Dolomite lining composite material and preparation method thereof
By using composite materials prepared by dolomite, talc and zinc stearate, replacing graphite in traditional dolomite liners, the problem of current instability in high-temperature and high-pressure synthesis is solved, the quality and efficiency of diamond synthesis are improved, and the quality and efficiency of diamond synthesis are achieved. Energy saving and efficiency enhancement.
Patent Information
- Application Number
- CN202411207190.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
During the high-temperature and high-pressure synthesis of diamonds, the graphite composition in the traditional dolomite lining leads to unstable current, affecting the temperature and pressure stability in the synthesis cavity, and may lead to crack hammer firing incidents. The existing technology cannot effectively solve this problem.
Using dolomite, talc and zinc stearate as the main components, a new dolomite-lined composite material is prepared through agitation and pressing process to replace traditional graphite, improve thermal insulation performance and reduce current fluctuation.
It effectively reduces the current fluctuation in the process of synthesizing diamonds, improves the synthesis quality and efficiency, increases output, reduces hammer consumption, and achieves energy saving and efficiency enhancement.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of heat-insulating and pressure-transmitting composite materials of superhard materials, and in particular relates to a dolomite lining composite material and a preparation method thereof. Background Art
[0002] In the process of high-temperature and high-pressure synthesis (HPHT) of diamond, the stability of electric current is crucial to maintain a constant high-temperature and high-pressure environment in the synthesis chamber. Current fluctuations may lead to unstable temperature and pressure, which in turn affects the synthesis efficiency and quality of diamond.
[0003] Traditionally, dolomite lining is generally used as a pressure transmission and heat preservation medium to maintain a stable high temperature and high pressure environment in the synthesis cavity. The dolomite lining on the market is mainly made of dolomite, graphite, and industrial sodium silicate, which are mixed in a certain proportion and then pressed and dried by a four-column hydraulic press. However, since the lining contains graphite, although it performs well in demolding and heat conduction, it also poses a challenge to the stability of the current due to its conductive properties. It may cause uneven distribution of current in the synthesis cavity, causing temperature and pressure instability, which in turn affects the efficiency and quality of synthetic diamond synthesis, and may even cause hammer cracking and blasting incidents.
[0004] CN114455930A discloses a method for preparing a dolomite composite material, which is mainly made of dolomite, a dispersant, zirconium oxide powder and water glass liquid. The dolomite composite material effectively increases the thermal insulation performance of the liner pipe without affecting the pressure transmission performance of the dolomite, thereby achieving energy saving and efficient production. However, the application cannot solve the problem that current fluctuations during synthesis affect the temperature changes in the synthesis cavity, resulting in cracking hammer explosions.
[0005] Therefore, a new method for preparing dolomite lining composite materials is urgently needed to solve the above-mentioned defects of the prior art. Summary of the invention
[0006] The main purpose of the present invention is to overcome the above-mentioned defects of the prior art and provide a dolomite-lined composite material, which can solve the problem of current fluctuations during synthesis and thus affect the change of temperature in the synthesis cavity, resulting in the problem of hammer explosion, thereby improving the quality and yield of synthetic diamonds.
[0007] The invention also provides a method for preparing the dolomite lining composite material.
[0008] To achieve the above object, the present invention provides the following technical solutions: A dolomite lining composite material mainly comprises dolomite, talcum powder, zinc stearate and sodium silicate, wherein the sum of dolomite, talcum powder and zinc stearate is 100%, talcum powder is 1-5%, zinc stearate is 0.2-1%, and the balance is dolomite.
[0009] Specifically, the amount of sodium silicate used can be 5-10% of the weight of the dolomite lining composite material, and the sodium silicate is preferably industrial sodium silicate.
[0010] Furthermore, the particle size range of the talc is preferably 44-75 μm.
[0011] The present invention also provides a method for preparing the above-mentioned dolomite lining composite material, which specifically comprises the following steps: Step 1: weigh dolomite, talc, zinc stearate and sodium silicate according to proportion; Step 2: The weighed dolomite is placed in a crusher for crushing, then filtered and sieved to obtain dolomite powder; Step 3: placing the crushed dolomite powder into a kneader, then adding talcum powder and zinc stearate, and mixing and stirring at a certain speed in the kneader to obtain a dolomite composite powder; Step 4: Place the mixed dolomite composite powder and sodium silicate in a kneader according to a certain proportion, mix and stir, and dry (drying temperature is 50-80°C, time is 60-120min) to obtain the final dolomite composite powder; Step 5: Place the mixed final dolomite composite powder into a mold on a four-column hydraulic press, and then press it (pressure is 8-14MPa, pressing time is 45-80s) into a dolomite lining embryo; Step 6: Place the pressed dolomite lining blank into a drying oven for drying (drying time 28-30 hours).
[0012] Furthermore, in step 2, the particle size of the dolomite powder obtained can be 125-250 μm.
