductivity, resulting in excellent electromagnetic wave absorption performance of the material.
[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0050] Examples 1 to 3 and Comparative Example 1
[0051] Table 1 Raw material dosage and selenization time in different cases
[0052]
[0053] 7.5 g of CuSO4·5H2O was dissolved in 300 mL of deionized water and completely dissolved under stirring at 70°C. Then, 30 mL of the prepared NaOH solution (containing 3.6 g of NaOH) was added. After continuous stirring for 5 min, 4.2 g of glucose was added and the reaction was continued for 30 min. The product was collected by centrifugation, the excess liquid was filtered, and the product was washed with deionized water and vacuum dried at 50°C for 12 h to obtain Cu2O cubic powder.
[0054] Se powder (amount as shown in Table 1) and Na2S·9H2O (amount as shown in Table 1) were dissolved in 50 mL of NaOH solution (concentration as shown in Table 1), kept at 120°C for 4 h, cooled naturally to room temperature, and the excess Se powder was filtered to collect the alkaline selenium-sulfur solution;
[0055] 3.47 mmol of the prepared Cu2O cubic powder was added to 400 mL of deionized water to obtain a Cu2O suspension. The selenium-sulfur solution was added to the obtained Cu2O suspension under continuous stirring, and the mixture was stirred at room temperature for selenization (see Table 1 for the selenization time). The product was collected by filtration, washed with deionized water, and vacuum dried to obtain a hollow selenized copper box.
[0056] Characterization and performance testing
[0057] 1) Scanning electron microscopy (SEM, ZEISS sigma500) and transmission electron microscopy (TEM, FEI-Tecnai G2 F20) were used to observe the surface and internal morphology of the samples prepared in different embodiments. X-ray powder diffraction (XRD, UltimalV, Cu / Kα), TEM-SEAD mode and EDS-Mapping energy spectrum (BRUKER XFlash 6130) were used to analyze the phase and composition of the samples.
[0058] Figure 1 Figure a is the XRD pattern of S-doped copper selenide boxes (S1-S3) with different sulfur contents. Figure 1 b is the standard diffraction spectrum of CuSe, CuS and Cu7S4. Figure 1 It can be seen that when the molar ratio V(S 2-):V(Se 2- )=1:5, despite the introduction of S element, the diffraction peak of S1 is almost the same as the standard diffraction spectrum of CuSe, except that the peak corresponding to the {110} crystal plane is slightly shifted to a higher angle. This indicates that the lattice parameter of S-doped CuSe becomes smaller because part of Se (1.98A) in S1 is replaced by S (1.84A) with a smaller ionic radius. It can be foreseen that the introduction of S element may be beneficial to breaking the Cu 2-x The symmetry of Se lattice leads to the formation of lattice defects. The dipoles induced by these defects will act as polarization centers to enhance dielectric polarization loss. However, as the proportion of S element increases, the characteristic peaks of copper selenide partially disappear (marked by solid circles). 2- ):V(Se 2- )=3:3, a new diffraction peak appears at 29.74°, corresponding to the {090} crystal plane of Cu2S. It is worth noting that, on the one hand, the diffraction peak of S2 at 46.09° completely corresponds to the CuSe{110} crystal plane, and there is no shift in the diffraction peak, which indicates that there is almost no S ion replacing Se ion in S2. On the other hand, it is slightly shifted to a lower angle relative to the Cu2S{573} crystal plane, indicating that some S ions in Cu2S may be replaced by Se ions. Until V(S 2- ):V(Se 2- )=5:1, the peak of Cu2S completely disappears, and the remaining diffraction peaks and Cu 1.8 S characteristic peaks correspond well, indicating that Cu 2-x Cu2S in S successfully transitioned to Cu1.8S. Although S3 contained a small amount of Se, the diffraction peak of S3 did not shift significantly to a low angle, indicating that Se ions did not penetrate into Cu 1.8 S in the crystal lattice. This may be because the ionic radius of Se is too large, and it cannot smoothly replace the position of S when its concentration is very low, so it combines with Cu and exists independently as CuSe.
[0059] Figure 2 (ac) are Cu doped with different S contents 2-x The morphology of Se boxes (S1-S3), the small figure in the upper right corner of (ac) is the corresponding TEM image, the scale bar is 0.5μm; Figure 2 From ac, we can see that when V(S 2- ):V(Se 2- )=1:5, S1 is in the shape of a braided ball, with the surface composed of loosely stacked nanoshuttles, and its size is larger than that of the original Cu2O template. Its hollow part can be observed in TEM, but the hollow cavity is not obvious due to the thick shell. 2- ):V(Se 2-)=3:3, S2 is in perfect cubic shape, and both the morphology and size are well inherited from the original Cu2O template. Due to the thin shell, many cubic cross-sections are observed in the SEM image, and obvious hollow parts and similar small cubes in the cubic cavity can be observed in the TEM image. 2- ):V(Se 2- )=5:1, S3 is quasi-cube-shaped, with the face of the cube concave inwards, and there are also concave cubes in the inner cavity of the cube, which together form a double-shell cube. The formation of the hollow shell depends on the diffusion of copper ions outwards and the reaction with Se 2- or S 2- Combined with copper selenide (10 -48 ) than copper sulfide (10 -35 ) has a smaller solubility product constant, so copper selenide is easier to form than copper sulfide. It is speculated that the Kirkendall effect occurs twice in this process, driving the formation of copper selenide shell and copper sulfide shell respectively.
