Rare earth aluminosilicate microcrystalline glass and preparation method thereof
By controlling the addition of oxide components and rare earth oxides in the microcrystalline glass, zirconium dioxide nanocrystallines are formed, which solves the problem of excessive lithium and aluminum content, and achieves low cost of rare earth aluminosilicate microcrystalline glass. High light transmittance and excellent mechanical properties, suitable for touch displays.
Patent Information
- Application Number
- CN202411162392.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
While the existing microcrystalline glasses improve light transmittance and mechanical properties, the excessive content of lithium and aluminum elements leads to an increase in production costs and poor transparency, making it difficult to meet the needs of touch display screens.
Rare earth aluminosilicate microcrystalline glass is used to control the mole percentage of SiO2, Al2O3, Na2O, Li2O, ZrO2, MgO and K2O to form zirconium dioxide nanocrystals, combined with rare earth oxides, reduce the content of lithium and aluminum elements, and increase the glass. light transmittance and mechanical properties.
It realizes the low cost, high light transmittance, excellent Vickers hardness and fracture toughness of rare earth aluminosilicate glass, and is suitable for touch display screens, meeting the application needs of electronic products.
Smart Images

Figure CN119038879A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass products, and in particular to a rare earth aluminosilicate glass-ceramic and a preparation method thereof. Background Art
[0002] Glass is a transparent material that can effectively transmit light and has excellent corrosion resistance, making it an ideal choice for manufacturing products such as windows, mirrors and displays. However, traditional glass usually has disadvantages such as fragility and poor scratch resistance, which limits its scope of use. With the development of science and technology, electronic products are becoming more and more popular, especially in recent decades, electronic devices such as mobile phones and tablets have become a necessity in people's lives. These electronic devices are equipped with touch screens with cover glass. Demand drives technological progress, and people's performance requirements for touch screens are also increasing.
[0003] Among cover glass, the main types are alkali-aluminosilicate glass, such as sodium-aluminosilicate glass and lithium-aluminosilicate glass. Among them, lithium-aluminosilicate glass has a lower glass transition temperature Tg. At the same time, lithium-aluminosilicate glass can be chemically strengthened by ion exchange, thereby greatly improving its strength. At present, the surface compressive stress and the depth of the ion exchange layer of alkali-aluminosilicate glass are mainly improved by adjusting and optimizing the components of the glass and the formula of chemical strengthening, but it still cannot meet the increasing application demand of touch screens of electronic products.
[0004] Glass-ceramic, also known as glass ceramics, is a special glass composed of a microcrystalline phase and a residual glass phase, with a dual phase of microcrystalline structure and amorphous structure. The preparation of glass-ceramic can be regarded as the synthesis of crystals by controlling solid-state reactions in supercooled glass. This solid-state reaction can be triggered by high temperature, i.e., heat treatment. It is also possible to induce glass crystallization at a lower temperature by adding nucleating agents such as TiO2, ZrO2, and precious metal nanoparticles, using heterogeneous nucleation. This allows the glass to precipitate uniform and fine crystals, thereby improving the hardness, fracture toughness, and drop resistance of the glass.
[0005] For touch screens, the microcrystalline glass used must have a high light transmittance. At present, the existing suitable microcrystalline glass systems mainly include lithium aluminum silicate microcrystalline glass, magnesium / zinc aluminum silicate microcrystalline glass (spinel), etc. Ion exchange is mainly carried out through lithium-sodium, lithium-potassium and sodium-potassium, using larger ions to exchange smaller ions, so that compressive stress is generated at the ion exchange point, inhibiting the expansion of microcracks on the glass surface, and improving properties such as hardness and fracture toughness. As for transparent microcrystalline glass, although it has higher mechanical strength than ordinary glass, this type of transparent microcrystalline glass will have Li during the crystallization process. + and Al 3+Generally, they will participate in crystallization. On the one hand, it will reduce the number of ions available for ion exchange. On the other hand, when a large amount of Al is enriched in the crystal, 3+ After that, the structure of the residual glass phase will be more compact, which is not conducive to ion exchange. Publication No. CN110217996A discloses that the maximum stress layer depth after two-step ion exchange with an aluminum oxide content of 22% is 93μm on average, while that with an aluminum oxide content of 17% and 18% is 106 and 98μm respectively. Therefore, non-alkali crystalline glass-ceramics are currently believed to be more effective for ion exchange.
[0006] Al2O3 plays a very positive role in improving the physical and chemical properties of glass. At the same time, the volume of [AlO4] tetrahedron is larger than that of [SiO4], and the Na2O3-bonded [AlO4] + It has better mobility. Therefore, Al2O3 needs to be introduced to promote ion exchange. However, blindly increasing the Al2O3 content will increase the viscosity of the high-aluminum silicate glass, increase the melting temperature, and reduce the process performance. For example, the invention patent application with publication number CN113880438A discloses a method for preparing zirconium dioxide microcrystalline glass and a terminal, whose aluminum oxide content is 17-22 mol%. Although the process problems caused by the increase in Al2O3 content can be improved by adding alkali metal oxides such as lithium oxide, the mechanical properties of the high-aluminum silicate glass will be weakened.