[0013] Furthermore, in step three, the rotation speed of the kneading machine can be 25-32 rpm, and the mixing and stirring time can be 10-15 min.
[0014] Furthermore, in step 4, the rotation speed of the kneading machine can be 5-14 rpm, and the mixing and stirring time can be 15-30 min.
[0015] Specifically, in step six, the drying temperature can be 200-380°C.
[0016] Compared with the prior art, the present invention has the following beneficial effects: Compared with the prior art, the present invention has the following beneficial effects: 1) The present invention provides a dolomite lining composite material, which is a heat-insulating and pressure-transmitting composite material that can be used for high-temperature and high-pressure synthesis of superhard materials; 2) The present invention uses talcum powder and zinc stearate to replace graphite without affecting the pressure transmission and heat preservation performance of the dolomite lining, which not only has good demoulding properties, but also talcum powder has a smaller thermal conductivity (0.25w / (m·k)) than graphite, which can achieve better thermal insulation and effectively reduce the current fluctuation during synthesis, thereby improving the quality and efficiency of synthetic diamonds, increasing production capacity, reducing hammer consumption, and achieving the advantages of energy saving and efficiency-enhancing production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a process flow chart of the preparation of the dolomite lining composite material of the present invention; Figure 2 The curve of the change of synthetic current when synthesizing diamond; (a) is the traditional dolomite lining, (b) is the dolomite lining composite material described in Example 1, and (c) is the dolomite lining composite material described in Example 2. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is further described in detail below in conjunction with implementation examples, but the protection scope of the present invention is not limited thereto.
[0019] In the following examples, the raw materials used are all common commercial products that can be directly purchased in the art or can be prepared by conventional methods in the art. The particle size range of the talc powder used is 44-75 μm.
[0020] Example 1 A dolomite lining composite material mainly comprises dolomite, talcum powder, zinc stearate and sodium silicate, wherein the sum of dolomite, talcum powder and zinc stearate is 100%, talcum powder is 2%, zinc stearate is 0.3% and dolomite is 97.7%. The sodium silicate is industrial sodium silicate (liquid-4), and the amount of industrial sodium silicate is 5% of the weight of the dolomite lining composite material.
[0021] The preparation method of the above-mentioned dolomite lining composite material (such as Figure 1 As shown), it specifically includes the following steps: 1) Prepare appropriate amounts of dolomite, talcum powder, zinc stearate and industrial sodium silicate according to proportion; 2) Weigh 500g of dolomite and place it in a crusher for crushing, then filter and screen it to obtain dolomite powder with a particle size of 125-250μm; 3) placing the crushed dolomite powder into a kneading machine, then adding talcum powder and zinc stearate (dolomite, talcum powder and zinc stearate are added in a mass ratio of 97.7:2:0.3) and mixing and stirring at a speed of 25 rpm for 15 minutes in the kneading machine to obtain a dolomite composite powder; 4) The mixed dolomite composite powder and industrial sodium silicate were placed in a kneader at a mass ratio of 95:5, mixed and stirred at a speed of 6 rpm for 30 minutes, and dried (drying temperature was 65°C, time was 90 minutes, the same below) to obtain the final dolomite composite powder; 5) Place the mixed dolomite composite powder into a mold on a four-column hydraulic press, and then press it into a dolomite lining embryo through the four-column hydraulic press (pressure 11MPa, pressing time 60s, the same below); 6) Put the pressed dolomite lining embryo into a drying oven for drying (the drying temperature is 300° C., the time is 29 hours, the same below), and obtain the obtained product.
[0022] Under the same conditions, the output of synthetic diamond products produced through high temperature and high pressure is increased by 1% compared to traditional dolomite lining.
[0023] High-temperature and high-pressure synthetic diamond (HPHT synthetic diamond for short) is a technology that converts graphite into diamond under high-temperature and high-pressure conditions. Synthetic current plays a vital role in the process of high-temperature and high-pressure synthetic diamond. It is mainly used to heat the reaction chamber to maintain the required high-temperature conditions. Temperature fluctuations will affect the quality of diamond. Pressure fluctuations can cause cracks inside the diamond. The stability of the synthetic current is crucial to the pressure and temperature stability inside the reaction chamber. The dolomite lining prepared by the present invention can reduce the fluctuation of the synthetic current during the synthesis of diamond, thereby improving the quality and efficiency of synthetic diamond. The traditional dolomite lining is composed of dolomite, graphite, and industrial sodium silicate, which are mixed and pressed and dried by a four-column press. The innovation of the present invention lies in replacing the graphite used with talcum powder and zinc stearate.
[0024] Example 2 A dolomite lining composite material mainly comprises dolomite, talcum powder, zinc stearate and sodium silicate, wherein the sum of dolomite, talcum powder and zinc stearate is 100%, talcum powder is 2.1%, zinc stearate is 0.4% and dolomite is 97.5%. The sodium silicate is industrial sodium silicate (liquid-4), and the amount of industrial sodium silicate is 5% of the weight of the dolomite lining composite material.