[0060] Figure 2 The (df) in the figure are the EDS mapping spectra of S1-S3 and the corresponding element statistics. The colored dot matrix confirms the uniformity of element distribution. It can be found that with the increase of S content, the Cu content increases and the Se content decreases. The atomic number ratios (S:Se) of S1-S3 are 0.11, 0.52 and 3.50, respectively, which are significantly smaller than the preset V(S 2- ):V(Se 2- ), which indicates that the priority of copper selenide in the reaction process is higher than that of copper sulfide, which is consistent with the solubility product mentioned above. In addition, in S1, the sum of S and Se elements is approximately equal to Cu, indicating that only CuS and CuSe exist in S1, and it is possible that S element partially replaces Se lattice. In addition, CuSe+Cu2S(S2) and CuSe+Cu 1.8 The combination pattern of S(S3) is also consistent with the element statistics in ef. The above results confirm the validity of XRD analysis.
[0061] 2) Determination of S-doped Cu by N2 adsorption-desorption method 2-x The specific surface area and pore size distribution of Se (S1-S3) are shown in Figure 3 , Figure 3 (ac) are the N2 adsorption and desorption curves of S1-S3, and the inset is the corresponding pore size distribution diagram; Figure 3 It can be seen that the three samples show type IV isotherms and the hysteresis loop is H3, indicating the presence of mesopores. The specific surface areas of S1-S3 are 29.41 m 2 / g, 58.99m 2 / g and 85.55m 2 / g, which is closely related to the degree of hollowing. According to the Barrrett Joyner-Halenda (BJH) model, the pore distribution range is 10-15nm.
[0062] Generally speaking, since metal selenides have better electronic conductivity than corresponding oxides or sulfides, the introduction of S may reduce the intrinsic conductivity of the product. However, for electromagnetic wave absorbing materials, it is necessary to mix the absorber and the matrix. The introduction of S elements in the cubic structure has a larger cavity volume and specific surface area, which reduces the particle density. Under the same filling mass, the volume fraction increases, it is easier to connect with each other, and it is easier to contact each other in the matrix to promote a conductive network, thereby improving the conductivity and showing stronger conductivity than selenide. This feature leads to a larger space to adjust electromagnetic parameters and optimize EMW absorption capacity.
[0063] 3) The complex dielectric constant of the sample at 2-18 GHz was measured using a vector network analyzer (VNA, PNA-N5234A). The sample powder was uniformly mixed with the paraffin matrix at different mass fractions and then pressed into a ring-shaped mold with an inner diameter of 3.04 mm and an outer diameter of 7.00 mm.
[0064] The copper selenide powder (T5) prepared in Comparative Example 1 and the samples S1 to S3 prepared in Examples 1 to 3 were filled in a paraffin matrix at different ratios to prepare sample / paraffin composite materials.
[0065] Figure 4 Where (ab) is the complex dielectric constant of T5, S1, S2 and S3 when the filling amount is 40wt%. Figure 4 As shown in (ab), compared with T5 / paraffin, after the introduction of S element, the ε′ of S1 / paraffin and S2 / paraffin decreased to a certain extent, which is beneficial to enhance their tanδ E And the ε″ value of S1 / paraffin shows an obvious dielectric resonance near 6.3GHz, which is attributed to the Cu 2-x Defects generated by S ion substitution in the Se lattice act as polarization centers and enhance polarization losses. In addition, it is also noted that the S3 / paraffin complex dielectric constant increases significantly, which may be attributed to two reasons. First, S3 has a significant double-shell structure and a large specific surface area, which is conducive to the construction of a conductive network and the response to electromagnetic waves. Second, the main component of S3 is Cu 1.8S, there are copper vacancies, forming a large number of electron holes in the energy band, making it have excellent conductivity. To further study the relationship between conductivity and dielectric loss, the conductivity of T1, S1, S2, S3 and paraffin composites was tested, which were 0.45S / m, 0.21S / m, 0.38S / m and 3.02S / m, respectively. The conductivity of S1 / paraffin is lower than that of T5 / paraffin, mainly because the intrinsic conductivity of the material decreases and the degree of hollowing decreases after sulfur doping. After that, the conductivity of the composite increases with the increase of the proportion of S element, which is related to the increase of the specific surface area of its microstructure. For most electromagnetic wave absorbing materials, the dielectric loss is determined by the polarization loss ε" P and conduction loss ε" C It consists of two parts. According to Debye theory, the calculation formula of ε″ value is as follows:
[0066]
[0067] Where ω is the angular frequency (ω = 2πf), τ is the relaxation time, σ is the conductivity (S / m), and ε0 is the free space dielectric constant (8.854×10 -12 F / m), ε ∞ and ε s They represent the dielectric constant in the high frequency limit and the static dielectric constant respectively.