[0007] Lithium oxide has three main applications in current cover glass: 1. Participate in the crystallization of microcrystalline glass. Lithium aluminum silicate microcrystalline glass is a typical network former that participates in the crystallization process, forming silicate crystals from the silicate glass matrix. In order to precipitate the predetermined lithium-containing crystal phase, the amount of lithium used is generally greater than 12 mol%, or even higher. 2. Improve the process problems caused by the increase in Al2O3 content. 3. Participate in the subsequent one-step or two-step ion exchange process. Due to the application requirements of lithium oxide, the current cover glass products generally have the problem of excessive lithium content, and the price of lithium-containing ores has remained high due to the rapid development of lithium batteries and the emphasis of countries around the world on new energy, which greatly increases the cost of lithium aluminum silicate microcrystalline glass. In the invention patent application with publication number CN113880438A, 8-12 mol% of lithium oxide and 6-10 mol% of sodium oxide are added to improve the process problems caused by excessive Al2O3 content, while ensuring that sufficient lithium and sodium elements are contained in the subsequent chemical strengthening process for ion exchange. A higher content of Li2O will greatly increase the overall cost of the glass. At the same time, a higher content of Li2O and Na2O will have a greater tendency to crystallize, which will have great limitations in actual production and application, and will easily cause the microcrystalline glass to become foggy and devitrified, making it difficult to meet the actual use requirements of existing touch screens.
[0008] Therefore, how to reduce the content of lithium and aluminum in glass-ceramics while improving the light transmittance and mechanical properties of glass-ceramics has become a technical problem that needs to be urgently solved in this field. Summary of the invention
[0009] The object of the present invention is to provide a rare earth aluminosilicate glass-ceramics and a preparation method thereof. The rare earth aluminosilicate glass-ceramics provided by the present invention has low contents of lithium and aluminum elements, low production cost, and has the advantages of good light transmittance, high Vickers hardness and fracture toughness.
[0010] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0011] The present invention provides a rare earth aluminosilicate glass-ceramics, which comprises, in terms of molar percentage based on oxides: SiO2: 56-62%; Al2O3: 10-18%; Na2O: 4-8%; Li2O: 4-10%; rare earth oxide: 2-4%; ZrO2: 1-3%; MgO≤4% and K2O≤2%, wherein MgO and K2O are not 0 at the same time;
[0012] The crystal phase of the rare earth aluminosilicate glass-ceramics is zirconium dioxide nanocrystals.
[0013] Preferably, the average crystal size of the zirconium dioxide nanocrystals is ≤30 nm.
[0014] Preferably, the rare earth oxide includes at least one of La2O3, Y2O3 and CeO2.
[0015] Preferably, when the rare earth oxide contains La2O3, the molar percentage of La2O3 in the rare earth aluminosilicate glass-ceramics is 1-3%; when the rare earth oxide contains Y2O3, the molar percentage of Y2O3 in the rare earth aluminosilicate glass-ceramics is ≤2%; when the rare earth oxide contains CeO2, the molar percentage of CeO2 in the rare earth aluminosilicate glass-ceramics is ≤1%.
[0016] Preferably, the rare earth aluminosilicate glass-ceramics satisfies the following condition, measured in molar percentage based on oxide: Al2O3+MgO-Li2O-Na2O-K2O≥0%.
[0017] The present invention provides a method for preparing the rare earth aluminosilicate glass-ceramics described in the above technical solution, comprising the following steps:
[0018] (1) melting, molding and annealing the raw materials in sequence to obtain basic glass;
[0019] (2) heat treating the base glass obtained in step (1) to obtain glass-ceramics containing ZrO2 crystals;
[0020] (3) The microcrystalline glass containing ZrO2 crystals obtained in step (2) is subjected to ion exchange in a salt bath to obtain rare earth aluminosilicate microcrystalline glass.
[0021] Preferably, the annealing holding temperature in step (1) is lower than the glass transition temperature Tg50±10°C.
[0022] Preferably, the holding temperature of the heat treatment in step (2) is 700-900° C., and the holding time of the heat treatment is 4-20 h.
[0023] Preferably, the salt bath composition in step (3) comprises: 50-100wt% NaNO3 and 0-50wt% KNO3.
[0024] Preferably, the temperature of the ion exchange in step (3) is 400-500° C., and the time of the ion exchange is 5-20 h.
