MgO-TiO2 crucible for vacuum induction melting as well as preparation and application of MgO-TiO2 crucible

By adding TiO2 as a sintering agent to the magnesium oxide crucible and using cold isostatic molding and high-temperature sintering processes, the MgO-TiO2 crucible was prepared, which solved the problem of chemical reaction and melt penetration in vacuum induction smelting of magnesium oxide crucibles, and achieved Special alloy smelting effect with high purity and long life.

CN119038960APending Publication Date: 2024-11-29INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411158177.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing magnesium oxide crucibles are prone to chemical reactions with the active elements in the alloy during vacuum induction smelting, resulting in a decrease in alloy purity and shortening the life of the crucible, which cannot effectively inhibit chemical erosion and melt penetration.

Method used

The ratio of 50 to 70 wt.% of electromelted magnesium oxide particles less than 1 mm, 10 to 40 wt.% of 1 to 3 mm, and 0 to 30 wt.% of 3 to 5 mm, was adopted, and 1 to 1 to 1 to 3 mm. 2wt.% aqueous solution and 4 to 6wt.% TiO2 are used as sintering agents to prepare MgO-TiO2 crucibles by cold isostatic molding and high-temperature sintering to ensure the chemical stability and thermal shock resistance of the crucible.

Benefits of technology

The prepared MgO-TiO2 crucible does not react chemically with the active elements in the alloy melt at high temperatures, which significantly improves the purity of the alloy, extends the service life of the crucible, and has excellent thermal shock resistance and low porosity. , suitable for batch induction smelting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038960A_ABST
    Figure CN119038960A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-chemical-stability MgO-TiO2 crucible for vacuum induction melting, and belongs to the technical field of high-temperature refractory materials. Electro-molten MgO sand and titanium dioxide are used as raw materials, after magnesite sand is uniformly mixed according to a certain particle size requirement, a crucible biscuit is formed by adopting cold isostatic pressing, and a high-chemical-stability MgO-TiO2 crucible is obtained; and carrying out sintering treatment in a high-temperature kiln at the temperature of 1680 + / -30 DEG C. The MgO-TiO2 crucible has the characteristics of high density, good thermal shock resistance and strong chemical stability, is suitable for batch-type induction melting conditions with relatively large temperature difference fluctuation, can resist melt permeation and chemical erosion, and can be used for preparing a high-temperature-resistant crucible. And the crucible and active elements (Al and Ti) in the alloy melt are not subjected to chemical reaction under high-temperature vacuum, so that the alloy melt is not polluted, and the purity of the alloy is improved. Therefore, the method is very suitable for smelting super-pure special alloy with high aluminum and titanium contents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high temperature refractory material preparation, and in particular to a MgO-TiO- ... 2 Preparation method of crucible, prepared MgO-TiO 2 Crucibles are used to melt special alloys containing active elements (Al, Ti). Background Art

[0002] Special alloys are a type of metal material used in special and extreme environments. They have good long-term organizational stability and excellent mechanical properties. Vacuum induction melting is the main method for producing special alloys. During the melting process, the active elements in the alloy will chemically corrode the oxide crucible, introduce gaseous impurity elements and inclusions into the alloy, thereby reducing the purity of the parent alloy, which is extremely harmful to the organization and mechanical properties of the special alloy. Therefore, the choice of crucible material has a great influence on the purity of the alloy.

[0003] The crucible materials used for melting special alloys include: alumina, magnesium oxide, zirconium oxide, calcium oxide, yttrium oxide, etc. Alumina crucible is the most widely used crucible material in the market, but its chemical stability is poor and it is impossible to melt high-purity special alloys; zirconium oxide and yttrium oxide crucibles have good chemical stability, but the raw materials are expensive and difficult to popularize; calcium oxide is the most suitable refractory material for producing high-purity special alloys. Due to its moisture absorption and hydration problem, it is difficult to produce and store calcium oxide crucibles. Magnesium oxide crucible is the main container for vacuum induction melting of special alloys in industry. Its raw materials are cheap, chemically stable, and non-hydrating, but its disadvantage is that it is easy to react chemically with active elements such as Al and Ti in the alloy, which increases the oxygen and magnesium content in the melt and introduces magnesium aluminum spinel inclusions. Therefore, improving the chemical stability of magnesium oxide crucibles and inhibiting the chemical reaction between active elements and crucibles are of great significance to improving the purity of special alloys. Summary of the invention

[0004] The present invention aims to overcome the shortcomings of magnesium oxide crucibles and to provide a MgO-TiO crucible for vacuum induction melting of ultra-pure special alloys with simple preparation process and low cost. 2 Preparation method of crucible, MgO-TiO prepared by the method 2 The crucible does not chemically react with the active elements in the alloy melt, does not pollute the melt and has a long service life.