[0068] Figure 4 (cd) is the ε of the composite materials of T5, S1, S2 and S3 with paraffin" C and ε" P Plotted against frequency, subtract ε" from ε" C The corresponding ε" P Value. Figure 4 From (cd), we can see that for T1 and S3, at the initial frequency (2GHz), their dielectric loss is almost entirely contributed by conductive loss. As the frequency increases, ε" P It gradually increases, which is due to the fact that the dielectric polarization cannot catch up with the alternating electric field at high frequency and relaxes. For S1 and S2, there is a certain polarization loss at 2GHz, which proves the existence of defect polarization caused by ion substitution, that is, part of Se is replaced by S or part of S is replaced by Se.
[0069] Figure 5 (a1, b1, c1) are the three-dimensional reflection loss diagrams of S1, S2, S3 and paraffin composite materials, (a2, b2, c2) are the two-dimensional reflection loss diagrams of S1, S2, S3 and paraffin composite materials, and (a3, b3, c3) are the effective bandwidth / reflection loss-thickness histograms of S1, S2, S3 and paraffin composite materials.
[0070] As we all know, when RL When the value exceeds -10dB, 90% of the electromagnetic waves can be dissipated by the absorber, which is called the effective absorption band (EAB). Figure 5 As shown, the R of S1 / paraffin Lmin At 2.7 mm, it is -46.3 dB, and the corresponding EAB is 3 GHz. With the doping of S elements, its structure evolves into a double-shell cube, and the R of S2 / paraffin Lmin The S1 has a good R L -Thickness stability, R in the range of 2.1-2.9mm L The values are all over -20dB. On the other hand, S2 shows good EAB-thickness stability, and its EAB value is over 4GHz in the range of 1.7-2.5mm. However, although S3 has a rare structure, its high conductivity prevents electromagnetic waves from entering the absorber, so it cannot effectively absorb electromagnetic waves.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for improving the electromagnetic wave absorption performance of a hollow copper selenide box, characterized in that: The following steps are involved: Se powder, Na2S and alkali solution are mixed and subjected to hydrothermal reaction to obtain a selenium-sulfur solution; Cu2O cubic powder and water are mixed, and the obtained suspension is mixed with a selenium-sulfur solution to perform a selenization-sulfurization reaction to obtain a S-doped hollow copper selenide box.
2. The method according to claim 1, characterized in that The usage ratio of the Se powder to the alkali solution is (2.12-6.35) mmol:50 mL; the concentration of the alkali solution is 10 mol / L.
3. The method according to claim 1, characterized in that The temperature of the hydrothermal reaction is 120° C. and the time is 4 hours.
4. The method according to claim 1, characterized in that: The preparation method of the Cu2O cubic powder comprises: mixing copper salt, alkali, glucose and water, and reducing them to obtain the Cu2O cubic powder.
5. The method according to claim 4, characterized in that The copper salt includes copper sulfate, and the alkali includes sodium hydroxide; the mass ratio of the copper salt, the alkali and the glucose is 7.5:3.6:4.
2.
6. The method according to claim 4 or 5, characterized in that: The reduction temperature is 70° C. and the time is 30 min.
7. The method according to claim 1, characterized in that In the selenium-sulfur solution, S 2- with Se 2- The molar ratio is (0.2-5):1 and not 5:
1.
8. The method according to claim 7, characterized in that In the selenium-sulfur solution, S 2- with Se 2- The molar ratio is 1:5 or 3:
3.
9. The method according to claim 1, characterized in that: The molar ratio of the Cu2O cubic powder to the Se powder is 3.47:(2.12-6.35).
10. The method according to claim 1, characterized in that The temperature of the selenization-sulfurization reaction is room temperature and the time is 5 hours.
Citation Information
Patent Citations
Selenium-copper composite spherical nano-particle with hollow structure as well as preparation method and application of selenium-copper composite spherical nano-particle
CN114870013A
Sulfur ion doped cuprous selenide honeycomb-shaped flexible nanosheet array structure material, preparation method and application of sulfur ion doped cuprous selenide honeycomb-shaped flexible nanosheet array structure material
CN115072674A
SU316649A1
Cited By
Electromagnetic composite absorbent with multi-interface hollow structure and preparation method thereof
CN119774553A
Electromagnetic composite absorber with multi-interface hollow structure and preparation method thereof
CN119774553B