By combining polyurethane prepolymers, timber diversified alcohols and phase change latent heat materials in asphalt concrete, the performance problems of asphalt pavement at high and low temperatures are solved, the stability and durability of asphalt concrete are improved, and aging is delayed process.
Patent Information
- Application Number
- CN202411168775.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
Under high temperature conditions, asphalt pavement is prone to diseases such as displacement, packing and rut, which reduces the service life of asphalt pavement. The existing technology is difficult to effectively improve the high-temperature and low-temperature performance, resistance to ultraviolet and oxidation resistance of asphalt concrete.
Polyurethane modified asphalt concrete is used to improve polyurethane by combining polyurethane prepolymer with lignin diversified alcohols, epoxy modified asphalt, temperature adapter, hardener, anti-flaking agent, antioxidant and modified glue powder. Dispersion and stability in asphalt concrete system, and the absorption and storage of heat of the phase change latent heat material can improve the phase change reversibility and cyclic thermal stability of asphalt.
It significantly improves the high-temperature and low-temperature properties of polyurethane modified asphalt concrete, delays the aging effect, enhances the weather resistance and durability of asphalt concrete, reduces softening and cracking phenomena, and improves thermal stability and toughness.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt concrete, in particular to a polyurethane modified asphalt concrete. Background Art
[0002] Asphalt concrete is a composite material, commonly used in pavements, parking lots, airports, and the core of dams. Since the beginning of the 20th century, asphalt concrete has been used in pavement construction. Asphalt concrete has many advantages such as high strength, seamlessness, flatness, low noise, low dust, comfortable driving, and fast repair, which makes it widely used in pavement construction. Under high temperature conditions, asphalt pavements are prone to slippage, bulging, rutting and other diseases under the repeated action of vehicles, which reduces the service life of asphalt pavements and is not conducive to the use of asphalt pavements. For this reason, we propose a polyurethane modified asphalt concrete, which has the effect of improving the high and low temperature performance, UV resistance, antioxidant and antibacterial properties of asphalt concrete. Summary of the invention
[0003] The purpose of the present invention is to provide a polyurethane modified asphalt concrete to solve the problems raised in the above background technology.
[0004] To achieve the above-mentioned object, the present invention provides the following technical scheme: a polyurethane modified asphalt concrete, comprising the following components in parts by weight: 100-150 parts of aggregate, 20-40 parts of epoxy modified asphalt, 5-8 parts of polyurethane prepolymer, 1-2 parts of wood diversification alcohol, 3-5 parts of temperature adaptor, 2-4 parts of hardener, 2-3 parts of anti-stripping agent, 1-3 parts of antioxidant and 1-3 parts of modified rubber powder;
[0005] The aggregate comprises fine aggregate, coarse aggregate, silica powder and fly ash in a mass ratio of 1:(2-4):(0.2-0.6):(0.1-0.2).
[0006] In the above scheme, the epoxy modified asphalt is modified by mixing base asphalt with epoxy silicone resin and curing agent.
[0007] In the above scheme, the polyurethane prepolymer comprises polyisocyanate and a binary catalyst in a mass ratio of 2:1.
[0008] In the above scheme, the temperature adaptor includes SBS, graphene and phase change latent heat material in a mass ratio of 1:(0.3-0.4):(0.2-0.6):(1.2-1.6).
[0009] In the above scheme, the phase change latent heat material includes polyethylene glycol and hydroxyethyl cellulose in a mass ratio of 1:(1.1-1.3).
[0010] In the above scheme, the hardener includes polysilazane and silicone resin in a mass ratio of 1:(0.5-0.5).
[0011] In the above scheme, the anti-stripping agent is hexadecyltrimethylammonium chloride or dioctadecylamine hydrochloride.
[0012] In the above scheme, the antioxidant is dodecyl phosphite or decabromodiphenyl ether.
[0013] In the above scheme, the polyurethane modified asphalt concrete comprises the following steps:
[0014] After heating and heat-insulating the base asphalt and shearing it, a curing agent and a high-temperature modifier are added, and the modified asphalt is obtained after stirring evenly; preheated polyurethane prepolymer and wood diversification alcohol mixture are added to the modified asphalt, and a temperature adaptor, a hardener, an anti-stripping agent, an antioxidant and modified rubber powder are added to the mixture, and the polyurethane modified asphalt is obtained after stirring evenly; aggregates are added to the polyurethane modified asphalt, and the polyurethane modified asphalt concrete is obtained after stirring evenly.