[0025] The invention provides a rare earth aluminosilicate glass-ceramics, which comprises, in terms of molar percentage based on oxides, SiO2: 56-62%; Al2O3: 10-18%; Na2O: 4-8%; Li2O: 4-10%; rare earth oxide: 2-4%; ZrO2: 1-3%; MgO≤4% and K2O≤2%, wherein MgO and K2O are not 0 at the same time; and the crystal phase of the rare earth aluminosilicate glass-ceramics is zirconium dioxide nanocrystals. The SiO2 in the rare earth aluminosilicate glass-ceramics provided by the present invention plays a very important role in improving the structure and performance of the glass. The [SiO4] tetrahedron, as the basic building block of the glass network, provides the glass with good mechanical strength and chemical stability. At the same time, the high chemical inertness and low thermal expansion coefficient of SiO2 make the glass have excellent corrosion resistance and thermal stability in various environments, so the introduction of SiO2 can significantly improve the overall performance of the glass. Al2O3 plays a very positive role in improving the physical and chemical properties of the glass. The aluminum element will form [AlO4] tetrahedron in the glass-ceramics. The volume of [AlO4] tetrahedron is larger than that of [SiO4], and the Na2O3 bonded to [AlO4]- + It has better mobility. The process of ZrO2 precipitation is accompanied by the transfer of alkali metal ions. Before ZrO2 precipitation, it exists in the glass as [ZrO6] octahedron with two units of negative charge. At this time, Na + , Li + ions are neutralized to achieve charge balance, so when ZrO2 is precipitated, the Na + , Li+ will be transferred to the surrounding of [AlO4]-tetrahedron, so the addition of alumina is more conducive to ion exchange, which can increase the depth of the exchange layer. The chemically strengthened microcrystalline glass shows excellent mechanical properties; Na2O and Li2O are the key exchange ions in the chemical strengthening of microcrystalline glass; K2O, Na2O and Li2O are all alkali metal oxides, which can increase the ion exchange rate and deepen the compressive stress layer, and can also play a role in breaking the network, reducing the viscosity and melting temperature of the glass. The coexistence of a small amount of K2O and Na2O can form a mixed alkali effect, which can optimize a series of glass properties; rare earth oxides can make the network structure of the glass dense, which can make the microcrystalline glass have better chemical stability and higher The glass transition temperature, strength and hardness of the microcrystalline glass are improved by adding zirconium dioxide to precipitate zirconium dioxide nanocrystals in the microcrystalline glass. Thanks to the small size (less than 30nm) of zirconium dioxide nanocrystals and the overall uniform crystallization characteristics, the microcrystalline glass does not show fogging and devitrification, ensuring that the microcrystalline glass material has excellent light transmittance; MgO exists in two coordination states in the glass (4-coordination and 6-coordination), but mostly exists in the form of [MgO6] octahedron, which makes the glass structure denser. In ion exchange, MgO can also increase the surface compressive stress after ion exchange; at the same time, the content of lithium and aluminum elements in the microcrystalline glass is lower, which can reduce its production cost while ensuring the performance of the microcrystalline glass, thereby realizing low-cost large-scale application. The results of the embodiment show that the rare earth aluminosilicate glass-ceramics provided by the present invention only contain uniformly distributed zirconium dioxide nanocrystals, and the average crystal size of the zirconium dioxide nanocrystals is ≤30nm, and the visible light transmittance of the rare earth aluminosilicate glass-ceramics is greater than 90%; at the same time, the surface compressive stress of the rare earth aluminosilicate glass-ceramics is ≥800MPa, and the Vickers hardness is >700kgf / mm 2 , the fracture toughness can reach 1.33~1.41MPa·m 1 / 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 X-ray diffraction patterns of the base glass provided in Example 1 and the rare earth aluminosilicate glass-ceramics obtained at different heat treatment temperatures;
[0027] Figure 2 X-ray diffraction patterns of the base glass provided in Example 4 and the rare earth aluminosilicate glass-ceramics obtained at different heat treatment temperatures;
[0028] Figure 3 TG-DSC graphs of the rare earth aluminosilicate glass-ceramics obtained in Examples 1 to 4 of the present invention;
[0029] Figure 4 1 is the light transmittance curve of the rare earth aluminosilicate glass-ceramics obtained in Examples 1 to 4 of the present invention. DETAILED DESCRIPTION
[0030] The present invention provides a rare earth aluminosilicate glass-ceramics, which comprises, in terms of molar percentage based on oxides: SiO2: 56-62%; Al2O3: 10-18%; Na2O: 4-8%; Li2O: 4-10%; rare earth oxide: 2-4%; ZrO2: 1-3%; MgO≤4% and K2O≤2%, wherein MgO and K2O are not 0 at the same time;
[0031] The crystal phase of the rare earth aluminosilicate glass-ceramics is zirconium dioxide nanocrystals.
[0032] In terms of molar percentage based on oxide, the rare earth aluminosilicate glass-ceramics provided by the present invention includes SiO2: 56-62%, preferably 57-61%, more preferably 58-60%, and further preferably 59%. In the present invention, SiO2 plays a very important role in improving the structure and performance of glass. [SiO4] tetrahedron, as the basic building block of the glass network, provides the glass with good mechanical strength and chemical stability; at the same time, the high chemical inertness and low thermal expansion coefficient of SiO2 make the glass have excellent corrosion resistance and thermal stability in various environments, so the introduction of SiO2 can significantly improve the overall performance of the glass; however, simply increasing the SiO2 content will increase the melting temperature and process complexity of the glass, thereby reducing production efficiency. Therefore, in the present invention, the molar percentage of SiO2 in the glass is controlled within the range of 56-62%.
[0033] The rare earth aluminosilicate glass-ceramics provided by the present invention comprises Al2O3: 10-18%, preferably 12-17%, more preferably 14-17%, and further preferably 15-16%, in terms of molar percentage based on oxide. In the present invention, Al2O3 plays a very positive role in improving the physical and chemical properties of the glass. The aluminum element forms [AlO4] tetrahedrons in the glass-ceramics. The volume of [AlO4] tetrahedrons is larger than that of [SiO4], and the Na2O3-bonded [AlO4]- + It has better mobility. The process of ZrO2 precipitation is accompanied by the transfer of alkali metal ions. Before ZrO2 precipitation, it exists in the glass as [ZrO6] octahedron with two units of negative charge. At this time, Na + , Li + ions are neutralized to achieve charge balance, so when ZrO2 is precipitated, the Na + , Li +It will be transferred to the surrounding of [AlO4]-tetrahedron, so the addition of alumina is more conducive to ion exchange and can increase the depth of the exchange layer. The chemically strengthened microcrystalline glass exhibits excellent mechanical properties; but if the Al2O3 content is too high, the viscosity of the glass will increase, the melting point will increase, and the process performance will decrease. Therefore, the molar percentage of Al2O3 in the glass is controlled within the range of 10-18%.
