Waterproof tin package and preparation method thereof

Through the double-layer structure of composite aerogel and impregnated mixed wax, the single performance and safety problems of existing plastic packaging bags are solved, and waterproof, antibacterial and antioxidant packaging bags are realized, which improves service life and durability.

CN119038949APending Publication Date: 2024-11-29毛佳耀
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410936097.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing plastic packaging bags have problems such as wrinkles, poor transparency, uneven thickness, and many fish eyes. They also contain toxic plasticizers, which affect food quality and human health. Their single performance cannot be distinguished based on the special properties of different products.

Method used

Using composite aerogel as the inner layer and impregnated mixed wax as the outer layer, hydrolyzing and oxidizing the tin salt to form a composite tin dioxide and graphene sheet layer, combined with ammonia water/ethanol spray modification, prepare waterproof tin packaging bags, and use gastrointestinal Acid esterification with carnauba wax and nanosilica fillers improve mechanical and hydrophobic properties.

Benefits of technology

It realizes waterproof, not easy to break, and has a long service life. It has antibacterial and antioxidant effects, improves the mechanical properties and hydrophobic properties of the packaging bag, and improves its durability and storage in use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941376180000091
    Figure BDA0004941376180000091
Patent Text Reader

Abstract

The invention discloses a waterproof tin package and a preparation method thereof, and relates to the technical field of packaging bags. Firstly, gallic acid and carnauba wax ester are subjected to chemical reaction and mixed to obtain a mixed wax raw material, the content of fatty alcohol in the mixed wax raw material is reduced, the brittleness is reduced, the toughness is improved, and the packaging bag is not prone to cracking in the using process; the nano silicon dioxide is combined with hydroxyl of gallic acid and is uniformly dispersed to form a rough surface, so that the mechanical property and hydrophobic property of the paper-based packaging material are improved. Secondly, preparing aerogel by compounding tin dioxide and a graphene sheet layer, and preparing an inner layer of the packaging bag; ammonia water and ethyl alcohol are mixed and sprayed for modification, so that the hydrophobicity is improved; graphene and gallic acid are synergistically antibacterial, so that the whole packaging bag is easier to store and not prone to mildewing; the inner layer and the outer layer are not prone to wrinkling and breaking, and can be repeatedly used. The prepared packaging bag has the effects of being waterproof, not prone to damage and long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging bags, in particular to a waterproof tin package and a preparation method thereof. Background Art

[0002] Packaging bags refer to bags used to package various items, making it convenient for goods to be transported and stored during the production and circulation process. They are widely used in daily life and industrial production. Existing packaging bags are generally made of paper or plastic film, which is formed by pressing two paper or plastic films together, and the items are stored through the internal cavity. Plastic packaging bags have good storage and portability, and can store and transport products quickly and efficiently. They are increasingly widely used in our daily production and life. Plastic film is a common daily necessity. The plastic film on the market is mainly polyethylene plastic film, but some products have problems such as wrinkles, poor transparency, uneven thickness, and many fish eyes in the film. Some plastic films are used for food packaging, but they contain toxic plasticizers, which affect the quality of food and endanger human health.

[0003] Currently available packaging bags offer a single performance profile, often lacking differentiation based on the specific properties of the product. To continuously improve packaging safety, the present invention has designed a waterproof tin packaging bag. This invention leverages graphene aerogel, combining the mechanical stability and hydrophobicity of graphene with the ultralightness and high porosity of aerogel, creating a new material for packaging bags that simultaneously delivers the advantages of being lightweight, waterproof, and having a long service life. Summary of the Invention

[0004] The purpose of the present invention is to provide a waterproof tin package and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a waterproof tin packaging, which is a packaging bag prepared with a composite aerogel as the inner layer and an outer layer impregnated with mixed wax.

[0006] Furthermore, the composite aerogel is an aerogel formed by hydrolyzing and oxidizing tin salt to form tin dioxide and composite with graphene sheets, and then modified by ammonia / ethanol spraying.

[0007] Furthermore, the mixed wax is prepared by esterifying tartaric acid and carnauba wax, and then adding inorganic filler nano-silica to modify the mixed wax liquid as the outer layer.

