Ceramic slurry as well as preparation method and application thereof
By using composite plasticizers and ball milling processes in ceramic slurries, the problems of mechanical properties and degreasing safety of ceramic green bodies are solved, and the high mechanical properties and safe degreasing of ceramic green bodies are achieved.
Patent Information
- Application Number
- CN202411169190.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ceramic casting and forming technology is difficult to meet the problems of strong mechanical properties and safety of degreasing of ceramic green bodies at the same time. The high decomposition temperature of traditional plasticizers or the low mechanical strength leads to defect generation and poor performance.
The composite plasticizer is used to mix high molecular weight plasticizers such as water G-260, propylene glycol polyester, trithylene phosphate, and low molecular weight plasticizers such as dibutyl phthalate to prepare ceramic slurry by ball milling, and During the degreasing process, the channel structure is used to preferentially remove low molecular weight plasticizers, and promote the decomposition of high molecular weight plasticizers and binders.
It significantly reduces the defects of ceramic green body, improves the mechanical properties of cast-formed ceramics, and ensures safe degreasing and high mechanical properties.
Smart Images

Figure CN119038962A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic tape casting, and in particular to a ceramic slurry and a preparation method and application thereof. Background Art
[0002] Ceramic materials not only have advantages such as excellent mechanical properties, outstanding chemical stability, and strong high-temperature stability, but also have different electrical, thermal, optical and other functions. With the rapid development of modern industry, new performance and processing requirements are put forward for the performance of ceramic materials. Traditional dry pressing to prepare ceramics has disadvantages such as uneven green bodies, limited shapes, low processing efficiency, and high mold consumption, which limits the large-scale use of ceramic materials in modern industrial scenarios. Tape casting, also known as tape casting, is a relatively mature forming method that can obtain high-quality, ultra-thin ceramic sheets. It has been widely used in the production of advanced ceramics such as monolithic capacitor ceramic sheets, thick film and thin film circuit substrates. The rapid development of tape casting has greatly promoted the rapid development of ceramic materials in modern industry, especially in the fields of electrical and electronics, information and communications, and integrated circuits.
[0003] The key to ceramic tape casting is to prepare a ceramic slurry with excellent performance, and to prepare a ceramic green body with sufficiently high mechanical properties through tape casting. The green body has no obvious defects after degreasing, and a ceramic thin plate with high density and excellent mechanical properties is obtained through high-temperature sintering. The formula composition of the ceramic slurry has a significant effect on the green body performance, degreasing performance and sintering performance of tape-cast ceramics. Among them, the plasticizer has a great influence on the mechanical properties of the green body and the degreasing behavior of the ceramic green body. After tape casting, the solvent evaporates, and the ceramic green body is composed of ceramic powder, binder and plasticizer. Among them, the plasticizer is a polymer material additive, which can usually increase the plasticity and toughness of the ceramic green body and improve the processing performance of ceramic tape casting. At present, the plasticizers commonly used in the process of ceramic tape casting include phthalates, such as dioctyl phthalate, di-n-octyl phthalate, butyl benzyl phthalate, dibutyl phthalate, etc., and also include aliphatic plasticizers, such as polyethylene glycol 400, polyethylene glycol 600, polyethylene glycol 1500, etc. However, the components of the traditional tape casting ceramic slurry usually only include a single plasticizer. Although it can ensure the excellent mechanical properties of the ceramic green body, this type of plasticizer usually has a high decomposition temperature, which makes it difficult to degrease the ceramic green body and a large number of defects; in addition, although some plasticizers can ensure that the plasticizer is smoothly discharged during the low-temperature degreasing process, and then decompose the binder in the high-temperature degreasing stage, which can produce heterogeneous defects, this type of plasticizer usually has low mechanical strength, resulting in poor mechanical properties of the tape casting ceramic green body. Therefore, it is impossible to simultaneously meet the needs of high-performance green body and safe degreasing of ceramic tape casting.