[0034] The rare earth aluminosilicate glass-ceramics provided by the present invention comprises Na2O: 4-8%, preferably 5-7%, more preferably 6%, in terms of molar percentage based on oxides. In the present invention, the sodium element can increase the depth of the exchange layer during ion exchange.
[0035] The rare earth aluminosilicate glass-ceramics provided by the present invention includes Li2O: 4-10%, preferably 5-9%, more preferably 6-8%, and further preferably 7%, in terms of molar percentage based on oxide. In the present invention, the lithium element can ensure the precipitation of lithium-containing crystal phase in the glass-ceramics while ensuring the effect of subsequent ion exchange strengthening; by adopting a lower amount of lithium element addition, while ensuring the performance of the glass after ion exchange, the cost of the glass is greatly reduced, and there is a great market application prospect; by controlling the amount of Li2O added, it can also be ensured that the crystal phase of the glass-ceramics contains only zirconium oxide crystals and does not contain Li-containing crystals.
[0036] In the present invention, Na2O and Li2O are key exchange ions in the chemical strengthening of microcrystalline glass, but at the same time, excessive Li2O and Na2O will cause crystals to precipitate in the glass. On the one hand, the precipitated crystals are not easy to control and are prone to form a variety of crystals, such as β-quartz, β-quartz solid solution, β-spodumene and other crystal phases, which seriously affect the optical properties of microcrystalline glass; on the other hand, the precipitation of lithium-containing crystal phases will reduce the number of exchangeable ions, affecting subsequent ion exchange strengthening. Therefore, the present invention controls the molar percentage of Na2O in the glass within the range of 4-8%, and the molar percentage of Li2O within the range of 4-10%, and the molar percentage of Na2O and Li2O satisfies the following relationship in terms of molar percentage based on oxide: 10%≤Li2O+Na2O≤16%.
[0037] The rare earth aluminosilicate glass-ceramics provided by the present invention includes K2O≤2%, preferably 0.5-2%, and more preferably 1-1.5%, in terms of molar percentage based on oxides. In the present invention, K2O, Na2O, and Li2O are all alkali metal oxides, which can increase the ion exchange rate and deepen the compressive stress layer, and can play a role in breaking the network, reducing the viscosity and melting temperature of the glass. The coexistence of a small amount of K2O and Na2O can form a mixed alkali effect, which can optimize a series of glass properties; ... + The radius is smaller than Na+ and Li + The maximum field strength is small, so the ability to combine with oxygen is weak; but too much K2O will hinder Li + and Na + Ion exchange will reduce the surface stress value, so the molar percentage of K2O in the glass is controlled to ≤2% in the present invention.
[0038] In terms of molar percentage based on oxide, the rare earth aluminosilicate glass-ceramics provided by the present invention includes MgO≤4%, preferably 0.5-4%, more preferably 1-3%, and further preferably 1-2%. In the present invention, the MgO mainly acts as a network exosome. MgO exists in two coordination states (4-coordination and 6-coordination) in the glass, but mostly exists in the form of [MgO6] octahedron, making the glass structure more compact. In ion exchange, MgO can increase the surface compressive stress of the rare earth aluminosilicate glass-ceramics obtained after ion exchange, but it will reduce the depth of the compressive stress layer. Therefore, the molar percentage of MgO is controlled to ≤4% in the present invention.
[0039] In the present invention, the MgO and K2O are not simultaneously 0. The present invention can ensure that the light transmittance and mechanical properties of the microcrystalline glass are improved while reducing the content of lithium and aluminum elements in the microcrystalline glass by controlling the glass to contain at least one of MgO and K2O.
[0040] In terms of molar percentage based on oxides, the rare earth aluminosilicate glass-ceramics provided by the present invention includes rare earth oxides: 2-4%. In the present invention, the rare earth oxide preferably includes at least one of La2O3, Y2O3 and CeO2, and more preferably any one of La2O3, La2O3 and Y2O3, La2O3 and CeO2, and La2O3, Y2O3 and CeO2. In the present invention, when the rare earth oxide includes La2O3, the molar percentage of La2O3 in the rare earth aluminosilicate glass-ceramics is preferably 1-3%, and more preferably 2%; when the rare earth oxide includes Y2O3, the molar percentage of Y2O3 in the rare earth aluminosilicate glass-ceramics is preferably ≤2%, and more preferably 1-2%; when the rare earth oxide includes CeO2, the molar percentage of CeO2 in the rare earth aluminosilicate glass-ceramics is preferably ≤1%, and more preferably 0.5-1%. In the present invention, the content of the rare earth oxide satisfies the following relationship in terms of molar percentage of oxide basis: La2O3+CeO2-Y2O3≥0. In the present invention, the rare earth oxide has a greater ion field strength and a higher dissociation energy than alkali metal and alkaline earth metal oxides, so it is difficult to be used as a forming body and reinforcing structure of the glass network structure, so the rare earth elements are mostly distributed in the gaps of the glass network structure and used as network modifiers. Therefore, after adding rare earth elements, due to the high charge and strong field of rare earth elements, they have a strong accumulation effect, which can make the network structure of the glass dense, and can make the microcrystalline glass have better chemical stability, higher glass transition temperature, strength and hardness; by controlling the type and amount of rare earth oxides, the hardness and other properties of the glass can be improved to a certain extent, so that the performance of the glass before and after crystallization is higher than that of ordinary lithium aluminum silicon cover glass; adding excessive rare earth oxides will lead to the depolymerization of the glass network, so the present invention controls the molar percentage of rare earth oxides in the glass within the range of 2-4%.