[0005] To achieve the above purpose, the technical solution steps adopted by the present invention are as follows:

[0006] 1)MgO-TiO 2 The particle size distribution of the crucible, the composition and content of the sintering agent are as follows:

[0007] The particle size ratio is 50-70wt.% of fused magnesium oxide particles with a particle size of less than 1mm, 10-40wt.% of fused magnesium oxide particles with a particle size of less than 3mm and greater than 1mm, and 0-30wt.% of fused magnesium oxide particles with a particle size of less than 5mm and greater than 3mm; 1-2wt.% aqueous solution is used as a binder; 4-6wt.% TiO 2 As a sintering agent;

[0008] 2) According to the crucible particle size ratio described in step 1, magnesia sand is put into a mixer, and the aqueous solution is added. After stirring evenly, TiO 2 Sintering agent to obtain MgO-TiO 2 of mixed materials.

[0009] 3) Add the mixed materials in step 2 into the cold isostatic pressing crucible mold, and at the same time, vibrate the vibrating table up and down to fill the materials and compact them. Then, put the crucible mold into the cold isostatic press and press to obtain MgO-TiO 2 Crucible blank.

[0010] 4) MgO-TiO in step 3 2 The crucible blank is placed in a high temperature kiln for high temperature sintering to produce MgO-TiO 2 Crucible.

[0011] In the step 1), the raw material used is high-purity fused magnesia aggregate, the MgO content is >98wt.%, and other impurities are mainly CaO and SiO 2 ,CaO / SiO 2 The molar ratio is 2.

[0012] In the step 1), the sintering agent TiO 2 The purity is >98.5wt.%, and the crystal structure is anatase.

[0013] The pressure in the pressure holding stage of step 3) is 220MPa-260MPa, and the pressure holding time is 2-4min, so that high-density MgO-TiO 2 Crucible blank;

[0014] In the step 4), the sintering system is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 60°C to 90°C / h; when the temperature is between 800°C and 1200°C, the heating rate is 90 to 120°C / h; when the temperature is between 1200°C and the holding temperature, the heating rate is 120 to 150°C / h, the holding temperature is 1650°C ± 30°C, and the time is 4h to 12h;

[0015] MgO-TiO of the present invention 2The crucible has the characteristics of high density, good thermal shock resistance and strong chemical stability. It is suitable for intermittent induction melting conditions with large temperature fluctuations. At the same time, it can resist the penetration and chemical erosion of the melt. Under high temperature and vacuum, the crucible does not chemically react with the active elements (Al, Ti) in the alloy melt, does not pollute the alloy melt, and improves the purity of the alloy. Therefore, it is very suitable for melting ultra-pure special alloys with high aluminum and titanium content.

[0016] Advantages of the present invention:

[0017] 1. MgO-TiO prepared by cold isostatic pressing process adopted in the present invention 2 Compared with pure MgO crucible, MgO-TiO 2 When the crucible is used to smelt nickel-based high-temperature alloys containing Al, Ti, etc., it does not react chemically with the active elements in the melt, inhibiting the occurrence of interface reactions, preventing the chemical erosion of the melt on the crucible, and preventing the O and Mg elements decomposed in the crucible from polluting the melt and the formation of inclusions at the interface. 2 The crucible has high chemical stability and resistance to melt erosion;

[0018] 2. TiO 2 It plays a role in the liquid phase sintering of MgO, making MgO-TiO 2 The apparent porosity of the crucible is lower, and the aggregates are tightly bonded, so it has a stronger resistance to melt penetration;