[0004] For example, the composition of the slurry in the Chinese invention patent "Beryllium Oxide Ceramic Tape Casting Slurry and Its Production Method" (CN108623288B) is: by weight percentage, 50% to 70% of powder, 30% to 50% of organic solvent, the powder is a mixture of beryllium oxide powder, silicon dioxide powder and magnesium oxide powder, and the organic solvent is a mixture of phthalate, toluene, butanone, isopropanol, phosphate anionic emulsifier and polyvinyl butyral. Among them, the plasticizer is only phthalate, and the decomposition temperature of phthalate is 295°C, but phthalate is a small molecular weight plasticizer containing a benzene ring structure, and the molecular weight is low, so it is difficult to ensure the mechanical properties of the formed ceramic green body.
[0005] For example, in the Chinese invention patent "A method for preparing high thermal conductivity silicon nitride ceramic substrate by tape casting of silicon powder" (CN115028461A), the plasticizer is a mixture of butyl benzyl phthalate and ethylene glycol; the amount of the plasticizer added is 0.5-15wt% of the total mass of the mixed powder; preferably, the mass percentage of butyl benzyl phthalate and ethylene glycol in the plasticizer is (40%-80%): (20%-60%), and the sum of the mass percentage is 100%. Even if butyl benzyl phthalate and ethylene glycol are used, both plasticizers are small molecular weight plasticizers with short molecular chains, resulting in poor mechanical properties of tape-cast ceramic green bodies. Summary of the invention
[0006] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, provide a ceramic slurry and its preparation method and application, and solve the technical problem in the prior art of how to satisfy the ceramic slurry tape casting to obtain a ceramic green body with strong mechanical properties and safe degreasing.
[0007] In order to achieve the above technical objectives, the technical solution of the present invention provides a method for preparing a ceramic slurry, comprising the following steps:
[0008] mixing the first plasticizer and the second plasticizer into a composite plasticizer;
[0009] Dissolving the composite plasticizer, binder and dispersant in a solvent to prepare a premixed liquid;
[0010] Adding the ceramic powder to the premixed liquid and ball-milling to obtain a ceramic slurry;
[0011] The first plasticizer is one or more of Sekisui G-260, propylene glycol adipate polyester, tricresyl phosphate, polyethylene glycol PEG400, polyethylene glycol PEG600 and polypropylene glycol PPG400;
[0012] The second plasticizer is one or more of dibutyl phthalate DBP, polyethylene glycol PEG200, polypropylene glycol PPG200 and diethylene glycol DEG.
[0013] In any embodiment, the mass ratio of the first plasticizer to the second plasticizer is (2-3):(2-3).
[0014] In any embodiment, the binder is one or both of polyvinyl butyral PVB and polyvinyl alcohol PVA; and / or the dispersant is a polymer dispersant, and the polymer dispersant is one or more of BYK111, BYK163 and Sago9900; the amount of the dispersant is 2%-5% of the mass of the ceramic powder.
[0015] In any embodiment, the solvent is a mixture of ethanol and butanone, and the mass ratio of the ethanol to the butanone is 1:(1-1.5); and / or the mass ratio of the composite plasticizer, the binder and the solvent is (2-3):(3-4):4; and / or the added amount of the ceramic powder is 60%-85% of the mass of the ceramic slurry.
[0016] In any embodiment, the mesh size of the ceramic powder is 300-400 mesh.
[0017] In any embodiment, the ceramic powder is obtained by the following steps: wet grinding the ceramic powder with alcohol, the ball milling time is 4-8h, the ball milling speed is 200-400rpm, and after wet grinding, it is dried in an oven, the drying temperature is 120-150°C, and the drying time is 6-10h.
[0018] In any embodiment, the rotation speed of the ball mill is 400-600 rpm, and the time of the ball mill is 10-24 h.