[0025] The preparation method of the upper dolomite lining composite material specifically comprises the following steps: 1) Prepare appropriate amounts of dolomite, talcum powder, zinc stearate and industrial sodium silicate according to proportion; 2) Weigh 500g of dolomite and place it in a crusher for crushing, then filter and screen it to obtain dolomite powder with a particle size of 135-220μm; 3) placing the crushed dolomite powder into a kneading machine, then adding talcum powder and zinc stearate (dolomite, talcum powder and zinc stearate are added in a mass ratio of 97.5:2.1:0.4) and mixing and stirring at a speed of 32 rpm for 15 minutes in the kneading machine to obtain a dolomite composite powder; 4) placing the mixed dolomite composite powder and industrial sodium silicate in a mass ratio of 95:5 into a kneader at a speed of 12 rpm for 30 minutes, and drying to obtain a final dolomite composite powder; 5) placing the mixed dolomite composite powder into a mold on a four-column hydraulic press, and then pressing it into a dolomite lining embryo through the four-column hydraulic press; 6) Put the pressed dolomite lining embryo into a drying oven for drying (the drying temperature is 300° C.).
[0026] Under the same conditions, the output of synthetic diamond products produced through high temperature and high pressure is increased by 1.5% compared to traditional dolomite lining.
[0027] Figure 2 The following Table 1 shows the change in synthesis current during diamond synthesis. Figure 2 It can be seen that the synthetic current fluctuation amplitude using the traditional dolomite lining is relatively large, resulting in instability of the temperature and pressure of the synthetic cavity, causing the quality of the synthetic diamond to deteriorate and the efficiency to decrease. The dolomite lining prepared by the present invention can effectively reduce the fluctuation of the synthetic current, as shown in Table 1 below. The synthetic current fluctuation of the dolomite lining described in Examples 1 and 2 is small, the temperature and pressure of the synthetic cavity are relatively stable, and the quality and efficiency of the synthetic diamond are improved. The dolomite lining prepared by the present invention can effectively reduce the fluctuation of the synthetic current.
[0028] Table 1 Current fluctuations of different syntheses Figure 2 It is shown in the figure that compared with the traditional dolomite lining, the dolomite lining prepared by the present invention has a smaller fluctuation amplitude of the synthetic diamond current, has a smaller impact on the temperature and pressure of the synthesis cavity, and can effectively improve the quality of synthetic diamond, especially the ratio of excellent crystals is significantly improved (see Table 2).
[0029] Table 2 Quality of diamonds synthesized from different sources
Claims
1. A dolomite lined composite material, It is characterized in that It mainly includes dolomite, talc, zinc stearate and sodium silicate, wherein the sum of dolomite, talc and zinc stearate is 100%, talc is 1-5%, zinc stearate is 0.2-1%, and the balance is dolomite.
2. The dolomite lined composite material according to claim 1, It is characterized in that The dosage of the sodium silicate is 5-10% of the weight of the dolomite lining composite material, and the sodium silicate is industrial sodium silicate.
3. The dolomite lined composite material according to claim 1, It is characterized in that The particle size of the talc powder is in the range of 44-75 μm.
4. The method for preparing the dolomite lined composite material according to any one of claims 1 to 3, It is characterized in that The steps include: Step 1: weigh dolomite, talc, zinc stearate and sodium silicate according to proportion; Step 2: The weighed dolomite is placed in a crusher for crushing, then filtered and sieved to obtain dolomite powder; Step 3: placing the crushed dolomite powder into a kneader, then adding talcum powder and zinc stearate, and mixing and stirring at a certain speed in the kneader to obtain a dolomite composite powder; Step 4: placing the mixed dolomite composite powder and sodium silicate in a kneader according to a certain proportion, mixing and stirring, and drying to obtain a final dolomite composite powder; Step 5: placing the mixed final dolomite composite powder into a mold on a four-column hydraulic press, and then pressing it into a dolomite lining embryo through the four-column hydraulic press; Step six: put the pressed dolomite lining blank into a drying box for drying.
5. The method for preparing the dolomite lined composite material according to claim 4, It is characterized in that In step 2, the particle size of the obtained dolomite powder is 125-250 μm.
6. The method for preparing the dolomite lined composite material according to claim 4, It is characterized in that In step 3, the rotation speed of the kneading machine is 25-32 rpm, and the mixing time is 10-15 min.
7. The method for preparing the dolomite lined composite material according to claim 4, It is characterized in that In step 4, the rotation speed of the kneading machine is 5-14 rpm, and the mixing time is 15-30 min.
8. The method for preparing the dolomite lined composite material according to claim 4, It is characterized in that In step six, the drying temperature is 200-380°C.