[0019] 3. MgO-TiO 2 The crucible has excellent thermal shock resistance and long service life, and can meet the working conditions of intermittent production of high-temperature alloys. 2 Reaction with MgO powder to produce Mg 2 TiO 4 Binding phase, due to Mg 2 TiO 4 Due to the different thermal expansion coefficients between the crucible and the magnesium oxide matrix, the volume shrinkage is not synchronized during the sintering process, which causes microcracks inside the crucible, thereby buffering thermal stress and preventing crack propagation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 MgO-TiO after vacuum induction melting of K417G alloy 2 Microstructure of the inner wall of the crucible (Example 1)

[0021] Figure 2 MgO-TiO after vacuum induction melting of K417G alloy 2 Crucible (Example 1)

[0022] Figure 3Microstructure of the inner wall of MgO crucible after vacuum induction melting of K417G alloy (Comparative Example 1)

[0023] Figure 4 MgO crucible morphology after vacuum induction melting of K417G alloy (Comparative Example 1)

[0024] Figure 5 MgO-TiO after vacuum induction melting of K417G alloy 2 Crucible (1wt.%TiO 2 ) Inner wall microstructure (Comparative Example 2)

[0025] Figure 6 MgO-TiO after vacuum induction melting of K417G alloy 2 Crucible (1wt.%TiO 2 ) Morphology (Comparative Example 2)

[0026] Figure 7 MgO-TiO after vacuum induction melting of K417G alloy 2 Crucible (3wt.%TiO 2 ) Inner wall microstructure (Comparative Example 3)

[0027] Figure 8 Vacuum induction melted K417G alloy containing 3wt.%TiO 2 MgO-TiO 2 Crucible (3wt.%TiO 2 ) Morphology (Comparative Example 3) DETAILED DESCRIPTION

[0028] 1)MgO-TiO 2 The particle size distribution of the crucible, the composition and content of the sintering agent are as follows:

[0029] The particle composition of the fused magnesium oxide (or magnesia) is as follows: 50-70wt.% of fused magnesium oxide particles with a particle size of less than 1mm, 10-40wt.% of fused magnesium oxide particles with a particle size of less than 3mm and greater than or equal to 1mm, and 0-30wt.% of fused magnesium oxide particles with a particle size of less than or equal to 5mm and greater than or equal to 3mm.

[0030] 1-2 wt.% aqueous solution as a binder; 4-6 wt.% TiO 2 As sintering agent; the rest is fused magnesium oxide (or magnesia);

[0031] 2) The MgO-TiO 2 Put the magnesia sand with the crucible size ratio into the mixer (or mixer), add the aqueous solution, stir evenly, and then add TiO 2 Sintering agent to obtain MgO-TiO2 Mixed materials;

[0032] 3) Add the mixed materials into the cold isostatic pressing crucible mold, and at the same time, vibrate the vibrating table where the mold is located up and down to fill the mold with materials and vibrate them. Then, put the crucible mold into the cold isostatic press, control the molding pressure at 220-260MPa, hold the pressure for 2-4min, and obtain MgO-TiO after automatic pressure release. 2 Crucible blank;

[0033] 4) MgO-TiO 2 The crucible blank is placed in a high-temperature kiln for high-temperature sintering. The sintering system is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 60°C to 90°C / h; when the temperature is between 800°C and 1200°C, the heating rate is greater than 90 to 120°C / h; when the temperature is greater than 1200°C to the holding temperature, the heating rate is greater than 120 to 150°C / h, the holding temperature is 1650°C ± 30°C, and the time is 4h to 12h;

[0034] Embodiment 1:

[0035] A vacuum induction melting high activity special alloy MgO-TiO 2 The preparation method of the crucible uses a crucible with a capacity of 2 kg in the embodiment, but the preparation method is not limited to preparing a crucible with this capacity. The preparation method of this specific embodiment is as follows:

[0036] 1)MgO-TiO 2 The particle size distribution of the crucible, the composition and content of the sintering agent are as follows:

[0037] The particle composition of the fused magnesium oxide (or magnesia) is such that 50wt.% of the fused magnesium oxide particles have a particle size of less than 1mm, 20wt.% of the fused magnesium oxide particles have a particle size of less than 3mm and greater than or equal to 1mm, and 30wt.% of the fused magnesium oxide particles have a particle size of less than or equal to 5mm and greater than or equal to 3mm.