[0019] In addition, the present invention also provides a ceramic slurry prepared by the above preparation method.
[0020] In addition, the present invention also proposes a ceramic slurry prepared by the above preparation method or the use of the above ceramic slurry in preparing ceramic green bodies by tape casting.
[0021] The above applications include:
[0022] The ceramic slurry is introduced into the slurry tank of the tape casting machine. After the ceramic slurry flows out of the slurry tank, it drips into the tape casting belt. Then, the solvent evaporates after entering the drying tunnel, and the tape cast ceramic monolayer is formed. The tape cast ceramic monolayer is stacked using a warm isostatic press to prepare a ceramic green body.
[0023] Tape casting parameters: drying oven temperature is 60-100°C, belt speed is 1-5mm / s, scraper blade thickness is 5-10mm, warm isostatic pressing temperature is 100-150°C, and pressure is 1-5MPa.
[0024] Compared with the prior art, the beneficial effects of the present invention include: in the preparation method of the ceramic slurry proposed by the present invention, the first plasticizer and the second plasticizer are mixed into a composite plasticizer; the composite plasticizer, the binder and the dispersant are dissolved in a solvent to prepare a premixed liquid; the ceramic powder is added to the premixed liquid and ball-milled to obtain a ceramic slurry; the first plasticizer is one or more of Sekisui G-260, propylene glycol adipate polyester, tricresyl phosphate, polyethylene glycol PEG400, polyethylene glycol PEG600 and polypropylene glycol PPG400; the second plasticizer is one or more of The plasticizer is one or more of dibutyl phthalate DBP, polyethylene glycol PEG200, polypropylene glycol PPG200 and diethylene glycol DEG; the decomposition temperature is different during the degreasing process, and the low molecular weight second plasticizer can be removed first to form a pore structure in the ceramic green body, which is convenient for the decomposition products of the high molecular weight first plasticizer and the binder to be removed in the pore structure, greatly reducing the generation of defects and greatly improving the mechanical properties of the tape-cast ceramic green body, thereby meeting the requirements of ceramic slurry tape-casting to obtain a ceramic green body with strong mechanical properties and safe degreasing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 TG / DSC images of ceramic green bodies prepared by the ceramic slurries of Example 1 and Comparative Example 1 according to the method of Application Example 1; wherein, Figure 1 (a) is the TG / DSC image of the ceramic green body made from the ceramic slurry corresponding to Example 1; Figure 1 (b) is the TG / DSC image of the ceramic green body made from the ceramic slurry corresponding to Comparative Example 1.
[0026] Figure 2 This is a graph showing the mechanical properties test results of ceramic green bodies made from the ceramic slurries of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention according to the method of Application Example 1.
[0027] Figure 3 This is a graph showing the test results of mechanical and thermal properties of ceramic green bodies made from the ceramic slurries of Examples 1-4, Comparative Examples 1 and 2 of the present invention according to the method of Application Example 1. DETAILED DESCRIPTION
[0028] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0029] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0030] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0031] This specific embodiment provides a method for preparing a ceramic slurry, comprising the following steps:
[0032] mixing the first plasticizer and the second plasticizer into a composite plasticizer;
[0033] The composite plasticizer, the binder and the dispersant are dissolved in a solvent to prepare a premixed liquid; the binder is one or two of polyvinyl butyral ester PVB and polyvinyl alcohol PVA; the dispersant is a high molecular polymer dispersant, and the high molecular polymer dispersant is one or more of BYK111, BYK163 and Sago9900, and the amount of the dispersant is 2%-5% of the mass of the ceramic powder; the solvent is a mixture of ethanol and butanone, and the mass ratio of the ethanol to the butanone is 1:(1-1.5); the mass ratio of the composite plasticizer, the binder and the solvent is (2-3):(3-4):4;
[0034] The ceramic powder is added to the premixed liquid and ball-milled to obtain a ceramic slurry; the amount of the ceramic powder added is 60%-85% of the mass of the ceramic slurry; the rotation speed of the ball mill is 400-600 rpm, and the ball milling time is 10-24 hours;
[0035] The first plasticizer is one or more of Sekisui G-260, propylene glycol adipate polyester, tricresyl phosphate, polyethylene glycol PEG400, polyethylene glycol PEG600 and polypropylene glycol PPG400;
[0036] The second plasticizer is one or more of dibutyl phthalate DBP, polyethylene glycol PEG200, polypropylene glycol PPG200 and diethylene glycol DEG;
[0037] The mass ratio of the first plasticizer to the second plasticizer is (2-3):(2-3);
[0038] The mesh number of the ceramic powder is 300-400 meshes, and the ceramic powder is obtained by the following steps: wet grinding the ceramic powder with alcohol, the ball milling time is 4-8h, the ball milling speed is 200-400rpm, and after wet grinding, drying in an oven, the drying temperature is 120-150℃, and the drying time is 6-10h.