[0015] Compared with the prior art, the beneficial effects of the present invention are: a polyurethane modified asphalt concrete, the polyurethane prepolymer is modified by wood diversification alcohol, the dispersibility of polyurethane in the asphalt concrete system is improved, the stability of the system is improved, thereby improving the high temperature performance of the polyurethane modified asphalt concrete, the phase change latent heat material absorbs and stores the heat received by the asphalt, improves the phase change reversibility and cyclic thermal stability of the asphalt, so as to reduce the possibility of asphalt softening and flowing due to high temperature, and uses hydroxyethyl cellulose as the hard segment in the phase change latent heat material, which can promote the soft and hard segment microphase separation of the phase change latent heat material to be more perfect, thereby ensuring that the prepared phase change latent heat material has good mechanical properties and thermal stability. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0017] A polyurethane modified asphalt concrete comprises the following components in parts by weight: 100-150 parts of aggregate, 20-40 parts of epoxy modified asphalt, 5-8 parts of polyurethane prepolymer, 1-2 parts of wood diversification alcohol, 3-5 parts of temperature adaptor, 2-4 parts of hardener, 2-3 parts of anti-stripping agent, 1-3 parts of antioxidant and 1-3 parts of modified rubber powder;
[0018] The polyurethane prepolymer is modified with wood polyols to improve the dispersibility of polyurethane in the asphalt concrete system and enhance the stability of the system, thereby improving the high temperature performance of the polyurethane modified asphalt concrete.
[0019] The aggregate comprises fine aggregate, coarse aggregate, silica powder and fly ash in a mass ratio of 1:(2-4):(0.2-0.6):(0.1-0.2).
[0020] The epoxy modified asphalt is prepared by mixing base asphalt with epoxy silicone resin and a curing agent for modification.
[0021] The polyurethane prepolymer comprises polyisocyanate and a binary catalyst in a mass ratio of 2:1. The binary catalyst catalyzes the generation of lignin-based polyurethane prepolymer, improves the UV resistance and oxidation resistance of polyurethane-modified asphalt concrete, and delays aging.
[0022] The temperature adaptor comprises SBS, graphene and phase change latent heat material in a mass ratio of 1:(0.3-0.4):(0.2-0.6):(1.2-1.6), wherein SBS has good temperature sensitivity, and graphene has high thermal conductivity, good toughness and chemical stability. By compounding asphalt with SBS and graphene, the SBS can improve the temperature sensitivity of asphalt, thereby better improving the low-temperature creep performance of asphalt. Meanwhile, by combining the phase change latent heat material with the modified asphalt, the phase change latent heat material absorbs and stores the heat received by the asphalt, thereby improving the phase change reversibility and cyclic thermal stability of the asphalt, thereby reducing the possibility of softening and flowing of the asphalt due to high temperature, and reducing the possibility of cracking due to low temperature, thereby making the asphalt have better weather resistance, thereby improving the durability of the asphalt concrete prepared by the modified asphalt; and by adding rubber powder, the thermal stability and toughness of the modified asphalt concrete are improved, thereby making the modified asphalt concrete less likely to crack or peel off at low temperatures.
[0023] The phase change latent heat material comprises polyethylene glycol and hydroxyethyl cellulose in a mass ratio of 1:(1.1-1.3). Polyethylene glycol, as a soft segment in the phase change latent heat material, can provide a wider phase change temperature selection range for the phase change latent heat material, and has the advantages of simple and neat structure, easy crystallization, large melting enthalpy, low thermal hysteresis effect, etc. Hydroxyethyl cellulose is used as a hard segment in the phase change latent heat material, which can promote the soft and hard segment microphase separation of the phase change latent heat material to be more perfect, and ensure that the prepared phase change latent heat material has good mechanical properties and thermal stability. The preparation method of the phase change latent heat material comprises the following steps:
[0024] The polyethylene glycol is added to an organic solvent, stirred and dissolved at 75-80°C, and then the hydroxyethyl cellulose is added, and reacted at 70-80°C for 1-2 hours to form a prepolymer; a chain extender is added to the prepolymer, and a chain extension reaction is carried out for 30 minutes. After the reaction is completed, the prepolymer is vacuum dried and crushed to obtain a phase change latent heat material. The degree of polymerization of the polyethylene glycol is 1000-3000. The phase change latent heat material prepared by the polyethylene glycol in the above degree of polymerization range has better phase change reversibility and thermal stability.
[0025] The hardener includes polysilazane and silicone resin in a mass ratio of 1:(0.5-0.5).
[0026] The anti-stripping agent is hexadecyltrimethylammonium chloride or dioctadecylamine hydrochloride. One end of the long hydrocarbon of the anti-stripping agent can form a chemical bond with the asphalt surface, while the other end has a bridging effect with inorganic matter, namely coarse and fine aggregates in concrete, so as to improve the adhesion between asphalt and other aggregates in concrete, further improve the mechanical properties of the prepared asphalt concrete, and thus improve durability.
[0027] The antioxidant is dodecyl phosphite or decabromodiphenyl ether, and the antioxidant improves the aging resistance and antioxidant capacity of the modified asphalt concrete.