[0038] A 1.0 wt.% aqueous solution was used as a binder; a 4 wt.% anatase TiO 2 As sintering agent; the rest is fused magnesium oxide (or magnesia);

[0039] 2) The MgO-TiO 2 Put the magnesia with the crucible size ratio into the mixer, add the aqueous solution, stir evenly, and then add TiO 2 Sintering agent to obtain MgO-TiO 2 Mixed materials;

[0040] 3) Add the mixed materials into the cold isostatic pressing crucible mold, and at the same time, vibrate the vibrating table where the mold is located up and down to fill the mold with materials and vibrate them. Then, put the crucible mold into the cold isostatic press, control the molding pressure at 220MPa, hold the pressure for 2min, and obtain MgO-TiO after automatic pressure release. 2 Crucible blank;

[0041] 4) MgO-TiO 2 The crucible blank is placed in a high-temperature kiln for high-temperature sintering. The sintering system is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 60°C / h; when the temperature is between 800°C and 1200°C, the heating rate is 90°C / h; when the temperature is between 1200°C and 1650°C, the heating rate is 120°C / h, the holding temperature is 1650°C, and the holding time is 4h; after cooling naturally to room temperature with the furnace, the sintered MgO-TiO 2 Crucible.

[0042] 5) MgO-TiO prepared in this example 2 The crucible was measured to have an apparent porosity of 9.7% and a bulk density of 3.20 g / cm 3 (Standard GB / T 2997-2015); High temperature flexural strength is 8MPa (Standard GB / T-3002-2004); Strength retention rate after compressed air quenching reaches 70% (Standard YB / T4018-1991).

[0043] 6) Using the MgO-TiO prepared in this example 2 The nickel-based high-temperature alloy (K417G alloy) was melted by vacuum induction melting in a crucible. The original composition is shown in Table 1.

[0044] Table 1 K417G alloy original composition

[0045]

[0046] The crucible can hold 2 kg of material. Under the condition of vacuum degree <0.1 Pa, induction heating is performed to 1600°C. After the melt is cleared, it is kept warm for 50 minutes. Then the melt is poured into the iron mold, and the chemical composition of the smelted K417G alloy is analyzed (Table 2). The smelted alloy is not contaminated by the crucible, and the O and Mg contents are not increased.

[0047] Table 2 Composition of K417G alloy after melting

[0048]

[0049] 7) After smelting, MgO-TiO 2 The crucible interface was scanned and observed, and the image showed that there was no interface reaction layer and permeation layer on the inner wall of the crucible ( Figure 1 ), MgO-TiO 2 The crucible is dense and chemically stable, with strong resistance to melt penetration and chemical erosion; the macroscopic morphology shows that the outer wall surface of the crucible is intact, without cracks, showing excellent thermal shock resistance. Figure 2 ).

[0050] Embodiment 2:

[0051] A vacuum induction melting high activity special alloy MgO-TiO 2 The preparation method of the crucible, the preparation method of this specific embodiment is as follows:

[0052] 1)MgO-TiO 2 The particle size distribution of the crucible, the composition and content of the sintering agent are as follows:

[0053] The particle composition of the fused magnesium oxide (or magnesia) is such that 60wt.% of the fused magnesium oxide particles have a particle size of less than 1mm, 20wt.% of the fused magnesium oxide particles have a particle size of less than 3mm and greater than or equal to 1mm, and 20wt.% of the fused magnesium oxide particles have a particle size of less than or equal to 5mm and greater than or equal to 3mm.

[0054] A 1.5 wt.% aqueous solution was used as a binder; a 5 wt.% anatase TiO 2 As sintering agent; the rest is fused magnesium oxide (or magnesia);

[0055] 2) The MgO-TiO 2 Put the magnesia with the crucible size ratio into the mixer, add the aqueous solution, stir evenly, and then add TiO 2 Sintering agent to obtain MgO-TiO 2 Mixed materials;

[0056] 3) Add the mixed materials into the cold isostatic pressing crucible mold, and at the same time, vibrate the vibrating table where the mold is located up and down to fill the mold with materials and vibrate them. Then, put the crucible mold into the cold isostatic press, control the molding pressure at 240MPa, hold the pressure for 2min, and obtain MgO-TiO after automatic pressure release. 2 Crucible blank;

[0057] 4) MgO-TiO 2 The crucible blank is placed in a high-temperature kiln for high-temperature sintering. The sintering system is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 80°C / h; when the temperature is between 800°C and 1200°C, the heating rate is 110°C / h; when the temperature is between 1200°C and the holding temperature, the heating rate is 130°C / h, the holding temperature is 1700°C, and the time is 4h; after cooling naturally to room temperature with the furnace, take out the sintered MgO-TiO2 Crucible.