[0039] This specific embodiment also provides a ceramic slurry prepared by the above preparation method.
[0040] This specific embodiment also proposes a ceramic slurry prepared by the above preparation method or an application of the above ceramic slurry in preparing a ceramic green body by tape casting, including:
[0041] The ceramic slurry is introduced into the slurry tank of the tape casting machine. After the ceramic slurry flows out of the slurry tank, it drips into the tape casting belt. Then, the solvent evaporates after entering the drying tunnel, and the tape cast ceramic monolayer is formed. The tape cast ceramic monolayer is stacked using a warm isostatic press to prepare a ceramic green body.
[0042] Tape casting parameters: drying oven temperature is 60-100°C, belt speed is 1-5mm / s, scraper blade thickness is 5-10mm, warm isostatic pressing temperature is 100-150°C, and pressure is 1-5MPa.
[0043] The ceramic powder in this specific embodiment includes one or more of alumina ceramic powder, non-oxide ceramic powder and functional ceramic powder. The alumina ceramic powder includes one or more of aluminum oxide, zirconium oxide and silicon oxide. The non-oxide ceramic powder includes one or more of aluminum nitride, silicon nitride, silicon carbide and boron nitride. The functional ceramic powder includes one or both of barium titanate and lithium carbonate.
[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0045] In the present invention, reference is made to “some embodiments”, “this embodiment”, examples, etc., which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.
[0046] If similar descriptions of "first / second" appear in the application documents, the following instructions are added. In the following description, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein.
[0047] In this embodiment, the term "and / or" is merely a description of the association relationship between associated objects, indicating that three relationships may exist. For example, object A and / or object B may represent three situations: object A exists alone, object A and object B exist at the same time, and object B exists alone.
[0048] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0049] Example 1
[0050] This embodiment provides a ceramic slurry, which is prepared by the following steps:
[0051] S1, the aluminum oxide was ball-milled at 200 rpm for 8 h with alcohol, and then dried and sieved at a drying temperature of 120° C. for 10 h to obtain aluminum oxide with a mesh size of 300-400 mesh;
[0052] S2, mixing Sekisui G-260 and dibutyl phthalate DBP into a composite plasticizer;
[0053] S3, dissolving the composite plasticizer, the binder polyvinyl butyral ester PVB and the dispersant polymer dispersant BYK111 in a solvent to prepare a premixed liquid; the solvent is a mixture of ethanol and butanone in a mass ratio of 1:1; the mass ratio of the composite plasticizer, the binder and the solvent is 3:3:4; the amount of BYK111 is 3% of the mass of the aluminum oxide;
[0054] S4. Add the ceramic powder alumina treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 70% of the mass of the ceramic slurry; the rotation speed of the ball mill is 500 rpm, and the ball milling time is 16 hours.
