Polyanion sodium battery positive electrode material as well as preparation method and application thereof

Through the solvent-thermal reaction of the high-boiling point organic solvent system, the nanoscale uniform dispersion and in-situ carbon coating of polyanionic sodium electropositive electrode materials are achieved, which solves the problem of large particle size and uneven distribution in the prior art, significantly improves sodium Electrochemical properties of ion batteries.

CN119038512AActive Publication Date: 2024-11-29CENT SOUTH UNIV

Patent Information

Application Number
CN202411150434.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing polyanionic sodium electropositive electrode material preparation process has large particle size and uneven distribution, making it difficult to achieve stable battery performance, especially low electronic conductivity, which affects electrochemical performance.

Method used

The solvent-thermal reaction is carried out using a high boiling point pure oil phase organic solvent system to achieve uniform dispersion of the precursor on the atomic scale, and the formation of nano-scale particles and in-situ carbon coating are achieved through the sintering process to improve the conductivity.

Benefits of technology

A nanoscale polyanionic sodium electropositive electrode material with uniform size distribution was prepared, which significantly improved the electrochemical performance of sodium ion batteries and expanded the scope of application of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038512A_ABST
    Figure CN119038512A_ABST
Patent Text Reader

Abstract

The invention provides a polyanion sodium battery positive electrode material and a preparation method and application thereof, and the preparation method comprises the following steps: mixing a polyanion source, a sodium source, a transition metal source and an organic solvent, and then carrying out solvothermal reaction to obtain a post-reaction liquid; the boiling point of the organic solvent is above 150 DEG C; precursor particles are separated from the reaction post-solution to obtain precursor particles coated with an organic solvent, and then the precursor particles coated with the organic solvent are sintered to obtain the polyanion sodium battery positive electrode material. According to the preparation method disclosed by the invention, the polyanion sodium battery positive electrode material is prepared based on a pure oil phase system, uniform dispersion of a precursor on an atomic scale can be realized, and the nano-scale uniformly dispersed polyanion sodium battery positive electrode material is prepared, so that the electrochemical performance of a sodium ion battery can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a polyanion sodium positive electrode material and a preparation method and application thereof. Background Art

[0002] The cathode materials of sodium-ion batteries include layered oxide cathode materials, polyanion cathode materials and Prussian blue cathode materials. Among them, polyanion sodium cathode materials are rich in variety, cost-controlled, simple in synthesis process, and have high chemical stability, thermal stability and electrochemical stability, and can achieve higher specific capacity and energy density. However, polyanion sodium cathode materials generally have the disadvantage of low electronic conductivity, and generally need to be carbon coated or the grain size reduced to improve their electrochemical performance.

[0003] At present, the preparation process of polyanion sodium positive electrode materials mainly includes sol-gel method and solid phase method. In the sol-gel method, the precursor material is first dissolved in a solvent to form a liquid precursor, and then a sol and a gel are prepared after a series of processes, and finally an electrode product is obtained by calcination. For example, CN 116666608A discloses a high entropy polyanion sodium ion battery positive electrode material and a preparation method thereof, which comprises the following steps: step 1, mixing a sodium source, a transition metal source, a phosphorus source, a carbon source and water, and obtaining a uniformly dispersed solution by stirring various element sources to obtain a first mixed system; step 2, placing the first mixed system in an oil bath for heating and reflux, obtaining a precursor by the sol-gel method, and drying the precursor; step 3, sintering the dried precursor for the first time to obtain a second mixed system, and the second mixed system is treated by ball milling to reduce the particle size; step 4, sintering the second mixed system after ball milling for the second time, and obtaining a high entropy phosphate positive electrode material after the second sintering.

[0004] The solid phase method is to mix the precursor materials evenly and then directly perform high-temperature calcination to prepare the electrode material; for example, CN114156452A discloses a sodium ion positive electrode material, its preparation method and use, the preparation method comprising: mixing a sodium source, a manganese source, an aluminum source, a phosphorus source and a carbon source, and sintering the mixed materials under a protective atmosphere to obtain the sodium ion positive electrode material; wherein the sodium ion positive electrode material comprises an inner core and a carbon coating layer located on the surface of the inner core; the chemical formula of the inner core is Na4MnAl(PO4)3; the elemental molar ratio of manganese, aluminum and phosphorus in the manganese source, aluminum source and phosphorus source is consistent with the stoichiometric ratio of Na4MnAl(PO4)3, and the polyanionic compound Na4MnAl(PO4)3 is prepared by the solid phase method.