[0041] Calculated by molar percentage based on oxide, the rare earth aluminosilicate glass-ceramics provided by the present invention includes ZrO2: 1-3%, preferably 2%. In the present invention, ZrO2 has high hardness and fracture toughness, and the grain size during crystallization is much smaller than the wavelength of visible light, which makes it have extremely high transmittance. Zirconium dioxide is added to precipitate zirconium dioxide nanocrystals in the microcrystalline glass. Thanks to the small size (less than 30nm) of zirconium dioxide nanocrystals and the overall uniform crystallization characteristics, the microcrystalline glass does not experience fogging and devitrification, thereby ensuring that the microcrystalline glass material has excellent light transmittance. Since the solubility of ZrO2 in the silicate glass system is relatively low, an excessively high content will cause the glass to become devitrified, and the introduction of ZrO2 will increase the viscosity of the glass, reduce the thermal expansion coefficient of the glass, and improve the alkali resistance of the glass. Considering that the alkali metal ions and alkaline earth metal ions in the present invention will increase the solubility of ZrO2, and Al2O3 will reduce the solubility of ZrO2, and combined with experiments, it is found that when the molar content of ZrO2 reaches 4%, glass devitrification will occur, and the molar percentage of ZrO2 in the glass is controlled within the range of 1 to 3%.
[0042] The rare earth aluminosilicate glass-ceramics provided by the present invention preferably meets the following conditions in terms of molar percentage of oxide basis: Al2O3+MgO-Li2O-Na2O-K2O≥0%. In the present invention, the crystallization of ZrO2 is related to the coordination of zirconium in the glass network. In a system with a high degree of polymerization (low non-bridging oxygen content), most of the Zr 4+ It exists in 6-coordination, but there is also a certain amount of Zr 4+ The ions exist in 8-coordination (CN=8) and are connected to the silicon-oxygen tetrahedron in a common edge manner. Al2O3 and MgO will form structures such as aluminum-oxygen tetrahedrons in the glass network, which often have negative charges and require network modifier ions (Na + , Li + ) for charge compensation, and this high coordination Zr (CN = 8) is due to the network modifier ions (Na + , Li + ) is too small to satisfy the charge balance, Zr (CN = 8) tends to form a locally ordered Zr-rich structure, and these Zr-rich regions become the precursors of crystallization, promoting the crystallization of ZrO2 during heat treatment. Therefore, in order to ensure the precipitation of ZrO2 crystals, the above conditions need to be met.
[0043] In the present invention, the crystal phase of the rare earth aluminosilicate glass-ceramics is zirconium dioxide nanocrystals; the average crystal size of the zirconium dioxide nanocrystals is preferably ≤30nm; the zirconium dioxide nanocrystals are preferably evenly distributed in the rare earth aluminosilicate glass-ceramics; the thickness of the rare earth aluminosilicate glass-ceramics is preferably ≤1mm, more preferably 1mm. The present invention introduces zirconium dioxide into the glass-ceramics to form evenly distributed zirconium dioxide nanocrystals in the glass-ceramics, so that the glass-ceramics does not have fogging and devitrification, ensuring that the glass-ceramics material has excellent light transmittance. When the thickness of the rare earth aluminosilicate glass-ceramics is ≤1mm, the visible light transmittance of the rare earth aluminosilicate glass-ceramics is greater than 90%.
[0044] The SiO2 in the rare earth aluminosilicate glass-ceramics provided by the present invention plays a very important role in improving the structure and performance of the glass. The [SiO4] tetrahedron, as the basic building block of the glass network, provides the glass with good mechanical strength and chemical stability. At the same time, the high chemical inertness and low thermal expansion coefficient of SiO2 make the glass have excellent corrosion resistance and thermal stability in various environments, so the introduction of SiO2 can significantly improve the overall performance of the glass. Al2O3 plays a very positive role in improving the physical and chemical properties of the glass. The aluminum element will form [AlO4] tetrahedron in the glass-ceramics. The volume of [AlO4] tetrahedron is larger than that of [SiO4], and the Na2O3 bonded to [AlO4]- + It has better mobility. The process of ZrO2 precipitation is accompanied by the transfer of alkali metal ions. Before ZrO2 precipitation, it exists in the glass as [ZrO6] octahedron with two units of negative charge. At this time, Na + , Li + ions are neutralized to achieve charge balance, so when ZrO2 is precipitated, the Na + , Li + Will transfer to [AlO4] -The addition of alumina is more conducive to ion exchange and can increase the depth of the exchange layer. The chemically strengthened glass-ceramics exhibits excellent mechanical properties. Na2O and Li2O are key exchange ions in chemical strengthening of glass-ceramics. K2O, Na2O and Li2O are alkali metal oxides, which can increase the ion exchange rate and deepen the compressive stress layer, and can also play a role in breaking the network, reducing the viscosity and melting temperature of the glass. The presence of a small amount of K2O and Na2O at the same time can form a mixed alkali effect, which can optimize a series of glass properties. Rare earth oxides can make the network structure of the glass dense, which can make the glass-ceramics have better chemical stability and higher Glass transition temperature, strength and hardness; ZrO2 has high hardness and fracture toughness, and the grain size during crystallization is much smaller than the wavelength of visible light, which makes it have extremely high transmittance. By adding zirconium dioxide, zirconium dioxide nanocrystals are precipitated in the microcrystalline glass. Thanks to the small size of zirconium dioxide nanocrystals (less than 30nm) and the overall uniform crystallization characteristics, the microcrystalline glass does not show fogging and devitrification, ensuring that the microcrystalline glass material has excellent light transmittance; MgO exists in two coordination states in the glass (4-coordination and 6-coordination), but most of it exists in the form of [MgO6] octahedron, making the glass structure denser. In ion exchange, MgO can also increase the surface compressive stress after ion exchange.