[0008] Furthermore, a method for preparing a waterproof tin package includes the following steps:

[0009] (1) In a three-necked flask equipped with a thermometer and a solvent circulation device, add 1 part of gallic acid, 0.5-50 parts of carnauba wax, 0.05-0.09 parts of acidic catalyst, and 4-6 parts of tetrahydrofuran as reaction solvent, and stir magnetically at a speed of 50-150 rpm. Slowly heat to 110-130°C on an oil bath to circulate the catalyst. The reaction is carried out for 12-18 hours to complete the reaction. The catalyst in the reaction solution is recovered under reduced pressure, and the remaining solid is filtered under reduced pressure. The reaction mixture is then treated with 10% concentrated The mixture was washed several times with a NaHCO3 aqueous solution and then washed three times with deionized water until neutral. The crude product was recrystallized twice with a mixed solvent of toluene and water to obtain an intermediate product; 1-3 parts of the intermediate product were added to 5 parts of anhydrous ethanol and heated in a water bath at 80-100°C for 30 minutes to obtain a mixed solution; 0.1-0.2 parts of hydrophobic fumed silica were added to the mixed solution, and magnetic stirring was continued for 15-45 minutes at a stirring speed of 200-400 rpm to obtain a mixed wax liquid;

[0010] (2) 5-10 parts of graphene oxide are mixed with 100-200 parts of deionized water, heated to 80-100°C and stirred for 1-2 hours; then 10 parts of 30% hydrogen peroxide are added, stirred for 15-45 minutes and filtered, and then the filter cake is centrifuged and washed 5 times with 3% hydrochloric acid, and then centrifuged and washed 5 times with deionized water. The washed colloidal product is added to 80-100 parts of deionized water and ultrasonically dispersed at a power of 200W for 20 minutes to obtain graphene oxide. The invention discloses a lamellar hydrosol; 10 parts of graphene oxide lamellar hydrosol and ethylene glycol are mixed in a volume ratio of 1:40, and ultrasonically dispersed at 200W power for 20 minutes, and then 3-5 parts of stannous chloride dihydrate are added to the obtained sol, and the obtained reactant is refluxed and stirred at 100-140°C for 1 hour at a stirring speed of 60rpm, and then centrifuged to remove unreacted tin salt, and the obtained precipitate is washed 3-5 times with deionized water to obtain a composite; 0.4-0.8 parts of the composite are mixed with 10 parts of deionized water, and ultrasonically dispersed at 200W power for 20 minutes. After 15 minutes, 0.1-0.3 parts of sodium dodecylbenzenesulfonate aqueous solution was added to the graphene oxide dispersion and stirred at a speed of 10,000 rpm for 15-45 minutes to obtain a foam; the foam was placed at 80°C for a reduction reaction for 6 hours, and then naturally cooled to 25°C to obtain a mixed hydrogel; the mixed hydrogel was soaked and washed with a 1 vol% ethanol aqueous solution for 24 hours at a solid-liquid ratio of 1:5 to obtain a washed mixed hydrogel; the washed mixed hydrogel was taken out and placed in a freezer at -45°C for 2 hours , then take it out and heat it to 25℃ to melt, and after drying at room temperature and pressure for 5 hours, aerogel with a thickness of 0.05-0.15cm is obtained; under nitrogen gas protection, the obtained aerogel is placed in a tubular furnace at 600-800℃ and heated for 1-2 hours, taken out and cooled to room temperature; the homemade modified solution is micro-atomized by high-pressure gas assistance, with a spray particle size of 30-50μm and a spray flow rate of 60-100ml / min. The aerogel is spray-modified for 30-60 minutes to prepare a modified composite aerogel as the inner layer;

[0011] (3) Immerse the prepared inner layer in the mixed wax liquid, with the dipping amount being 1-5g / m 2 , after dipping for 3-5 minutes, drying at 35°C for 30-60 minutes, and then placing in an environment with a relative humidity of 50% and a temperature of 25°C for 24 hours to obtain a multi-layer packaging bag material containing tin; the multi-layer packaging bag material containing tin is color-printed and bag-made to obtain a waterproof tin packaging bag.

[0012] Furthermore, the acidic catalyst in step (1) is one of p-toluenesulfonic acid, copper sulfate, and cerium sulfate.

[0013] Furthermore, in step (1), the oil bath heating temperature rise rate is 10°C / min.

[0014] Furthermore, in the step (1), the volume ratio of toluene to water in the mixed solvent is 4:1.

[0015] Furthermore, the centrifugal washing speed in step (2) is 5000 rpm.

[0016] Furthermore, the concentration of the sodium dodecylbenzenesulfonate aqueous solution in step (2) is 50 mg / ml.

[0017] Furthermore, the homemade modified solution in step (2) is obtained by mixing 20 vol% ammonia solution and 90 vol% ethanol solution in a volume ratio of 4-8:1.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention uses composite aerogel as the inner layer and the outer layer is impregnated with mixed wax to prepare a waterproof tin packaging bag, so as to achieve the effects of being waterproof, not easy to be damaged and having a long service life.