[0058] 5) MgO-TiO prepared in this example 2 The crucible was tested: the apparent porosity was 9.5% and the volume density was 3.21 g / cm 3 (Standard GB / T 2997-2015); High temperature flexural strength is 8.4MPa (Standard GB / T-3002-2004); Strength retention rate after compressed air quenching reaches 75% (Standard YB / T4018-1991).

[0059] 6) Using the MgO-TiO prepared in this example 2 The crucible vacuum induction melting of nickel-based high-temperature alloy (K417G alloy), the original composition of the alloy is shown in Table 1. The crucible capacity can hold 2Kg of material. Under the condition of vacuum degree <0.1Pa, induction heating to 1600℃, after the melt is cleared, keep warm for 50min. Then the melt is poured into the iron mold, and the chemical composition analysis is carried out (Table 3). The alloy after melting is extremely low in Mg and O contamination of the crucible.

[0060] Table 3 Composition of K417G alloy after melting

[0061]

[0062] Embodiment 3:

[0063] A vacuum induction melting high activity special alloy MgO-TiO 2 The preparation method of the crucible, the preparation method of this specific embodiment is as follows:

[0064] 1)MgO-TiO 2 The particle size distribution of the crucible, the composition and content of the sintering agent are as follows:

[0065] The particle composition of the fused magnesium oxide (or magnesia) is such that 70wt.% of the fused magnesium oxide particles have a particle size of less than 1mm, 30wt.% of the fused magnesium oxide particles have a particle size of less than 3mm and greater than or equal to 1mm, and 0wt.% of the fused magnesium oxide particles have a particle size of less than or equal to 5mm and greater than or equal to 3mm.

[0066] A 2wt.% aqueous solution was used as a binder; a 6wt.% anatase TiO 2 As sintering agent; the rest is fused magnesium oxide (or magnesia);

[0067] 2) The MgO-TiO 2 Put the magnesia with the crucible size ratio into the mixer, add the aqueous solution, stir evenly, and then add TiO 2 Sintering agent to obtain MgO-TiO 2Mixed materials;

[0068] 3) Add the mixed materials into the cold isostatic pressing crucible mold, and at the same time, vibrate the vibration table where the mold is located up and down to fill the mold with materials and vibrate them. Then, put the crucible mold into the cold isostatic press, control the molding pressure at 260MPa, hold the pressure for 2min, and obtain MgO-TiO after automatic pressure release. 2 Crucible blank;

[0069] 4) MgO-TiO 2 The crucible blank is placed in a high-temperature kiln for high-temperature sintering. The sintering system is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 90°C / h; when the temperature is between 800°C and 1200°C, the heating rate is 120°C / h; when the temperature is between 1200°C and the holding temperature, the heating rate is 150°C / h, the holding temperature is 1700°C, and the time is 12h; after cooling naturally to room temperature with the furnace, take out the sintered MgO-TiO 2 Crucible.

[0070] 5) MgO-TiO prepared in this example 2 The crucible was tested: the apparent porosity was 9.3% and the volume density was 3.21 g / cm 3 , (standard GB / T 2997-2015), the high temperature flexural strength at 1400℃ is 7MPa (standard GB / T-3002-2004); the strength retention rate after compressed air quenching reaches 68% (standard YB / T4018-1991).

[0071] 6) Using the MgO-TiO prepared in this example 2 The crucible vacuum induction melting of nickel-based high-temperature alloy (K417G alloy), the original composition of the alloy is shown in Table 1. The crucible capacity can hold 2Kg of material. Under the condition of vacuum degree <0.1Pa, induction heating to 1600℃, after the melt is cleared, keep warm for 50min. Then pour the melt into the iron mold for chemical composition analysis.