[0005] However, the particles obtained by the sol-gel method and the solid phase method are large in size and uneven in size distribution, making it difficult to achieve stable battery performance. Therefore, it is necessary to develop a method for preparing nanoscale polyanion sodium cathode materials with uniform size distribution and ensure that the electrode materials have high electrical conductivity, thereby showing excellent electrochemical performance. Summary of the invention

[0006] The object of the present invention is to provide a polyanion sodium cathode material and a preparation method and application thereof. The preparation method prepares the polyanion sodium cathode material based on a pure oil phase system, can achieve uniform dispersion of the precursor at the atomic scale, and prepare a nano-scale uniformly dispersed polyanion sodium cathode material, thereby effectively improving the electrochemical performance of a sodium ion battery.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a polyanion sodium positive electrode material, the preparation method comprising the following steps:

[0009] (1) mixing a polyanion source, a sodium source, a transition metal source and an organic solvent, and then performing a solvothermal reaction to obtain a reaction solution;

[0010] The boiling point of the organic solvent is above 150°C;

[0011] (2) Separating precursor particles from the reaction liquid in step (1) to obtain precursor particles coated with an organic solvent, and then sintering the precursor particles coated with an organic solvent to obtain the polyanion sodium cathode material.

[0012] The present invention adopts a high-boiling point pure oil phase organic solvent system to prepare the polyanion sodium cathode material, rather than a traditional water phase system. During solvent thermal treatment, atomic-level dispersion can be achieved, which is beneficial to the formation of high-quality products in the sintering process. The sample obtained after sintering is nano-scale particles with uniform size distribution, which ensures that the material has a high electrical conductivity and greatly improves the electrochemical performance of the polyanion sodium cathode material.

[0013] In addition, the present invention adopts a high-boiling point organic solvent system to carry out a solvothermal reaction, and can obtain precursor particles coated with an organic solvent. The residual organic solvent realizes in-situ carbon coating during the subsequent sintering process, further improving the electrical conductivity of the material. At the same time, the preparation method of the present invention has high universality and can prepare different types of polyanionic sodium cathode materials.

[0014] The boiling point of the organic solvent is above 150°C, for example, it can be 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] Preferably, the organic solvent in step (1) comprises any one of fatty amines, fatty acids, chain olefins or phenyl ether compounds, or a combination of at least two thereof, preferably a combination of fatty amines and fatty acids.

[0016] Preferably, the fatty amine comprises oleylamine and / or octadecylamine, preferably oleylamine.

[0017] Preferably, the fatty acid comprises oleic acid.

[0018] Preferably, the chain olefin includes a C15-C25 straight chain olefin, for example, C15, C18, C20, C22 or C25, preferably octadecene.

[0019] Preferably, the phenyl ether compound includes diphenyl ether.

[0020] Preferably, the organic solvent in step (1) comprises any one of oleylamine, oleic acid, octadecylamine, octadecene, and diphenyl ether, or a combination of at least two thereof, preferably a combination of oleylamine and oleic acid.

[0021] The invention adopts a high boiling point organic solvent for preparation, especially oleylamine and / or oleic acid. Oleylamine has reducing property and can effectively reduce trivalent iron in the iron source. Oleylamine or oleic acid has a high boiling point and can stably exist in the solvent thermal reaction and can act as a capping agent to control the grain size at the nanometer scale. Oleylamine or oleic acid has a certain surfactant effect and can make each precursor material uniformly dispersed in the solvent.

[0022] Preferably, the organic solvent in step (1) comprises a fatty amine and a fatty acid in a volume ratio of (2.5-10):1, for example, it can be 2.5:1, 3.5:1, 4.5:1, 5.5:1, 6.5:1, 7.5:1, 8.5:1, 9.5:1 or 10:1, preferably oleylamine and oleic acid in a volume ratio of (2.5-5):1, for example, it can be 2.5:1, 3.5:1, 4.5:1 or 5:1, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0023] The present invention preferably uses oleylamine and oleic acid in a specific ratio. If the oleylamine is too little and the oleic acid is too much, the cost will be too high and the reaction process will be too violent, which may easily cause the reaction liquid to escape. If the oleylamine is too much and the oleic acid is too little, the precursors will not be mixed evenly during the reaction, and high-quality positive electrode materials cannot be obtained by subsequent sintering.