[0020] First, gallic acid is mixed with carnauba wax, and during a heating process, the carboxylic acid groups contained in the gallic acid undergo an esterification reaction with the carnauba wax to obtain a mixed wax raw material; the esterification reaction not only reduces the fatty alcohol content in the mixed wax, but also further reduces its brittleness and improves its toughness based on the excellent mechanical properties of the carnauba wax, making the packaging bag less likely to crack during use, but also the gallic acid ester compounds generated by the esterification have high-efficiency antioxidant properties, making the packaging bag protected by the mixed wax coating less likely to age during use, thereby increasing the overall service life of the packaging bag; nano-silica is added to the mixed wax as an inorganic filler, and is adsorbed and bonded with the organic gallic acid through hydroxyl groups, thereby improving the dispersibility of the silica particles, which can act more evenly on the mixed wax coating of the packaging paper, have a relatively large surface area and excellent mechanical strength, and as fine particles, increase the surface roughness of the composite wax coating of the packaging paper, and can reduce the surface energy, thereby achieving the effect of simultaneously improving the mechanical properties and hydrophobic properties of the paper-based packaging material.

[0021] Secondly, tin salt is hydrolyzed and oxidized to form tin dioxide, which is then composited with graphene sheets to prepare aerogel, and the inner layer of the packaging bag is prepared; through a growth environment composited with water and organic solvents, the morphology of tin dioxide is controlled, so that in the sheet composite aerogel material prepared by the present invention, the tin dioxide nanoparticles are evenly distributed and spherical, thereby increasing its roughness and achieving a hydrophobic effect; the prepared aerogel is then modified by spraying a mixture of ammonia water and ethanol to improve its hydrophobicity; in addition, both the graphene in the inner layer and the gallic acid in the outer layer have antibacterial effects, so the packaging bag as a whole is easier to store and less likely to mold; the double-layer structure of the packaging bag relies on the high elasticity of the inner layer aerogel, which is composited with the modified mixed wax coating, to improve the wrinkles and breakage of the packaging bag during use, so that it can be reused repeatedly. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are provided in detail. The test methods for various indicators of a waterproof tin package prepared in the following examples are as follows:

[0024] Mechanical properties: The radial strength and latitudinal strength of the samples prepared in the examples and comparative examples were tested according to the GB / T8946-2013 standard; the maximum tensile stress was measured according to the GB / T1040-2006 standard.

[0025] Waterproof performance: The samples prepared in the examples and comparative examples were subjected to contact angle tests.

[0026] Example 1

[0027] (1) In a three-necked flask equipped with a thermometer and a solvent circulation device, 1 part of gallic acid, 0.5 parts of carnauba wax, 0.05 parts of acidic catalyst p-toluenesulfonic acid, and 4 parts of reaction solvent tetrahydrofuran were added, and magnetic stirring was performed at a stirring speed of 50 rpm. The mixture was slowly heated to 110°C on an oil bath at a heating rate of 10°C / min to circulate the catalyst. The reaction was completed for 12 hours, and the catalyst in the reaction solution was recovered under reduced pressure. The remaining solid was filtered under reduced pressure and washed several times with a 10% concentration of NaHCO3 aqueous solution and then washed 3 times with deionized water until neutral. The crude product was recrystallized twice with a mixed solvent of toluene and water, with a volume ratio of toluene to water of 4:1, to obtain an intermediate product; 1 part of the intermediate product was added to 5 parts of anhydrous ethanol and heated in a water bath at 80°C for 30 minutes to obtain a mixed solution; 0.1 part of hydrophobic fumed silica was added to the mixed solution, and magnetic stirring was performed for 15 minutes at a stirring speed of 200 rpm to obtain a mixed wax liquid;

[0028] (2) 5 parts of graphene oxide were mixed with 100 parts of deionized water, heated to 80°C and stirred for 1 hour; then 10 parts of 30% hydrogen peroxide were added, stirred for 15 minutes and filtered, and the filter cake was centrifuged and washed 5 times with 3% hydrochloric acid at a speed of 5000 rpm, and then centrifuged and washed 5 times with deionized water. The washed colloidal product was added to 80 parts of deionized water and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain a graphene oxide sheet hydrosol; 10 parts of graphene oxide were added to the mixture, and the mixture was filtered and washed 5 times with 3% hydrochloric acid at a speed of 5000 rpm. The graphene sheet aqueous sol was mixed with ethylene glycol in a volume ratio of 1:40, and after ultrasonic dispersion at 200W power for 20 minutes, 3 parts of stannous chloride dihydrate were added to the obtained sol, and the obtained reactant was refluxed and stirred at 100°C for 1 hour at a stirring speed of 60rpm, and then centrifuged to remove unreacted tin salt at a speed of 5000rpm. The obtained precipitate was washed three times with deionized water to obtain a composite; 0.4 parts of the composite was mixed with 10 parts of deionized water, and after ultrasonic dispersion at 200W power for 15 minutes, 0.1 parts of 50m g / ml sodium dodecylbenzenesulfonate aqueous solution was added to the graphene oxide dispersion and stirred at a speed of 10000 rpm for 15 minutes to obtain a foam; the foam was placed at 80 ° C for reduction reaction for 6 hours, and then naturally cooled to 25 ° C to obtain a mixed hydrogel, and the mixed hydrogel was soaked and washed with 1 vol% ethanol aqueous solution for 24 hours with a solid-liquid ratio of 1:5 to obtain a washed mixed hydrogel; the washed mixed hydrogel was taken out and placed in a -45 ° C freezer for 2 hours, and then taken out and heated to 25 ° C to melt, and then the mixed hydrogel was taken out and heated to 25 ° C to melt. After press drying for 5 hours, an aerogel with a thickness of 0.05 cm was obtained. Under nitrogen protection, the obtained aerogel was placed in a tube furnace and heated for 1 hour at 600°C, then taken out and cooled to room temperature. A homemade modified solution was obtained by mixing 20 vol% ammonia aqueous solution and 90 vol% ethanol aqueous solution in a volume ratio of 4:1. The homemade modified solution was micro-atomized by high-pressure gas with a spray particle size of 30 μm and a spray flow rate of 60 ml / min. The aerogel was spray-modified for 30 minutes to prepare a modified composite aerogel as the inner layer.