[0055] Example 2
[0056] This embodiment provides a ceramic slurry, which is prepared by the following steps:
[0057] S1, ball milling zirconium oxide with alcohol at 200 rpm for 8 hours, then drying and sieving, the drying temperature is 150 ° C, the drying time is 6 hours, and the mesh size of zirconium oxide is 300-400 mesh;
[0058] S2, mixing the plasticizer polypropylene glycol PPG600 and dibutyl phthalate DBP into a composite plasticizer;
[0059] S3, dissolving the composite plasticizer, the binder polyvinyl butyral ester PVB and the dispersant polymer dispersant BYK111 in a solvent to prepare a premixed liquid; the solvent is a mixture of ethanol and butanone in a mass ratio of 1:1; the mass ratio of the composite plasticizer, the binder and the solvent is 1:2:2; the amount of BYK111 is 2% of the mass of zirconium oxide;
[0060] S4. Add the ceramic powder zirconium oxide treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 80% of the mass of the ceramic slurry; the rotation speed of the ball mill is 400 rpm, and the ball milling time is 12 hours.
[0061] Example 3
[0062] This embodiment provides a ceramic slurry, which is prepared by the following steps:
[0063] S1. Aluminum nitride was ball-milled with alcohol at 200 rpm for 5 h, then dried and sieved at a drying temperature of 130° C. for 8 h to obtain aluminum oxide with a mesh size of 300-400 mesh;
[0064] S2, mixing high molecular weight plasticizer polyethylene glycol PEG600 and dibutyl phthalate DBP into a composite plasticizer;
[0065] S3, dissolving the composite plasticizer, the binder polyvinyl alcohol PVA and the dispersant polymer dispersant BYK111 in a solvent to prepare a premixed solution; the solvent is a mixture of ethanol and butanone in a mass ratio of 1:1; the mass ratio of the composite plasticizer, the binder and the solvent is 1:2:2; the amount of BYK111 is 2% of the mass of the aluminum oxide;
[0066] S4. Add the aluminum nitride ceramic powder treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 80% of the mass of the ceramic slurry; the rotation speed of the ball mill is 400 rpm, and the ball milling time is 12 hours.
[0067] Example 4
[0068] This embodiment provides a ceramic slurry, which is prepared by the following steps:
[0069] S1, ball milling silicon nitride with alcohol at 300 rpm for 6 hours, then drying and sieving, the drying temperature is 130 ° C, the drying time is 8 hours, and the mesh size of 300-400 mesh alumina is obtained;
[0070] S2, mixing high molecular weight plasticizer polypropylene glycol PPG400 and polyethylene glycol PPG200 into a composite plasticizer;
[0071] S3, dissolving the composite plasticizer, the binder polyvinyl alcohol PVA and the dispersant polymer dispersant BYK111 in a solvent to prepare a premixed solution; the solvent is a mixture of ethanol and butanone in a mass ratio of 1:1; the mass ratio of the composite plasticizer, the binder and the solvent is 2.5:3.5:4; the amount of BYK111 is 5% of the mass of the alumina;
[0072] S4. Add the ceramic powder silicon nitride treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 85% of the mass of the ceramic slurry; the rotation speed of the ball mill is 600 rpm, and the ball milling time is 16 hours.
[0073] Comparative Example 1
[0074] This comparative example proposes a ceramic slurry, which is different from Example 1 in that only polyethylene glycol 600 is used as a plasticizer and is prepared by the following steps:
[0075] S1, the aluminum oxide was ball-milled at 200 rpm for 8 h with alcohol, and then dried and sieved at a drying temperature of 120° C. for 10 h to obtain aluminum oxide with a mesh size of 300-400 mesh;
[0076] S2, Sekisui G-260 as a plasticizer;
[0077] S3, dissolving Sekisui G-260, binder polyvinyl butyral PVB and dispersant polymer dispersant BYK111 in a solvent to prepare a premixed solution, wherein the solvent is a mixture of ethanol and butanone in a mass ratio of 1:1, and the mass ratio of the plasticizer, the binder and the solvent is 3:3:4; the amount of BYK111 is 3% of the mass of the alumina;
[0078] S4. Add the ceramic powder alumina treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 70% of the mass of the ceramic slurry; the rotation speed of the ball mill is 500 rpm, and the ball milling time is 16 hours.