[0045] The crystal phase of the rare earth aluminosilicate glass-ceramics provided by the present invention is zirconium dioxide nanocrystals, which can prevent the glass-ceramics from fogging and devitrification, thereby ensuring that the glass-ceramics material has excellent light transmittance; the content of lithium and aluminum elements in the glass-ceramics is lower, which can reduce its production cost while ensuring the performance of the glass-ceramics, thereby realizing low-cost large-scale application.
[0046] The present invention also provides a method for preparing the rare earth aluminosilicate glass-ceramics described in the above technical solution, comprising the following steps:
[0047] (1) melting, molding and annealing the raw materials in sequence to obtain basic glass;
[0048] (2) heat treating the base glass obtained in step (1) to obtain glass-ceramics containing ZrO2 crystals;
[0049] (3) The microcrystalline glass containing ZrO2 crystals obtained in step (2) is subjected to ion exchange in a salt bath to obtain rare earth aluminosilicate microcrystalline glass.
[0050] The invention sequentially melts, shapes and anneals raw materials to obtain basic glass.
[0051] The present invention has no special restrictions on the specific type, amount and addition method of the raw materials, as long as the amount of various oxides in the rare earth aluminosilicate glass-ceramics meets the requirements.
[0052] The present invention has no special requirements for the melting temperature and time, which can be determined according to the technical common sense of those skilled in the art as long as the melt can be kept clear. In one embodiment of the present invention, the melting temperature is 1550-1650°C.
[0053] The present invention has no particular limitation on the specific operation of the molding, and molding operations well known to those skilled in the art may be used.
[0054] In the present invention, the annealing is preferably performed in a muffle furnace. The present invention has no particular limitation on the specific model of the muffle furnace, and a commercially available muffle furnace well known to those skilled in the art can be used.
[0055] In the present invention, the annealing holding temperature is preferably lower than the glass transition temperature Tg50±10°C, more preferably lower than the glass transition temperature Tg50°C; the annealing holding time is preferably 2 to 4 hours, more preferably 2.5 to 3.5 hours, and further preferably 3 hours; the annealing cooling method is preferably furnace cooling. The present invention can reduce the internal stress in the base glass through annealing treatment; and can further reduce the internal stress in the base glass by controlling the parameters of the annealing treatment.
[0056] After obtaining the basic glass, the present invention performs heat treatment on the basic glass to obtain microcrystalline glass containing ZrO2 crystals.
[0057] In the present invention, the holding temperature of the heat treatment is preferably 700-900°C, more preferably 750-850°C, and further preferably 800°C; the holding time of the heat treatment is preferably 4-20h, more preferably 8-16h, and further preferably 10-12h; the cooling method of the heat treatment is preferably furnace cooling. The present invention can precipitate zirconium dioxide crystals in the glass by heat treating the base glass, thereby obtaining microcrystalline glass containing ZrO2 crystals; by controlling the process parameters of the heat treatment, ZrO2 crystals can be fully precipitated, and at the same time, lithium crystals will not be given too much nucleation and growth time, thereby ensuring that the crystal phase of the microcrystalline glass contains only zirconium oxide crystals and does not contain Li-containing crystals.
[0058] After the heat treatment, the present invention preferably performs a polishing treatment on the heat treated product to obtain a glass-ceramic containing ZrO2 crystals. The present invention has no particular limitation on the specific operation of the polishing treatment, as long as the surface of the glass is smooth and free of impurities.
[0059] In the present invention, the thickness of the microcrystalline glass containing ZrO2 crystals is preferably ≤1 mm, more preferably 0.5 to 1 mm, and further preferably 0.8 to 1 mm. The present invention can further improve the light transmittance of the microcrystalline glass by controlling the thickness of the microcrystalline glass.
[0060] After obtaining the microcrystalline glass containing ZrO2 crystals, the present invention performs ion exchange on the microcrystalline glass containing ZrO2 crystals in a salt bath to obtain rare earth aluminosilicate microcrystalline glass.
[0061] In the present invention, the salt bath composition preferably includes: 50-100wt% NaNO3 and 0-50wt% KNO3, more preferably 60-90wt% NaNO3 and 10-40wt% KNO3, and further preferably 70-80wt% NaNO3 and 20-30wt% KNO3. The present invention can exchange sodium for lithium, potassium for sodium, and a small portion of potassium for lithium by performing ion exchange in the salt bath; and the efficiency of ion exchange can be improved by controlling the composition of the salt bath.
[0062] In the present invention, the ion exchange is preferably a low-temperature ion exchange; the temperature of the ion exchange is preferably 400-500°C, more preferably 420-480°C, and further preferably 450°C; the time of the ion exchange is preferably 5-20h, and more preferably 10-15h. The present invention can form an ion exchange layer on the surface of the microcrystalline glass through ion exchange, which can enable the microcrystalline glass to form a surface compressive stress greater than 800MPa, further enhancing the performance of the glass; by controlling the composition of the salt bath and the parameters of the ion exchange, the stress layer depth of the surface compressive stress can reach 50-70μm. The higher ion exchange layer depth and surface compressive stress make the chemically strengthened microcrystalline glass have higher hardness and fracture toughness. The Vickers hardness of the glass after ion exchange is greater than 700Kgf / mm 2 At the same time, the use of low-temperature ion exchange can avoid the impact of high temperature on zirconium dioxide crystals, such as causing the grains to become larger.