[0029] (3) Immerse the prepared inner layer in the mixed wax liquid, with the dipping amount being 1g / m 2 After immersing for 3 minutes, drying at 35°C for 30 minutes, and then placing it in an environment with a relative humidity of 50% and a temperature of 25°C for 24 hours to obtain a multi-layer packaging bag material containing tin; the multi-layer packaging bag material containing tin is color-printed and bag-made to obtain a waterproof tin packaging bag.

[0030] Example 2

[0031] (1) In a three-necked flask equipped with a thermometer and a solvent circulation device, 1 part of gallic acid, 25 parts of carnauba wax, 0.07 parts of acidic catalyst copper sulfate, and 5 parts of reaction solvent tetrahydrofuran were added, and magnetic stirring was performed at a stirring speed of 100 rpm. The mixture was slowly heated to 120°C on an oil bath at a heating rate of 10°C / min to circulate the catalyst. The reaction was completed for 15 hours, and the catalyst in the reaction solution was recovered under reduced pressure. The remaining solid was filtered under reduced pressure and washed several times with a 10% concentration of NaHCO3 aqueous solution and then washed 3 times with deionized water until neutral. The crude product was recrystallized twice with a mixed solvent of toluene and water, with a volume ratio of toluene to water of 4:1, to obtain an intermediate product; 2 parts of the intermediate product were added to 5 parts of anhydrous ethanol and heated in a water bath at 90°C for 30 minutes to obtain a mixed solution; 0.15 parts of hydrophobic fumed silica were added to the mixed solution, and then magnetic stirring was performed for 30 minutes at a stirring speed of 300 rpm to obtain a mixed wax liquid;

[0032] (2) 7.5 parts of graphene oxide were mixed with 150 parts of deionized water, heated to 90°C and stirred for 1.5 hours; then 10 parts of 30% hydrogen peroxide were added, stirred for 30 minutes and filtered, and the filter cake was centrifuged and washed 5 times with 3% hydrochloric acid at a speed of 5000 rpm, and then centrifuged and washed 5 times with deionized water. The washed colloidal product was added to 90 parts of deionized water and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain a graphene oxide sheet hydrosol; 10 parts of The graphene oxide sheet aqueous sol was mixed with ethylene glycol in a volume ratio of 1:40, and after ultrasonic dispersion at 200W power for 20 minutes, 4 parts of stannous chloride dihydrate were added to the obtained sol, and the obtained reactant was refluxed and stirred at 120°C for 1 hour at a stirring speed of 60rpm, and then centrifuged to remove the unreacted tin salt at a speed of 5000rpm. The obtained precipitate was washed 4 times with deionized water to obtain a composite; 0.6 parts of the composite was mixed with 10 parts of deionized water, and after ultrasonic dispersion at 200W power for 15 minutes, 0.2 parts of 5 0mg / ml sodium dodecylbenzenesulfonate aqueous solution was added to graphene oxide dispersion, and stirred at a speed of 10000rmp for 30min to obtain a foam; the foam was placed at 80℃ for reduction reaction for 6h, and then naturally cooled to 25℃ to obtain a mixed hydrogel, and the mixed hydrogel was soaked and washed with 1vol% ethanol aqueous solution for 24h, with a solid-liquid ratio of 1:5, to obtain a washed mixed hydrogel; the washed mixed hydrogel was taken out and placed in a -45℃ freeze treatment for 2h, and then taken out and heated to 25℃ to melt, and then cooled to room temperature and normal temperature. After press drying for 5 hours, an aerogel with a thickness of 0.1 cm was obtained. The obtained aerogel was placed in a tubular furnace under nitrogen protection and heated for 1.5 hours at 700°C, then taken out and cooled to room temperature. A homemade modified solution was obtained by mixing 20 vol% ammonia aqueous solution with 90 vol% ethanol aqueous solution in a volume ratio of 6:1. The homemade modified solution was micro-atomized with high-pressure gas assistance, with a spray particle size of 40 μm and a spray flow rate of 80 ml / min. The aerogel was spray-modified for 45 minutes to prepare a modified composite aerogel as the inner layer.