[0072] Table 4 Composition of K417G alloy after melting

[0073]

[0074] Compared with the prior art, this specific implementation case has the following positive effects:

[0075] This specific implementation method uses high-purity fused magnesia and anatase TiO 2 MgO-TiO prepared by mixing, cold isostatic pressing and high temperature sintering 2 The crucible overcomes the shortcomings of pure MgO crucible, such as low chemical stability and poor resistance to melt erosion.2 There is no chemical reaction between the crucible and the active elements in the melt, and there is no permeation layer and chemical reaction layer on the interface ( Figure 1 ), the crucible does not contaminate the melt, thus improving the purity of the alloy. 2 By dissolving in MgO crystals at high temperature, the chemical stability of MgO is improved, and the Mg and O elements generated by the substitution reaction between the MgO crucible and the active elements in the alloy are prevented from entering the melt. At the same time, the problem of the interface products generated on the inner wall of the crucible contaminating the melt is also avoided. Another positive effect of inhibiting the interface reaction of the crucible melt is that as the number of times the crucible is melted increases, the inner wall of the crucible still maintains the MgO-TiO 2 The nature of the crucible, the inner wall will not degenerate into its own oxide, preventing the problem of the chemical stability of the crucible decreasing with the increase of smelting times. In contrast, the inner wall of the MgO crucible is uneven, and there are permeation layers and chemical reaction layers ( Figure 3 ), the reaction layer is eroded and penetrated by the melt, causing the MgO crucible to gradually peel off and decompose into the melt, contaminating the melt. In short, TiO 2 The addition of improves the chemical stability of MgO crucible, MgO-TiO 2 The crucible has stronger resistance to melt erosion than the MgO crucible and the purity of the smelted alloy is higher, with the contents of O and Mg being less than 0.0005wt.%.

[0076] MgO-TiO 2 The crucible has both dense structure and excellent thermal shock resistance. 2 The binary system has the characteristic of the lowest eutectic point of 1630℃. The liquid phase is generated at a high temperature of 1650℃ to 1700℃, which promotes the sintering of the crucible aggregate and the matrix, increases the connection strength between the particles, and improves the crucible's ability to resist melt penetration. 2 In situ reaction generates Mg 2 TiO 4 Second phase, Mg 2 TiO 4 The thermal expansion coefficient of the crucible is different from that of the MgO matrix. During the cooling process after sintering, micro cracks are generated inside the crucible, which increases the MgO-TiO 2 Thermal shock resistance of crucible. By observing the MgO-TiO 2 The outer wall of the crucible has no cracks and is intact as a whole ( Figure 2 ). It can be seen that MgO-TiO 2 The crucible has excellent thermal shock resistance and can be used for intermittent vacuum induction melting with large temperature differences and more stringent melting conditions.

[0077] MgO-TiO 2The preparation process of the crucible is simple, the raw materials used to prepare the crucible are abundant in resources and low in price, and it is easier to popularize and apply in industry.

[0078] Comparative Example 1: The difference from Example 2 is that no TiO 2 As a sintering agent, a pure MgO crucible was prepared, and the other processes and conditions were the same as those in Example 2. Figure 3 This is a photo of the inner wall of the crucible after smelting. A melt erosion layer is formed on the inner wall. After smelting, the Mg content in the alloy increases from 2ppm to 15ppm, and the O content increases from <3ppm to 6ppm.

[0079] Comparative Example 2 is different from Example 2 in that 1 wt.% TiO 2 As a sintering agent, MgO-TiO 2 Crucible, other processes and conditions are the same as in Example 2. Add 1TiO 2 After that, the inner wall of the MgO crucible still has an erosion layer ( Figure 5 ), and the thermal shock resistance is poor, and multiple cracks appear on the outer wall of the crucible after melting ( Figure 6 ), the Mg content in the alloy after smelting is still relatively high.

[0080] Comparative Example 3 is different from Example 2 in that 3 wt.% TiO 2 As a sintering agent, MgO-TiO 2 Crucible, other processes and conditions are the same as in Example 2. Add 3wt.% TiO 2 After that, the inner wall of the crucible becomes dense, the chemical corrosion layer disappears, and the Mg content in the alloy is 5ppm. It can be seen that the addition of 3wt.% TiO 2 The chemical stability and corrosion resistance of the MgO crucible have been significantly improved, but its thermal shock resistance is still poor, and multiple cracks appear on the outer wall of the crucible.