[0028] Specifically, in the present invention:
[0029] Preparation of polyurethane prepolymer: 1.1g of anhydrous glycerol and 2.2g of potassium hydroxide are dispersed in 20g of acetone to obtain a catalyst solution, 0.81g of lignin polyol and the catalyst solution are mixed and stirred evenly in a 50mL micro-high pressure reactor, and the mixture is kept at 150°C for 2h with a magnetic stirring speed of 400rpm / min to obtain oxypropylated lignin polyol; 1.6g of oxypropylated lignin polyol, 0.135g of stannous octoate and 0.135g of bis(dimethylaminoethyl)ether are mixed in a 50mL centrifuge tube, and after oscillating on a vortex oscillator for 10 minutes, 2.4g of polyisocyanate is added to the centrifuge tube, and the mixture is mixed evenly and reacted for 10min to obtain a lignin-based polyurethane prepolymer.
[0030] The preparation method of the phase change latent heat material comprises the following steps: adding 1 kg of polyethylene glycol (with a degree of polymerization of 2000) into 2 L of propanol solvent, stirring and dissolving at 80°C, and then adding 1.3 kg of hydroxyethyl cellulose to disperse it in the above organic mixed solution, wherein the mass ratio of the above polyethylene glycol to the hydroxyethyl cellulose is 1:1.3, and reacting at 80°C for 1 hour to form a uniform prepolymer; adding 0.1 kg of chain extender trimethylolpropane into the above prepolymer, and carrying out a chain extension reaction for 30 minutes. After the reaction is completed, pouring the prepolymer into a mold, keeping it in a vacuum drying oven at 100°C for 48 hours, and crushing it to obtain the phase change latent heat material, wherein the crushed particle size of the phase change latent heat material is 2 mm.
[0031] The polyurethane modified asphalt concrete comprises the following steps:
[0032] After heating and heat-insulating the base asphalt and shearing it, a curing agent and a high-temperature modifier are added, and the modified asphalt is obtained after stirring evenly; preheated polyurethane prepolymer and wood diversification alcohol mixture are added to the modified asphalt, and a temperature adaptor, a hardener, an anti-stripping agent, an antioxidant and modified rubber powder are added to the mixture, and the polyurethane modified asphalt is obtained after stirring evenly; aggregates are added to the polyurethane modified asphalt, and the polyurethane modified asphalt concrete is obtained after stirring evenly.
[0033] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A polyurethane modified asphalt concrete, characterized in that: The invention comprises the following components in parts by weight: 100-150 parts of aggregate, 20-40 parts of epoxy modified asphalt, 5-8 parts of polyurethane prepolymer, 1-2 parts of wood diversified alcohol, 3-5 parts of temperature adaptor, 2-4 parts of hardener, 2-3 parts of anti-stripping agent, 1-3 parts of antioxidant and 1-3 parts of modified rubber powder; The aggregate comprises fine aggregate, coarse aggregate, silica powder and fly ash in a mass ratio of 1:(2-4):(0.2-0.6):(0.1-0.2).
2. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The epoxy modified asphalt is prepared by mixing base asphalt with epoxy silicone resin and a curing agent for modification.
3. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The polyurethane prepolymer comprises polyisocyanate and a binary catalyst in a mass ratio of 2:
1.
4. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The temperature adaptor comprises SBS, graphene and phase change latent heat material in a mass ratio of 1:(0.3-0.4):(0.2-0.6):(1.2-1.6).
5. The polyurethane modified asphalt concrete according to claim 4, characterized in that: The phase change latent heat material comprises polyethylene glycol and hydroxyethyl cellulose in a mass ratio of 1:(1.1-1.3).
6. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The hardener includes polysilazane and silicone resin in a mass ratio of 1:(0.5-0.5).
7. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The anti-stripping agent is hexadecyltrimethylammonium chloride or dioctadecylamine hydrochloride.
8. The polyurethane modified asphalt concrete according to claim 1, characterized in that: The antioxidant is dodecyl phosphite or decabromodiphenyl ether.
9. A polyurethane modified asphalt concrete, characterized in that: The polyurethane modified asphalt concrete comprises the following steps: After heating and heat-insulating the base asphalt and shearing it, a curing agent and a high-temperature modifier are added, and the modified asphalt is obtained after stirring evenly; preheated polyurethane prepolymer and wood diversification alcohol mixture are added to the modified asphalt, and a temperature adaptor, a hardener, an anti-stripping agent, an antioxidant and modified rubber powder are added to the mixture, and the polyurethane modified asphalt is obtained after stirring evenly; aggregates are added to the polyurethane modified asphalt, and the polyurethane modified asphalt concrete is obtained after stirring evenly.
Citation Information
Cited By
A hyperbranched polymer asphalt modifier, strong and tough modified asphalt based thereon and a method for preparing the same
CN122790247A