[0033] (3) Immerse the prepared inner layer in the mixed wax liquid, with the dipping amount being 3g / m 2 After immersing for 4 minutes, it was dried at 35°C for 45 minutes, and then placed in an environment with a relative humidity of 50% and a temperature of 25°C for 24 hours to obtain a multi-layer packaging bag material containing tin; the multi-layer packaging bag material containing tin was color-printed and bag-made to obtain a waterproof tin packaging bag.

[0034] Example 3

[0035] (1) In a three-necked flask equipped with a thermometer and a solvent circulation device, 1 part of gallic acid, 50 parts of carnauba wax, 0.09 parts of acidic catalyst cerium sulfate, and 6 parts of reaction solvent tetrahydrofuran were added, and magnetic stirring was performed at a stirring speed of 150 rpm. The mixture was slowly heated to 130°C on an oil bath at a heating rate of 10°C / min to circulate the catalyst. The reaction was completed for 18 hours, and the catalyst in the reaction solution was recovered under reduced pressure. The remaining solid was filtered under reduced pressure and washed several times with a 10% concentration of NaHCO3 aqueous solution and then washed 3 times with deionized water until neutral. The crude product was recrystallized twice with a mixed solvent of toluene and water, with a volume ratio of toluene to water of 4:1, to obtain an intermediate product; 3 parts of the intermediate product were added to 5 parts of anhydrous ethanol and heated in a water bath at 100°C for 30 minutes to obtain a mixed solution; 0.2 parts of hydrophobic fumed silica were added to the mixed solution, and then magnetic stirring was performed for 45 minutes at a stirring speed of 400 rpm to obtain a mixed wax liquid;

[0036] (2) 10 parts of graphene oxide were mixed with 200 parts of deionized water, heated to 100 ° C and stirred for 2 hours; then 10 parts of 30% hydrogen peroxide were added, stirred for 45 minutes and filtered, and the filter cake was centrifuged and washed 5 times with 3% hydrochloric acid at a speed of 5000 rpm, and then centrifuged and washed 5 times with deionized water. The washed colloidal product was added to 100 parts of deionized water and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain a graphene oxide sheet hydrosol; 10 parts of graphene oxide were added to 200 parts of deionized water and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain a graphene oxide sheet hydrosol; The graphene sheet aqueous sol was mixed with ethylene glycol in a volume ratio of 1:40, and after ultrasonic dispersion at 200W power for 20 minutes, 5 parts of stannous chloride dihydrate were added to the obtained sol, and the obtained reactant was refluxed and stirred at 140°C for 1 hour at a stirring speed of 60 rpm, and then centrifuged to remove the unreacted tin salt at a speed of 5000 rpm. The obtained precipitate was washed 5 times with deionized water to obtain a composite; 0.8 parts of the composite was mixed with 10 parts of deionized water, and after ultrasonic dispersion at 200W power for 15 minutes, 0.3 parts of 50 10000 rpm, stirring at 10000 rpm for 45 min to obtain a foam; the foam was placed at 80 ° C for 6 h for reduction reaction, and then naturally cooled to 25 ° C to obtain a mixed hydrogel; the mixed hydrogel was soaked and washed with 1 vol% ethanol aqueous solution for 24 h, with a solid-liquid ratio of 1:5, to obtain a washed mixed hydrogel; the washed mixed hydrogel was taken out and placed in a -45 ° C freezer for 2 h, then taken out and heated to 25 ° C to melt, and then heated to room temperature and normal temperature. After press drying for 5 hours, an aerogel with a thickness of 0.15 cm was obtained. The obtained aerogel was placed in a tubular furnace under nitrogen protection and heated for 2 hours at 800°C, then taken out and cooled to room temperature. A homemade modified solution was obtained by mixing 20 vol% ammonia aqueous solution and 90 vol% ethanol aqueous solution in a volume ratio of 8:1. The homemade modified solution was micro-atomized with high-pressure gas assistance at a spray particle size of 50 μm and a spray flow rate of 100 ml / min. The aerogel was spray-modified for 60 minutes to prepare a modified composite aerogel as the inner layer.

[0037] (3) Immerse the prepared inner layer in the mixed wax liquid, with the immersion amount being 5g / m 2 After immersing for 5 minutes, it is dried at 35°C for 60 minutes, and then placed in an environment with a relative humidity of 50% and a temperature of 25°C for 24 hours to obtain a multi-layer packaging bag material containing tin; the multi-layer packaging bag material containing tin is color-printed and bag-made to obtain a waterproof tin packaging bag.