[0024] Preferably, the molar amount of the organic solvent added in step (1) is 30-45 times the theoretical molar amount of the polyanion sodium cathode material, for example, it can be 30 times, 35 times, 40 times or 45 times, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, conductive carbon is also added during the mixing in step (1).

[0026] Preferably, the conductive carbon includes any one of carbon nanotubes, Super P, Ketjen black, acetylene black or graphene, or a combination of at least two thereof.

[0027] Preferably, the added amount of the conductive carbon is 10-20wt% of the theoretical amount of the polyanion sodium cathode material, for example, it can be 10wt%, 15wt% or 20wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the polyanion source in step (1) comprises any one of a phosphorus source, a sulfur source, a fluorine source, a silicon source or a boron source, or a combination of at least two of them.

[0029] Preferably, the phosphorus source includes any one of diammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate or phosphoric acid, or a combination of at least two thereof.

[0030] Preferably, the sulfur source includes any one of ammonium bisulfate, sodium bisulfate, sodium sulfate, sulfuric acid or vanadyl sulfate, or a combination of at least two thereof.

[0031] Preferably, the fluorine source includes any one of hydrofluoric acid, sodium fluoride or ammonium fluoride, or a combination of at least two of them.

[0032] Preferably, the silicon source comprises sodium silicate and / or silicic acid.

[0033] Preferably, the boron source includes any one of sodium tetraborate, boric acid or ammonium borate, or a combination of at least two thereof.

[0034] Preferably, the sodium source in step (1) comprises any one of sodium oleate, sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium bisulfate, sodium sulfate, sodium fluoride, sodium oxalate, sodium acetate, sodium formate, sodium citrate or sodium hydroxide, or a combination of at least two thereof, preferably sodium oleate.

[0035] Preferably, the transition metal source in step (1) comprises any one of an iron source, a vanadium source, a titanium source or a manganese source, or a combination of at least two thereof.

[0036] Preferably, the iron source includes any one of ferric acetylacetonate, ferric nitrate, ferrous nitrate, ferric phosphate, ferrous phosphate, ferrous acetylacetonate, ferrous oxalate, ferrous carbonate, ferrous sulfate or ferrous sulfate, or a combination of at least two thereof.

[0037] Preferably, the vanadium source includes any one of vanadium acetylacetonate, vanadyl acetylacetonate, sodium metavanadate, ammonium metavanadate, sodium orthovanadate, vanadyl oxalate or vanadyl sulfate, or a combination of at least two thereof.

[0038] Preferably, the titanium source includes any one of titanium acetylacetonate, metatitanic acid, titanium sulfate, titanium isopropoxide, tetraethyl titanate or tetrabutyl titanate, or a combination of at least two thereof.

[0039] Preferably, the manganese source includes any one of manganese acetylacetonate, manganese carbonate, manganese sulfate or manganese acetate, or a combination of at least two thereof.

[0040] Preferably, the mixing temperature in step (1) is 20-180°C, for example, 20°C, 50°C, 80°C, 100°C, 125°C, 150°C or 180°C, and the mixing time is 5-300 min, for example, 10 min, 30 min, 50 min, 70 min, 100 min, 125 min, 150 min, 175 min, 200 min, 225 min, 250 min, 275 min or 300 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, the temperature of the solvent thermal reaction in step (1) is 180-300°C, for example, 180°C, 200°C, 250°C or 300°C, and the time is 5-300min, for example, 10min, 30min, 50min, 70min, 100min, 125min, 150min, 175min, 200min, 225min, 250min, 275min or 300min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the solvent thermal reaction includes two heating stages or three heating stages. When it includes two heating stages, the first insulation stage is heated to 100-140°C, such as 100°C, 120°C or 140°C, and then kept warm for 10-30min, such as 10min, 20min or 30min. The second insulation stage is heated to 250-270°C, such as 250°C, 260°C or 270°C, and then kept warm for 30-60min, such as 30min, 40min, 50min or 60min, and then cooled to room temperature.