[0063] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] Examples 1 to 8
[0065] The compositions of the rare earth aluminosilicate glass-ceramics provided in Examples 1 to 8 are shown in Table 1, in terms of molar percentage based on oxides;
[0066] The method for preparing the rare earth aluminosilicate glass-ceramics provided in Examples 1 to 8 comprises the following steps:
[0067] (1) melting the raw materials at 1600° C., then forming and annealing them in sequence, and finally cooling them in the furnace to obtain the basic glass; the annealing is performed in a muffle furnace; the annealing temperature is 50° C. lower than the glass transition temperature Tg, and the annealing time is 3 hours;
[0068] (2) heat treating the base glass obtained in step (1), and then polishing the base glass after furnace cooling to obtain a 0.8 mm thick glass-ceramic containing ZrO2 crystals; the heat treatment temperature is 700°C, 750°C, 800°C, 850°C and 900°C, respectively, and the heat treatment time is 10 h, which corresponds to 700°C / 10 h, 750°C / 10 h, 800°C / 10 h, 850°C / 10 h and 900°C / 10 h in Table 2, respectively;
[0069] (3) subjecting the microcrystalline glass containing ZrO2 crystals obtained in step (2) to ion exchange in a salt bath to obtain rare earth aluminosilicate microcrystalline glass; the salt bath composition is: 60wt% NaNO3 and 40wt% KNO3; the ion exchange temperature is 450°C, and the ion exchange time is 5h.
[0070] The appearance characteristics of the base glass and the glass-ceramics containing ZrO2 crystals obtained in the preparation process of the rare earth aluminosilicate glass-ceramics provided in Examples 1 to 8 are shown in Table 1:
[0071] Table 1 Composition of rare earth aluminosilicate glass-ceramics provided in Examples 1 to 8 and appearance characteristics of base glass and glass-ceramics containing ZrO2 crystals during preparation
[0072]
[0073]
[0074] From the appearance characteristics of the microcrystalline glass containing ZrO2 crystals in Table 1, it can be seen that the ZrO2 crystals precipitated inside the glass after heat treatment and crystallization do not affect the colorless and transparent appearance of the microcrystalline glass.
[0075] The properties of the base glass obtained in step (1) of Examples 1 to 8, the glass-ceramics containing ZrO2 crystals obtained in step (2), and the rare earth aluminosilicate glass-ceramics obtained in step (3) were tested, and the results are shown in Table 2:
[0076] Table 2 Properties of the glasses provided in Examples 1 to 8
[0077]
[0078]
[0079] In Table 2, AP1 is the base glass, the temperature and time below AP1 represent the microcrystalline glass containing ZrO2 crystals obtained at different heat treatment temperatures for 10 hours, AP2 refers to the aluminosilicate glass obtained by directly ion exchange of the base glass, and the temperature and time below AP2 represent the rare earth aluminosilicate microcrystalline glass obtained by ion exchange of the microcrystalline glass containing ZrO2 crystals obtained by heat treatment of the base glass at different temperatures for 10 hours.
[0080] From the results in Table 2, it can be seen that the Vickers hardness and fracture toughness of the rare earth aluminosilicate glass-ceramics obtained after crystallization of the present invention are improved to a certain extent compared with the uncrystallized base glass. The Vickers hardness of the uncrystallized base glass is between 636 and 655 Kgf / mm. 2 The Vickers hardness of the rare earth aluminosilicate glass-ceramics obtained by the crystallized ZrO2 crystal-containing glass-ceramics provided by the present invention can reach 649-684 Kgf / mm 2 The fracture toughness of the glass obtained by direct ion exchange of the uncrystallized base glass is 1.03~1.18MPa·m 1 / 2 The fracture toughness of the crystallized glass containing ZrO2 crystals can reach 1.30-1.38 MPa·m 1 / 2 The fracture toughness of the rare earth aluminosilicate glass-ceramics obtained after ion exchange can reach 1.33-1.41 MPa·m 1 / 2 , which has been significantly improved.
[0081] At the same time, it can be seen from Table 2 that with the precipitation of ZrO2 in the rare earth aluminosilicate glass-ceramics, the ion exchange capacity of the glass is not weakened, but the depth of the ion exchange layer is increased. For the surface compressive stress of the chemically strengthened glass, with the continuous increase of the ion exchange temperature (the same ion exchange time), the surface compressive stress shows a trend of first increasing and then decreasing. At the same time, with the extension of the ion exchange time (the ion exchange temperature remains unchanged), the surface compressive stress shows a trend of first increasing and then decreasing. This is the result of the structural relaxation of the glass under high temperature conditions (i.e. immersed in high temperature molten salt). In the early stage of ion exchange, the increase of surface compressive stress is dominant, and in the later stage, the structural relaxation under stress is dominant. As for the stress layer depth of the chemically strengthened glass, the stress layer depth increases with the increase of ion exchange temperature or the extension of time.
[0082] The rare earth aluminosilicate glass-ceramics provided in Examples 1 to 8 of the present invention can achieve a surface compressive stress CS ≥ 800 MPa, and a strengthening depth, i.e., an ion exchange layer depth DOL> 50 μm, which is beneficial to improving drop resistance and can better meet the application requirements of touch display screens.