[0081] Table 5 Impurity content (wt.%) of K417G alloy after melting in different crucible materials

[0082] Implementation Cases Apparent porosity Bulk density Thermal shock resistance High temperature strength Comparative Example 1 13.6% <![CDATA[3.14g / cm 3 ]]> 54% 11MPa Comparative Example 2 11.4% <![CDATA[3.16g / cm 3 ]]> 41% 1.5MPa Comparative Example 3 10.1% <![CDATA[3.21g / cm 3 ]]> 43% 6MPa

[0083] Table 6 Impurity content (wt.%) of K417G alloy after melting in different crucible materials

[0084] Implementation Cases O N H Mg Comparative Example 1 0.0006 <0.0003 <0.0001 0.0015 Comparative Example 2 0.0005 <0.0003 <0.0001 0.0009 Comparative Example 3 0.0004 <0.0003 <0.0001 0.0005

Claims

1. The preparation method of MgO-TiO2 crucible for vacuum induction melting is as follows: Step 1: Raw material preparation: Use fused magnesia as the main material, and sintering agent titanium dioxide and binder as crucible preparation raw materials; Step 2: after the fused magnesia raw material, sintering agent and binder in step 1 are uniformly mixed, a crucible blank is pressed by cold isostatic pressing technology; Step 3: Place the crucible blank obtained in step 2 into a gas furnace for heating and sintering. After sintering, the crucible is naturally cooled along with the furnace to obtain a MgO-TiO2 crucible with high chemical stability for vacuum induction melting.

2. The preparation method according to claim 1, characterized in that : In step (1), the main raw material used is high-purity fused magnesium oxide aggregate, and the MgO mass content is >98%.

3. The preparation method according to claim 1, characterized in that : In step (1), the sintering agent is titanium dioxide having anatase crystal form; The particle size is 75 μm or less, preferably 45 μm or less, and more preferably 40 μm or less.

4. The preparation method according to claim 1, characterized in that : In step (1), the binder used is an aqueous solution; the proportion of the binder in the raw material is 1-2wt.%, preferably 1-1.5wt.%, and more preferably 1.2-1.5wt.%.

5. The preparation method according to claim 1 or 2, characterized in that: In the steps (1) and (2), the fused MgO sand used is prepared according to the following mass percentage ratio: 0 to less than 1mm 50%-70%; 1 to less than 3mm 10%-40%; 3- to less than 5mm 0% - 30%; The preferred ratio is: 0 to less than 1 mm 55-60%; 1 to less than 3 mm 40-45%; 3- to less than 5mm 0%.

6. The preparation method according to claim 1 or 3, characterized in that In step (1), the proportion of sintering agent TiO2 in the raw material is 4-6wt.%, preferably 4.5-5.0%, and more preferably 4.7-4.8%.

7. The preparation method according to claim 1, characterized in that In step (2), the cold isostatic pressing pressure is 220 MPa to 260 MPa, preferably 220 to 240 MPa, more preferably 240 MPa; the time is 2 to 4 minutes, preferably 2 to 3 minutes.

8. The preparation method according to claim 1, characterized in that : In step (3), the heating and sintering process is as follows: heating stage rate: when the temperature is less than 800°C, the heating rate is 60°C-90°C / h (preferably 80-90°C / h), when the temperature is between 800°C and 1200°C, the heating rate is greater than 90-120°C / h (preferably 100-110°C / h), when the temperature is greater than 1200°C-holding temperature, the heating rate is greater than 120-150°C / h (preferably 130-140°C / h), the holding temperature is 1680°C±30°C (preferably 1650-1700°C, more preferably 1680-1700°C), and the time is 4h-12h (preferably 8h-10h).

9. A MgO-TiO2 crucible prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the MgO-TiO2 crucible according to claim 9 in smelting special alloys containing active elements (such as one or both of Al and Ti).

Citation Information

Patent Citations

  • Preparation method of magnesia crucible with high intensity, density and purity

    CN103030407A

  • Magnesium oxide whisker in-situ synthesized spinel reinforced magnesium oxide-based crucible and preparation method of crucible

    CN108424124A

  • Preparation method of formed crucible with desulfurization and rare earth element addition functions

    CN116003108A

  • Method for manufacturing high-capacity MgO crucible by adopting cold isostatic pressing technology

    CN118290125A

  • Method for manufacturing erosion-resistant magnesium crucible by adopting cold isostatic pressing technology

    CN118290126A