[0043] Preferably, the solvent thermal reaction includes two heating stages or three heating stages. When it includes three heating stages, the first insulation section is heated to 110-130°C, for example, 110°C, 120°C or 130°C, and then kept warm for 10-30min, for example, 10min, 20min or 30min. The second insulation section is heated to 170-190°C, for example, 170°C, 180°C or 190°C, and then kept warm for 10-30min, for example, 10min, 20min or 30min. The third insulation section is heated to 250-270°C, for example, 250°C, 260°C or 270°C, and then kept warm for 10-30min, for example, 10min, 20min or 30min, and then cooled to room temperature.

[0044] Preferably, the method of separating the precursor particles in step (2) comprises mixing the reaction liquid with an alcohol solvent, solid-liquid separation and drying.

[0045] Preferably, the solid-liquid separation method includes centrifugation, the centrifugal speed is 11000-13000 rpm, for example, it can be 11000 rpm, 12000 rpm or 13000 rpm, and the centrifugal time is 3-10 min, for example, it can be 3 min, 5 min, 7 min or 10 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] Preferably, the drying includes drying at 40-60°C, such as 40°C, 50°C or 60°C, and vacuum drying for 1-3h, such as 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the alcohol solvent includes ethanol.

[0048] Preferably, the sintering temperature in step (2) is 300-800°C, for example, 300°C, 400°C, 500°C, 600°C, 700°C or 800°C, and the sintering time is 1-30h, for example, 1h, 5h, 10h, 15h, 20h, 25h or 30h, and is carried out in a protective gas.

[0049] Preferably, the sintering in step (2) is first carried out at a temperature of 300-350°C, such as 300°C, 325°C or 350°C, for 1-3h, such as 1h, 2h or 3h, and then at a temperature of 500-600°C, such as 500°C, 550°C or 600°C, for 5-8h, such as 5h, 6h, 7h or 8h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0051] (1) adding a polyanion source, a sodium source, a transition metal source and conductive carbon to an organic solvent according to the formula amount, stirring at a temperature of 20-180° C. for 5-300 minutes, and then performing a solvothermal reaction at 180-300° C. for 5-300 minutes to obtain a reaction liquid;

[0052] The organic solvent has a boiling point of above 150° C. and includes any one of oleylamine, oleic acid, octadecylamine, octadecene or diphenyl ether, or a combination of at least two thereof;

[0053] (2) pouring the reaction liquid of step (1) into an alcohol solvent, separating the solid and the liquid and drying, to obtain the organic solvent-coated precursor particles, and then sintering the organic solvent-coated precursor particles in a protective gas at a temperature of 300-800° C. for 1-30 h to obtain the polyanion sodium cathode material.

[0054] In a second aspect, the present invention provides a polyanion sodium cathode material, wherein the polyanion sodium cathode material is prepared by the preparation method described in the first aspect.

[0055] Preferably, the polyanion sodium cathode material includes sodium ferric sulfate, composite sodium ferric phosphate, sodium ferric fluorophosphate, sodium ferric phosphate, sodium vanadium phosphate, sodium ferric orthosilicate or sodium ferric pentaborate.

[0056] In a third aspect, the present invention provides a sodium ion battery, wherein the sodium ion battery comprises the polyanion sodium cathode material as described in the second aspect.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] (1) The present invention adopts a high boiling point organic solvent for preparation, and can achieve atomic-level dispersion during the solvent thermal treatment of the precursor material, which is conducive to the formation of high-quality products in the sintering process;

[0059] (2) The sample obtained after sintering in the present invention is a nano-scale particle with uniform size distribution, which can greatly improve the electrochemical performance of the polyanion sodium cathode material;

[0060] (3) The residual organic solvent of the present invention can form an in-situ carbon coating during the sintering process, further improving the electrical conductivity of the material;

[0061] (4) The preparation method of the present invention has a wide range of applications and can be used to prepare polyanionic sodium positive electrode materials including sulfates, composite phosphates, fluorophosphates, phosphates, sodium iron phosphates, sodium vanadium phosphates, sodium iron orthosilicate or sodium iron pentaborate. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is the XRD diagram of the polyanion sodium cathode material described in Example 1 of the present invention;

[0063] Figure 2 This is a TEM image of the polyanion sodium cathode material described in Example 1 of the present invention;

[0064] Figure 3 This is a rate performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Examples 1 and 4 of the present invention;

[0065] Figure 4 This is a cycle performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Example 1 of the present invention;