[0079] Comparative Example 2
[0080] This comparative example proposes a ceramic slurry, which is different from Example 1 in that only dibutyl phthalate DBP is used as a plasticizer and is prepared by the following steps:
[0081] S1, the aluminum oxide was ball-milled at 200 rpm for 8 h with alcohol, and then dried and sieved at a drying temperature of 120° C. for 10 h to obtain aluminum oxide with a mesh size of 300-400 mesh;
[0082] S2, using dibutyl phthalate DBP as a plasticizer;
[0083] S3, dissolving the dibutyl phthalate DBP plasticizer, the binder polyvinyl butyral ester PVB and the dispersant polymer dispersant BYK111 in the above 2) in a solvent to prepare a premixed solution, wherein the solvent is a mixture of ethanol and butanone in a ratio of 1:1, and the mass ratio of the plasticizer, the binder and the solvent is 3:3:4; the amount of BYK111 is 3% of the mass of the alumina;
[0084] S4. Add the ceramic powder alumina treated in step S1 to the premixed liquid and transfer it to a planetary ball mill for ball milling to obtain a ceramic slurry; the amount of the ceramic powder added is 70% of the mass of the ceramic slurry; the rotation speed of the ball mill is 500 rpm, and the ball milling time is 16 hours.
[0085] Application Example 1
[0086] The ceramic slurries prepared in Examples 1-4, Comparative Example 1 and Comparative Example 2 are used for tape casting to prepare ceramic green bodies, comprising the following steps:
[0087] The ceramic slurry is introduced into the slurry tank of the tape casting machine. After the ceramic slurry flows out of the slurry tank, it drips into the tape casting belt. Then, the solvent evaporates after entering the drying tunnel, and the tape cast ceramic monolayer is formed. The tape cast ceramic monolayer is stacked using a warm isostatic press to prepare a ceramic green body.
[0088] Tape casting parameters: drying oven temperature is 80°C, belt speed is 3 mm / s, scraper blade thickness is 7 mm, warm isostatic pressing temperature is 120°C, and pressure is 3 MPa.
[0089] like Figure 1 As shown, the ceramic slurry prepared in Example 1 can effectively reduce the maximum heat absorption peak during the degreasing process from 4.98 to 3.98 Mw / mg, and reduce the thermal stress during the degreasing process by nearly 20%.
[0090] like Figure 2 As shown, the flexural strength of the ceramic green body prepared according to the steps of Application Example 1 of the ceramic slurry prepared in Example 1 is improved from 4.9 to 22.3 MPa compared with the ceramic green body prepared according to the steps of Application Example 1 of the ceramic slurry prepared in Example 1, while the thermal stress of green body degreasing is effectively suppressed, the flexural strength of the green body is only slightly decreased.
[0091] The ceramic green bodies prepared in Examples 1-4 and Comparative Examples 1-2 were used to prepare ceramics according to the following steps:
[0092] The ceramic green body is degreased and sintered in sequence to obtain ceramics, with a degreasing rate of 0.5°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 120 min, a sintering temperature of 1850°C, and a sintering time of 120 min.
[0093] The mechanical and thermal properties of the prepared ceramics were tested according to the standard GB / T 3962-2017. The results are as follows: Figure 3As shown, the flexural strength and thermal conductivity of the ceramics corresponding to the ceramic green bodies of Examples 1-4 are significantly better than those of the ceramics made from the ceramic green bodies of Comparative Examples 1-2. The thermal conductivity of the ceramics made from Examples 1-4 can be as high as over 310 W / m·K, and the flexural strength of the ceramics made from Examples 1-4 can be as high as over 210 MPa; the thermal conductivity of the ceramics made from Comparative Examples 1-2 is as low as over 200 W / m·K, and the flexural strength of the ceramics made from Examples 1-4 is as low as below 125 MPa.