[0038] Comparative Example 1

[0039] The difference between Comparative Example 1 and Example 2 is that gallic acid is not added, specifically, step (1) is different, and step (1) is changed to: in a three-necked flask equipped with a thermometer and a solvent circulation device, 25 parts of carnauba wax are added to 5 parts of anhydrous ethanol, and heated in a water bath at 90°C for 30 minutes to obtain a mixed solution; 0.15 parts of hydrophobic fumed silica are taken and added to the mixed solution, and then magnetically stirred for 30 minutes at a stirring speed of 300 rpm to obtain a mixed wax liquid; the remaining steps are the same as in Example 2.

[0040] Comparative Example 2

[0041] The difference between Comparative Example 2 and Example 2 is that nano-silica is not added, specifically the difference in step (1). Step (1) is changed to: in a three-necked flask equipped with a thermometer and a solvent circulation device, 1 part of gallic acid, 25 parts of carnauba wax, 0.07 parts of acidic catalyst copper sulfate, and 5 parts of reaction solvent tetrahydrofuran are added, and magnetic stirring is performed at a stirring speed of 100 rpm. The mixture is slowly heated to 120° C. on an oil bath at a heating rate of 10° C. / min to circulate the catalyst. The reaction is completed for 15 hours, and the catalyst in the reaction solution is recovered under reduced pressure. The remaining solid is filtered under reduced pressure, washed several times with a 10% concentration of NaHCO3 aqueous solution, and then washed three times with deionized water until neutral. The crude product is recrystallized twice with a mixed solvent of toluene and water, and the volume ratio of toluene to water is 4:1 to obtain a mixed wax liquid; the remaining steps are the same as in Example 2.

[0042] Comparative Example 3

[0043] The difference between Comparative Example 3 and Example 2 is that no tin salt intercalation is added, specifically the difference in step (2). Step (2) is changed to: 7.5 parts of graphene oxide are mixed with 150 parts of deionized water, heated to 90°C and stirred for 1.5h; then 10 parts of 30% hydrogen peroxide are added, stirred for 30min and filtered, and then the obtained filter cake is centrifuged and washed 5 times with hydrochloric acid having a concentration of 3% by mass at a speed of 5000rpm, and then centrifuged and washed 5 times with deionized water. The washed colloidal product is added to 90 parts of deionized water and ultrasonically dispersed at a power of 200W for 20min to obtain a graphene oxide dispersion; 0.2 parts of a 50mg / ml aqueous solution of sodium dodecylbenzenesulfonate are added to the graphene oxide dispersion and stirred at a speed of 10000rmp for 30min to obtain a foam; the foam is placed at 80°C for reduction reaction 6h, and then naturally cooled to 25°C to obtain a hydrogel, and the hydrogel was soaked and washed with a 1vol% ethanol aqueous solution for 24h, with a solid-liquid ratio of 1:5 to obtain a washed hydrogel; the washed hydrogel was taken out and placed at -45°C for freezing treatment for 2h, then taken out and heated to 25°C to melt, and dried at room temperature and pressure for 5h to obtain an aerogel with a thickness of 0.1cm; under nitrogen gas protection, the obtained aerogel was placed in a tubular furnace at 700°C and heated for 1.5h, taken out and cooled to room temperature; 20vol% ammonia aqueous solution and 90vol% ethanol aqueous solution were mixed in a volume ratio of 6:1 to obtain a homemade modified solution; the homemade modified solution was subjected to high-pressure gas-assisted micro-atomization, with a spray particle size of 40μm and a spray flow rate of 80ml / min, and the aerogel was spray-modified for 45min to prepare a modified composite aerogel as the inner layer; the remaining steps were the same as in Example 2.

[0044] Comparative Example 4

[0045] The difference between Comparative Example 4 and Example 2 is that the modification is not performed by mixing ammonia and ethanol. Specifically, step (2) is changed to: 7.5 parts of graphene oxide are mixed with 150 parts of deionized water, heated to 90° C. and stirred for 1.5 hours; then 10 parts of 30% hydrogen peroxide are added, stirred for 30 minutes and filtered, and the filter cake is then centrifuged and washed 5 times with 3% hydrochloric acid at a speed of 5000 rpm, and then centrifuged and washed 5 times with deionized water. The washed colloidal product was added to 90 parts of deionized water and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain a graphene oxide sheet hydrosol; 10 parts of the graphene oxide sheet hydrosol was mixed with ethylene glycol at a volume ratio of 1:40, and ultrasonically dispersed at a power of 200 W for 20 minutes. Then, 4 parts of stannous chloride dihydrate were added to the obtained sol, and the obtained reactants were refluxed at 120° C. for 1 hour at a stirring speed of 60 rpm, and then centrifuged to remove unreacted tin salts at a speed of 5. 000rpm, the obtained precipitate was washed 4 times with deionized water to prepare a composite; 0.6 parts of the composite was mixed with 10 parts of deionized water, and after ultrasonication at 200W for 15 minutes, 0.2 parts of a 50 mg / ml aqueous solution of sodium dodecylbenzenesulfonate was added to the graphene oxide dispersion, and stirred at a speed of 10000rpm for 30 minutes to obtain a foam; the foam was placed at 80℃ for reduction reaction for 6 hours, and then naturally cooled to 25℃ to obtain a mixed hydrogel, which was then used to prepare a composite. The washed mixed hydrogel was immersed in a 1 vol% ethanol aqueous solution for 24 hours with a solid-liquid ratio of 1:5 to obtain a washed mixed hydrogel; the washed mixed hydrogel was taken out and frozen at -45°C for 2 hours, then taken out and heated to 25°C to melt, and dried at room temperature and pressure for 5 hours to obtain an aerogel with a thickness of 0.1 cm; under nitrogen gas protection, the obtained aerogel was placed in a tubular furnace at 700°C and heated for 1.5 hours, taken out and cooled to room temperature to prepare a composite aerogel as the inner layer; the remaining steps were the same as in Example 2.