[0066] Figure 5 This is the XRD diagram of the polyanion sodium cathode material described in Example 2 of the present invention;

[0067] Figure 6 This is a TEM image of the polyanion sodium cathode material described in Example 2 of the present invention;

[0068] Figure 7 This is a rate performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Example 2 and Example 11 of the present invention;

[0069] Figure 8 This is a cycle performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Example 2 of the present invention;

[0070] Fig. 9 This is the XRD diagram of the polyanion sodium positive electrode material described in Example 3 of the present invention;

[0071] Fig.10 This is a TEM image of the polyanion sodium cathode material described in Example 3 of the present invention;

[0072] Fig.11 This is a rate performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Examples 3 and 13 of the present invention;

[0073] Fig.12 This is a cycle performance diagram of a button-type half-cell made of the polyanion sodium cathode material described in Example 3 of the present invention. DETAILED DESCRIPTION

[0074] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0075] Example 1

[0076] This embodiment provides a method for preparing a polyanion sodium cathode material, wherein the polyanion sodium cathode material is Na4Fe3(PO4)2(P2O7) / C / MWCNTs, wherein C is coated on the surface of Na4Fe3(PO4)2(P2O7), and MWCNTs are doped in Na4Fe3(PO4)2(P2O7), and the preparation method comprises the following steps:

[0077] (1) Add 2.3996 g NaH2PO4 (20 mmol), 5.2976 g Fe(acac)3 (15 mmol) and 0.328 g MWCNTs (10 wt% of polyanionic sodium cathode material) into a 250 mL four-necked flask, then add 50 mL oleylamine, and stir at 20°C for 300 min to mix evenly;

[0078] (2) In a N2 atmosphere at a flow rate of 0.5 L / min, the mixture was purged for 10 min, then heated to 120°C and kept warm for 30 min, then heated to 250°C and kept warm for 30 min. After the insulation was completed, a uniform solution was obtained;

[0079] (3) The obtained solution was cooled to room temperature and poured into a beaker containing 200 mL of ethanol, and the prepared nanoparticles were uniformly precipitated. The solid sample was then obtained by centrifugation at 12000 rpm for 5 min. The obtained solid sample was placed in a vacuum dryer at 40° C. for 2 h to obtain nanoparticles uniformly coated with oleylamine.

[0080] (4) transferring the dried solid sample to a tube furnace, heating the sample to 300° C. at a heating rate of 10° C. / min in an Ar atmosphere for low-temperature pre-calcination, holding the sample at this temperature for 1 h, then heating the sample to 550° C. at a heating rate of 10° C. / min for high-temperature calcination, holding the sample at this temperature for 10 h, and cooling the sample to room temperature to obtain the polyanion sodium positive electrode material;

[0081] The XRD pattern of the polyanion sodium positive electrode material in this embodiment is as follows: Figure 1 As shown in the TEM image Figure 2 As shown, the rate performance diagram of the button half-cell is as follows Figure 3 As shown, the cycle performance diagram of the button half-cell is as follows Figure 4 shown.

[0082] Example 2

[0083] This embodiment provides a method for preparing a polyanion sodium cathode material, wherein the polyanion sodium cathode material is Na2FePO4F / C / MWCNTs, wherein C is coated on the surface of Na2FePO4F, and MWCNTs are doped in Na2FePO4F. The preparation method comprises the following steps:

[0084] (1) In a 250 mL four-necked flask, 0.5751 g NH4H2PO4 (5 mmol), 3.0444 g sodium oleate (10 mmol), 1.7659 g Fe(acac)3 (5 mmol) and 0.216 g MWCNTs (20 wt% of polyanionic sodium cathode material) were added, and then 50 mL oleylamine, 15 mL oleic acid and 172 uL 49% HF (5 mmol) were added, and the mixture was stirred at 175 ° C for 5 min to mix well;

[0085] The volume ratio of oleylamine to oleic acid is 3.33:1;

[0086] (2) In a N2 atmosphere at a flow rate of 0.5 L / min, the mixture was purged for 10 min, then heated to 180°C and kept warm for 30 min, then heated to 250°C and kept warm for 30 min. After the insulation was completed, a uniform solution was obtained;

[0087] (3) The obtained solution was cooled to room temperature and poured into a beaker containing 150 mL of ethanol, and the prepared nanoparticles were uniformly precipitated. The solid sample was then centrifuged at 12000 rpm for 5 min to obtain a solid sample. The obtained solid sample was placed in a vacuum dryer at 40° C. for 2 h to obtain nanoparticles uniformly coated with oleylamine and oleic acid.