[0083] Figure 1 X-ray diffraction (XRD) diagrams of the base glass provided in Example 1 and the rare earth aluminosilicate glass-ceramics obtained at different heat treatment temperatures. Figure 1 It can be seen that the heat treatment methods of 700℃ / 10h, 750℃ / 10h and 800℃ / 10h adopted in Example 1 precipitate ZrO2 crystals. The sample of Example 1 did not crystallize under the heat treatment of 700℃ / 10h, but precipitated ZrO2 crystals under the heat treatment of 750℃ / 10h, and the glass was still colorless and transparent; when the crystallization temperature was further increased to 800℃, the XRD diffraction peak intensity became stronger, indicating that the degree of ZrO2 crystallization increased.
[0084] Figure 2 X-ray diffraction (XRD) diagrams of the base glass provided in Example 4 and the rare earth aluminosilicate glass-ceramics obtained at different heat treatment temperatures. Figure 2 It can be seen that the heat treatment methods of 750℃ / 10h, 800℃ / 10h and 850℃ / 10h adopted in Example 4 are used to precipitate ZrO2 crystals. The sample of Example 4 did not undergo crystallization under the heat treatment of 750℃ / 10h, but precipitated ZrO2 crystals under the heat treatment of 800℃ / 10h, and the glass was still colorless and transparent; when the crystallization temperature was further increased to 850℃, the degree of ZrO2 crystallization increased and the diffraction peak intensity became stronger.
[0085] Figure 3 TG-DSC graphs of rare earth aluminosilicate glass-ceramics obtained in Examples 1 to 4 of the present invention. Figure 3 It can be seen that the aluminum silicon content of the rare earth aluminosilicate glass-ceramics obtained in Example 1 is relatively low, while its lithium content is relatively high, so the glass transition temperature Tg and the crystallization peak temperature Tp are relatively low.
[0086] Figure 4 The light transmittance curves of the rare earth aluminosilicate glass-ceramics obtained in Examples 1 to 4 of the present invention are shown in FIG. Figure 4 It can be seen that the transmittance of the microcrystalline glass of the present invention in the visible light band (380nm-780nm) can reach more than 90%.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A rare earth aluminosilicate glass-ceramics, which comprises, in terms of molar percentage based on oxides: SiO2: 56-62%; Al2O3: 10-18%; Na2O: 4-8%; Li2O: 4-10%; rare earth oxides: 2-4%; ZrO2: 1-3%; MgO≤4% and K2O≤2%, where MgO and K2O are not 0 at the same time; The crystal phase of the rare earth aluminosilicate glass-ceramics is zirconium dioxide nanocrystals.
2. The rare earth aluminosilicate glass-ceramics according to claim 1, characterized in that: The average crystal size of the zirconium dioxide nanocrystals is ≤30 nm.
3. The rare earth aluminosilicate glass-ceramics according to claim 1, characterized in that: The rare earth oxide includes at least one of La2O3, Y2O3 and CeO2.
4. The rare earth aluminosilicate glass-ceramics according to claim 3, characterized in that: When the rare earth oxide contains La2O3, the molar percentage of La2O3 in the rare earth aluminosilicate glass-ceramics is 1-3%; when the rare earth oxide contains Y2O3, the molar percentage of Y2O3 in the rare earth aluminosilicate glass-ceramics is ≤2%; when the rare earth oxide contains CeO2, the molar percentage of CeO2 in the rare earth aluminosilicate glass-ceramics is ≤1%.
5. The rare earth aluminosilicate glass-ceramics according to claim 1, characterized in that: Measured in molar percentage based on oxides, the rare earth aluminosilicate glass-ceramics meets the following condition: Al2O3+MgO-Li2O-Na2O-K2O≥0%.
6. The method for preparing the rare earth aluminosilicate glass-ceramics according to any one of claims 1 to 5, comprising the following steps: (1) melting, molding and annealing the raw materials in sequence to obtain basic glass; (2) heat treating the base glass obtained in step (1) to obtain glass-ceramics containing ZrO2 crystals; (3) The microcrystalline glass containing ZrO2 crystals obtained in step (2) is subjected to ion exchange in a salt bath to obtain rare earth aluminosilicate microcrystalline glass.
7. The preparation method according to claim 6, characterized in that: The annealing holding temperature in the step (1) is lower than the glass transition temperature Tg50±10°C.
8. The preparation method according to claim 6, characterized in that: The heat treatment in step (2) is carried out at a holding temperature of 700 to 900° C. and for a holding time of 4 to 20 hours.
9. The preparation method according to claim 6, characterized in that: The salt bath composition in step (3) includes: 50-100wt% NaNO3 and 0-50wt% KNO3.
10. The preparation method according to claim 6, characterized in that: The temperature of the ion exchange in step (3) is 400-500° C., and the time of the ion exchange is 5-20 hours.
Citation Information
Patent Citations
Aluminosilicate glass composition, aluminosilicate glass and preparation method and application of aluminosilicate glass
CN109160727A
Glass ceramic for chemical strengthening, chemically strengthened glass as well as application and electronic equipment of chemically strengthened glass
CN110217994A
Transparent toughened glass ceramic and preparation method thereof
CN110627365A
Seed crystal toughened lithium aluminosilicate microcrystalline glass composite material and preparation method thereof
CN112408803A
Microcrystalline glass and terminal
CN113880438A