[0046] Effect Examples

[0047] Table 1 below shows the performance analysis results of a waterproof tin package using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0048] Table 1

[0049]

[0050] From the comparison of the experimental data of mechanical properties of the embodiment and the comparative example, it can be found that the present invention mixes gallic acid with carnauba wax, and during the heating process, the carboxylic acid groups contained in the gallic acid undergo an esterification reaction with the carnauba wax to obtain a mixed wax raw material; the esterification reaction not only reduces the fatty alcohol content in the mixed wax, but also further reduces its brittleness and improves its toughness based on the excellent mechanical properties of the carnauba wax, making the packaging bag less likely to crack during use, and the gallic acid ester compounds generated by esterification have high antioxidant properties, making the packaging bag protected by the mixed wax coating less likely to age during use, thereby improving the overall service life of the packaging bag; nano-silicon dioxide is added to the mixed wax as an inorganic filler, and is adsorbed and bonded with organic gallic acid through hydroxyl groups, improving the dispersibility of the silicon dioxide particles, and can act more evenly on the mixed wax coating of the packaging paper, which has excellent mechanical strength and improves its durability. From the comparison of the experimental data of hydrophobic properties of the embodiment and the comparative example, it can be found that the present invention uses fine silicon dioxide particles to improve the surface roughness of the composite wax coating of the packaging paper, and can reduce the surface energy, thereby achieving the effect of simultaneously improving the mechanical properties and hydrophobic properties of the paper-based packaging material. Secondly, tin salt is hydrolyzed and oxidized to form tin dioxide, which is then composited with graphene sheets to prepare aerogel, and the inner layer of the packaging bag is prepared; through a growth environment composited with water and organic solvents, the morphology of tin dioxide is controlled, so that in the sheet composite aerogel material prepared by the present invention, the tin dioxide nanoparticles are evenly distributed and spherical, thereby increasing its roughness and achieving a hydrophobic effect; the prepared aerogel is then modified by spraying a mixture of ammonia water and ethanol to improve its hydrophobicity; in addition, both the graphene in the inner layer and the gallic acid in the outer layer have antibacterial effects, so the packaging bag as a whole is easier to store and less likely to mold; the double-layer structure of the packaging bag relies on the high elasticity of the inner layer aerogel, which is composited with the modified mixed wax coating, to improve the wrinkles and breakage of the packaging bag during use, so that it can be reused repeatedly.

[0051] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims, not the foregoing description, and all variations within the meaning and range of equivalents of the claims are intended to be encompassed therein. Any reference in a claim should not be construed as limiting the claim to which it relates.

Claims

1. A waterproof tin package, characterized in that: The packaging is a packaging bag with a composite aerogel as an inner layer and an outer layer impregnated with mixed wax.

2. A waterproof tin packaging according to claim 1, characterized in that: The composite aerogel is an aerogel formed by hydrolyzing and oxidizing tin salt to form tin dioxide and composite with graphene sheets, and then modified by ammonia / ethanol spraying.

3. The waterproof tin packaging according to claim 1, characterized in that: The mixed wax is prepared by mixing and esterifying edible acid and carnauba wax, and then adding inorganic filler nano-silicon dioxide to modify the mixed wax liquid as the outer layer.