[0088] (4) transferring the dried solid sample to a tube furnace, heating the sample to 300°C at a heating rate of 10°C / min in an Ar atmosphere for low-temperature pre-calcination, keeping the temperature for 1 hour, and then heating the sample to 550°C at a heating rate of 10°C / min for high-temperature calcination, keeping the temperature for 5 hours, and cooling the sample to room temperature to obtain a polyanion sodium cathode material;

[0089] The XRD pattern of the polyanion sodium positive electrode material in this embodiment is as follows: Figure 5 As shown in the TEM image Figure 6 As shown, the rate performance diagram of the button half-cell is as follows Figure 7 As shown, the cycle performance diagram of the button half-cell is as follows Figure 8 shown.

[0090] Example 3

[0091] This embodiment provides a method for preparing a polyanion sodium cathode material, wherein the polyanion sodium cathode material is Na2Fe2(SO4)3 / C / MWCNTs, wherein C is coated on the surface of Na2Fe2(SO4)3, and MWCNTs are doped in Na2Fe2(SO4)3. The preparation method comprises the following steps:

[0092] (1) In a 250 mL four-necked flask, 0.691 g NH4HSO4 (6 mmol), 1.218 g sodium oleate (4 mmol), 1.4127 g Fe(acac)3 (4 mmol) and 0.0892 g MWCNTs (10 wt% of polyanionic sodium cathode material) were added, followed by 50 mL oleylamine and 15 mL oleic acid, and the mixture was stirred at 25 °C for 100 min to mix well;

[0093] The volume ratio of oleylamine to oleic acid is 3.33:1;

[0094] (2) In a N2 atmosphere at a flow rate of 0.5 L / min, the mixture was purged for 10 min, then heated to 120°C and kept warm for 30 min, then heated to 180°C and kept warm for 30 min, and finally heated to 250°C and kept warm for 30 min. After the insulation was completed, a uniform solution was obtained;

[0095] (3) The resulting solution was cooled to room temperature and poured into a beaker containing 125 mL of ethanol. The prepared nanoparticles were uniformly precipitated, and then a solid sample was obtained by centrifugation at 12,000 rpm for 5 min. The obtained solid sample was placed in a vacuum dryer at 40° C. for 2 h to obtain nanoparticles uniformly coated with oleylamine and oleic acid.

[0096] (4) transferring the dried solid sample to a tube furnace, heating the sample to 370° C. at a heating rate of 5° C. / min in an Ar atmosphere for low-temperature calcination, holding the sample for 10 h, and cooling the sample to room temperature to obtain the polyanion sodium cathode material;

[0097] The XRD pattern of the polyanion sodium positive electrode material in this embodiment is as follows: Fig. 9 As shown in the TEM image Fig.10 As shown, the rate performance diagram of the button half-cell is as follows Fig.11 As shown, the cycle performance diagram of the button half-cell is as follows Fig.12 shown.

[0098] Example 4

[0099] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of embodiment 1 except that MWCNTs are not added in step (1) to make the adaptability of the obtained polyanion sodium cathode material change.

[0100] The rate performance diagram of the button half-cell made of the polyanion sodium positive electrode material described in this embodiment is as follows: Figure 3 shown.

[0101] Example 5

[0102] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 1 except that an equal volume of oleylamine in step (1) is replaced by oleic acid.

[0103] Example 6

[0104] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 1 except that the volume of oleylamine in step (1) is replaced by octadecylamine.

[0105] Example 7

[0106] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 1 except that an equal volume of oleylamine in step (1) is replaced by octadecene.

[0107] Example 8

[0108] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 1 except that an equal volume of oleylamine in step (1) is replaced by diphenyl ether.

[0109] Example 9

[0110] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 2 except that the volume of oleic acid in step (1) is 10 mL and the volume ratio of oleylamine to oleic acid is 5:1.

[0111] Example 10

[0112] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Embodiment 2 except that the volume of oleic acid in step (1) is 20 mL and the volume ratio of oleylamine to oleic acid is 2.5:1.