[0094] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a ceramic slurry, characterized in that: The following steps are involved: mixing the first plasticizer and the second plasticizer into a composite plasticizer; Dissolving the composite plasticizer, binder and dispersant in a solvent to prepare a premixed liquid; Adding the ceramic powder to the premixed liquid and ball-milling to obtain a ceramic slurry; The first plasticizer is one or more of Sekisui G-260, propylene glycol adipate polyester, tricresyl phosphate, polyethylene glycol PEG400, polyethylene glycol PEG600 and polypropylene glycol PPG400; The second plasticizer is one or more of dibutyl phthalate DBP, polyethylene glycol PEG200, polypropylene glycol PPG200 and diethylene glycol DEG.
2. The method for preparing a ceramic slurry according to claim 1, characterized in that: The mass ratio of the first plasticizer to the second plasticizer is (2-3):(2-3).
3. The method for preparing ceramic slurry according to claim 1, characterized in that: The binder is one or two of polyvinyl butyral PVB and polyvinyl alcohol PVA; and / or the dispersant is a high molecular polymer dispersant, and the high molecular polymer dispersant is one or more of BYK111, BYK163 and Sago9900; the amount of the dispersant is 2%-5% of the mass of the ceramic powder.
4. The method for preparing ceramic slurry according to claim 1, characterized in that: The solvent is a mixture of ethanol and butanone, and the mass ratio of the ethanol to the butanone is 1:(1-1.5); and / or the mass ratio of the composite plasticizer, the binder and the solvent is (2-3):(3-4):4; and / or the added amount of the ceramic powder is 60%-85% of the mass of the ceramic slurry.
5. The method for preparing ceramic slurry according to claim 1, characterized in that: The mesh number of the ceramic powder is 300-400 meshes.
6. The method for preparing ceramic slurry according to claim 1, characterized in that: The ceramic powder is obtained by the following steps: wet grinding the ceramic powder with alcohol, the ball milling time is 4-8 hours, the ball milling speed is 200-400rpm, and after wet grinding, the ceramic powder is dried in an oven, the drying temperature is 120-150°C, and the drying time is 6-10 hours.
7. The method for preparing ceramic slurry according to claim 1, characterized in that: The rotation speed of the ball mill is 400-600 rpm, and the time of the ball mill is 10-24 hours.
8. A ceramic slurry, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the ceramic slurry obtained by the preparation method according to any one of claims 1 to 7 or the ceramic slurry according to claim 8 in preparing ceramic green bodies by tape casting.
10. The use according to claim 9, characterized in that: include: The ceramic slurry is introduced into the slurry tank of the tape casting machine, and the ceramic slurry flows out of the slurry tank and drips into the tape casting belt, and then enters the drying tunnel to evaporate the solvent, and the tape casting ceramic monolayer is formed, and the tape casting ceramic monolayer is stacked by a warm isostatic press to prepare a ceramic green body; Tape casting parameters: drying oven temperature is 60-100°C, belt speed is 1-5mm / s, scraper blade thickness is 5-10mm, warm isostatic pressing temperature is 100-150°C, and pressure is 1-5MPa.
Citation Information
Patent Citations
Water-based debinding binder used for ceramic injection moulding
CN108947545A
Solid-phase sintered silicon carbide product and preparation method thereof
CN113831136A
Silicon nitride ceramic substrate and preparation method thereof
CN116462515A
Silicon nitride ceramic substrate and preparation method and application thereof
CN117185825A
Plastic material for the preparation of glass-ceramic foam, glass-ceramic foam prepared from this material and a method of preparation of this glass-ceramic foam
WO2023116954A1