4. A method for preparing a waterproof tin package, characterized in that: The method comprises the following preparation steps: (1) In a three-necked flask equipped with a thermometer and a solvent circulation device, add 1 part of gallic acid, 0.5-50 parts of carnauba wax, 0.05-0.09 parts of acidic catalyst, and 4-6 parts of tetrahydrofuran, a reaction solvent, and perform magnetic stirring at a stirring speed of 50-150 rpm. Slowly heat to 110-130° C. on an oil bath to circulate the catalyst. The reaction is carried out for 12-18 hours to complete the reaction. The catalyst in the reaction solution is recovered under reduced pressure, and the remaining solid is filtered under reduced pressure and then treated with 10% concentrated The mixture was washed with NaHCO3 aqueous solution for several times, and then washed with deionized water for 3 times until neutral, and the crude product was recrystallized twice with a mixed solvent of toluene and water to obtain an intermediate product; 1-3 parts of the intermediate product were added to 5 parts of anhydrous ethanol, and heated in a water bath at 80-100°C for 30 minutes to obtain a mixed solution; 0.1-0.2 parts of hydrophobic fumed silica were added to the mixed solution, and then magnetically stirred for 15-45 minutes at a stirring speed of 200-400rpm to obtain a mixed wax liquid; (2) 5-10 parts of graphene oxide are mixed with 100-200 parts of deionized water, heated to 80-100° C. and stirred for 1-2 hours; then 10 parts of 30% by mass hydrogen peroxide are added, stirred for 15-45 minutes and filtered, and then the obtained filter cake is centrifuged and washed 5 times with 3% by mass hydrochloric acid, and then centrifuged and washed 5 times with deionized water, and the washed colloidal product is added to 80-100 parts of deionized water, and ultrasonically dispersed at a power of 200 W for 20 minutes to obtain graphene oxide. The invention discloses a lamellar hydrosol; 10 parts of the graphene oxide lamellar hydrosol and ethylene glycol are mixed in a volume ratio of 1:40, and after ultrasonic dispersion at 200W power for 20 minutes, 3-5 parts of stannous chloride dihydrate are added to the obtained sol, and the obtained reactant is refluxed and stirred at 100-140°C for 1 hour at a stirring speed of 60rpm, and then centrifuged to remove unreacted tin salt, and the obtained precipitate is washed with deionized water for 3-5 times to obtain a composite; 0.4-0.8 parts of the composite are mixed with 10 parts of deionized water, and ultrasonic dispersion at 200W power for 20 minutes is performed. After 15 minutes, 0.1-0.3 parts of sodium dodecylbenzene sulfonate aqueous solution are added to the graphene oxide dispersion, and stirred at a speed of 10000 rpm for 15-45 minutes to obtain a foam; the foam is placed at 80°C for a reduction reaction for 6 hours, and then naturally cooled to 25°C to obtain a mixed hydrogel, and the mixed hydrogel is soaked and washed with a 1 vol% ethanol aqueous solution for 24 hours, with a solid-liquid ratio of 1:5, to obtain a washed mixed hydrogel; the washed mixed hydrogel is taken out and placed at -45°C for freezing for 2 hours , then take it out and heat it to 25℃ to melt, and after drying at room temperature and pressure for 5h, aerogel with a thickness of 0.05-0.15cm is obtained; under the protection of nitrogen gas, the obtained aerogel is placed in a tubular furnace at 600-800℃ and heated for 1-2h, taken out and cooled to room temperature; the homemade modified solution is micro-atomized by high-pressure gas, the spray particle size is 30-50μm, the spray flow rate is 60-100ml / min, and the aerogel is spray-modified for 30-60min to prepare a modified composite aerogel as the inner layer; (3) Immerse the prepared inner layer in the mixed wax liquid, with the immersion amount being 1-5 g / m 2 , after dipping for 3-5 minutes, drying at 35°C for 30-60 minutes, and then placing in an environment with a relative humidity of 50% and a temperature of 25°C for 24 hours to obtain a multi-layer packaging bag material containing tin; the multi-layer packaging bag material containing tin is color-printed and bag-made to obtain a waterproof tin packaging bag.

5. The method for preparing a waterproof tin package according to claim 4, characterized in that: The acidic catalyst in step (1) is one of p-toluenesulfonic acid, copper sulfate and cerium sulfate.

6. The method for preparing a waterproof tin package according to claim 4, characterized in that: The oil bath heating temperature rise rate in step (1) is 10°C / min.

7. The method for preparing a waterproof tin package according to claim 4, characterized in that: In the step (1), the volume ratio of toluene to water in the mixed solvent is 4:

1.

8. The method for preparing a waterproof tin package according to claim 4, characterized in that: The centrifugal washing speed in step (2) is 5000 rpm.

9. The method for preparing a waterproof tin package according to claim 4, characterized in that: The concentration of the sodium dodecylbenzenesulfonate aqueous solution in the step (2) is 50 mg / ml.

10. The method for preparing a waterproof tin package according to claim 4, characterized in that: The homemade modified solution in step (2) is obtained by mixing 20 vol% ammonia solution and 90 vol% ethanol solution in a volume ratio of 4-8:1.

Citation Information

Patent Citations

  • Easily-degradable packaging plastic and preparation method thereof

    CN107652523A

  • Preparation method of SnO2-graphene aerogel material with gas-sensitive characteristic

    CN109775748A

  • Hydrophobic graphene aerogel and preparation method and application thereof

    CN110155993A

  • Nano silicon aerogel packaging composite film and preparation method thereof

    CN113968989A

  • Recyclable composite packaging bag

    CN114541169A