[0113] Embodiment 11

[0114] This embodiment provides a method for preparing a polyanion sodium cathode material, the preparation method is the same as that of embodiment 2 except that the volume of oleic acid in step (1) is 5 mL and the volume ratio of oleylamine to oleic acid is 10:1;

[0115] The rate performance diagram of the button half-cell made of the polyanion sodium positive electrode material described in this embodiment is as follows: Figure 7 shown.

[0116] Example 12

[0117] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of Example 2 except that the volume of oleic acid in step (1) is 25 mL and the volume ratio of oleylamine to oleic acid is 2:1.

[0118] Example 13

[0119] This embodiment provides a method for preparing a polyanion sodium cathode material. The preparation method is the same as that of embodiment 3 except that MWCNTs are not added in step (1) to adapt the obtained polyanion sodium cathode material.

[0120] The rate performance diagram of the button half-cell made of the polyanion sodium positive electrode material described in this embodiment is as follows: Fig.11 shown.

[0121] Comparative Example 1

[0122] This comparative example provides a method for preparing a polyanion sodium cathode material, wherein the preparation method is the same as that of Example 1 except that the volume of oleylamine in step (1) is replaced by ethanol;

[0123] In this comparative example, all the ethanol evaporated and the corresponding precursor particles could not be separated.

[0124] Comparative Example 2

[0125] This comparative example provides a method for preparing a polyanion sodium positive electrode material, which is the same as Example 1 except that the volume of oleylamine in step (1) is replaced by water;

[0126] In this comparative example, a large amount of water evaporates and the corresponding precursor particles cannot be separated.

[0127] The polyanion sodium positive electrode material, conductive agent (Super P), and binder (PVDF) obtained in the above embodiments and comparative examples are coated with slurry in a ratio of 8:1:1, and button batteries are assembled in a glove box with water and oxygen less than 0.01 ppm, wherein metallic sodium is used as the negative electrode, the electrolyte used in Examples 3 and 13 is 1M NaClO4 in EC:PC (1:1 vol%) with 5% FEC, and the electrolyte used in the remaining embodiments is 1M NaPF6in EC:PC (1:1 vol%) with 5% FEC, and the diaphragm is a glass fiber membrane.

[0128] The prepared button cell was subjected to cycle performance and rate performance tests at a constant temperature of 30°C, and the voltage window and current density were Figure 3 , Figure 4 , Figure 7 , Figure 8 , Fig.11 and Fig.12 As shown in the table 1, the test results are shown in Table 1:

[0129] Table 1

[0130]

[0131] From Table 1 we can see that:

[0132] It can be seen from Example 1 that the present invention uses a pure phase high-boiling point organic solvent not only to obtain nano-scale particles with uniform size distribution, but also to make the organic solvent as a carbon source coated on the surface of the particles to prepare a polyanion sodium cathode material with excellent performance; it can be seen from Example 1 and Example 4, Example 3 and Example 13 that the present invention preferably also adds conductive carbon during the preparation process, so as to further improve the conductivity of the material; it can be seen from Example 1 and Examples 5-8 that the type of organic solvent of the present invention will affect the performance of the polyanion sodium cathode material; it can be seen from Examples 2 and Examples 9-12 that the present invention preferably uses an oleylamine + oleic acid system, and the mass ratio of the two will affect the uniformity of particle distribution, thereby affecting the performance of the product.

[0133] In summary, the present invention provides a polyanion sodium cathode material and a preparation method and application thereof. The preparation method prepares the polyanion sodium cathode material based on a pure oil phase system, can achieve uniform dispersion of the precursor salt at the atomic scale, and prepare a nanoscale uniformly dispersed polyanion sodium cathode material, thereby effectively improving the electrochemical performance of sodium ion batteries.

[0134] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a polyanion sodium positive electrode material, It is characterized in that The preparation method comprises the following steps: (1) mixing a polyanion source, a sodium source, a transition metal source and an organic solvent, and then performing a solvothermal reaction to obtain a reaction solution; The boiling point of the organic solvent is above 150°C; (2) Separating precursor particles from the reaction liquid in step (1) to obtain precursor particles coated with an organic solvent, and then sintering the precursor particles coated with an organic solvent to obtain the polyanion sodium cathode material.

2. The preparation method according to claim 1, It is characterized in that The organic solvent in step (1) comprises any one or a combination of at least two of aliphatic amines, fatty acids, chain olefins or phenyl ether compounds, preferably a combination of aliphatic amines and fatty acids; Preferably, the fatty amine comprises oleylamine and / or octadecylamine, preferably oleylamine; Preferably, the fatty acid comprises oleic acid; Preferably, the chain olefin comprises a C15-C25 straight chain olefin, preferably octadecene; Preferably, the phenyl ether compound includes diphenyl ether.

3. The preparation method according to claim 1 or 2, It is characterized in that The organic solvent in step (1) comprises a fatty amine and a fatty acid in a volume ratio of (2.5-10):1, preferably oleylamine and oleic acid in a volume ratio of (2.5-5):1; Preferably, the molar amount of the organic solvent added in step (1) is 30-45 times the theoretical molar amount of the polyanion sodium cathode material; Preferably, conductive carbon is also added during the mixing in step (1); Preferably, the conductive carbon comprises any one of carbon nanotubes, Super P, Ketjen black, acetylene black or graphene, or a combination of at least two thereof; Preferably, the added amount of the conductive carbon is 10-20 wt % of the theoretical amount of the polyanion sodium positive electrode material.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The polyanion source in step (1) comprises any one of a phosphorus source, a sulfur source, a fluorine source, a silicon source or a boron source, or a combination of at least two thereof; Preferably, the sodium source in step (1) comprises any one of sodium oleate, sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium bisulfate, sodium sulfate, sodium fluoride, sodium oxalate, sodium acetate, sodium formate, sodium citrate or sodium hydroxide, or a combination of at least two thereof; Preferably, the transition metal source in step (1) comprises any one of an iron source, a vanadium source, a titanium source or a manganese source, or a combination of at least two thereof.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The mixing temperature in step (1) is 20-180° C. and the mixing time is 5-300 min. Preferably, the temperature of the solvent thermal reaction in step (1) is 180-300° C. and the time is 5-300 min.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The method of separating the precursor particles in step (2) includes mixing the reaction liquid with an alcohol solvent, solid-liquid separation and drying; Preferably, the sintering in step (2) is carried out at a temperature of 300-800° C. for a time of 1-30 h in a protective gas atmosphere.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: (1) adding a polyanion source, a sodium source, a transition metal source and conductive carbon to an organic solvent according to the formula amount, stirring at a temperature of 20-180° C. for 5-300 minutes, and then performing a solvothermal reaction at 180-300° C. for 5-300 minutes to obtain a reaction liquid; The organic solvent has a boiling point above 150° C. and includes any one or a combination of at least two of aliphatic amines, fatty acids, chain olefins or phenyl ether compounds; (2) pouring the reaction liquid of step (1) into an alcohol solvent, separating the solid and the liquid and drying, to obtain the organic solvent-coated precursor particles, and then sintering the organic solvent-coated precursor particles in a protective gas at a temperature of 300-800° C. for 1-30 h to obtain the polyanion sodium cathode material.

8. A polyanion sodium cathode material, It is characterized in that The polyanion sodium cathode material is prepared by the preparation method according to any one of claims 1 to 7.

9. The polyanion sodium positive electrode material according to claim 8, It is characterized in that The polyanion sodium positive electrode material includes any one of composite sodium iron phosphate, sodium iron sulfate, sodium iron fluorophosphate, sodium iron phosphate, sodium vanadium phosphate, sodium iron orthosilicate or sodium iron pentaborate.

10. A sodium ion battery, It is characterized in that The sodium ion battery comprises the polyanion sodium cathode material as claimed in claim 8 or 9.

Citation Information

Patent Citations

  • Method for preparing polyanionic lithium ion battery anode material

    CN101794878A

  • High-rate lithium vanadium phosphate positive electrode material, and preparation method and application thereof

    CN105406071A

  • Carbon-cladded sodium ferric pyrophosphate material and preparation method thereof as well application of carbon-cladded sodium ferric pyrophosphate material serving as sodium-ion battery positive electrode material

    CN108123129A

  • Low-temperature sodium ion battery positive electrode material, preparation method and battery

    CN117613256A

Cited By

  • Anion-doped sodium ferric sulfate positive electrode material for sodium ion battery as well as preparation method and application of anion-doped sodium ferric sulfate positive electrode material

    CN121097072A