Porous aluminum oxide, battery diaphragm, battery and electric equipment
By using porous alumina particles with mesoporous surface and interior in the battery separator, controlling their morphology and particle size distribution, the problem of taking into account the fluidity and base film support role of alumina particles in the coating is solved, and the separator is improved The heat shrinkability and surface flatness improve the reliability and stability of the battery.
Patent Information
- Application Number
- CN202411525869.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-30
AI Technical Summary
In the prior art, alumina particles are difficult to take into account high fluidity and good base film support in the battery separator coating, resulting in poor heat shrinkability and surface flatness of the separator.
The porous alumina particles with mesoporous presence on the surface and inside are used to control their morphology as quadrilateral prism crystals with a thickness of no less than 20% of the length of the bottom surface. The rest angle is in the range of 36°~38.5°, and the particle size distribution is narrow. A uniform coating is formed to improve the heat shrinkability and surface flatness of the membrane.
By optimizing the morphology and particle size distribution of porous alumina particles, good coating dispersion and surface flatness are formed, the thermal shrinkage and mechanical strength of the separator are improved, and the reliability and stability of the battery are improved.
Smart Images

Figure CN119038968A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to porous alumina, a battery separator, a battery, and electrical equipment. Background Art
[0002] In order to increase the mechanical properties, heat resistance and breakdown voltage of diaphragms based on high molecular polymers such as polyolefins, a ceramic coating with ceramic particles added is often formed on one or both sides of the polymer film (base film) in the prior art. Alumina particles, as a common ceramic particle with high strength, thermal stability and strong chemical stability, have become the preferred material for ceramic particles in the ceramic coating.
[0003] The coating of the diaphragm not only places requirements on the strength, thermal stability and chemical stability of the ceramic particles, but also places requirements on the self-fluidity of the ceramic particles and their support for the base film based on the requirements of the heat shrinkage performance and surface flatness of the diaphragm. However, alumina particles have a high affinity with water, and are difficult to dry and disperse. In order to meet the requirements of the dispersibility and self-fluidity of alumina, alumina particles with excellent self-fluidity are often used as coating ceramics for diaphragms in the prior art. However, their support for the base film is poor, resulting in poor improvement in the heat shrinkage of the resulting diaphragm; and alumina particles with poor self-fluidity are prone to poor dispersibility and poor uniformity of the formed coating, affecting the surface flatness of the diaphragm. Summary of the invention
[0004] The object of the present invention is to provide a porous alumina, the particles of which are mainly quadrangular prism-shaped crystals with a thickness not less than 20% of the length of the bottom side, and a repose angle not higher than 38.5° and not lower than 36°, so that the surface flatness of the coating formed based on the porous alumina can be improved.
[0005] Another object of the present invention is to provide a battery separator.
[0006] Another object of the present invention is to provide a battery.
[0007] Another object of the present invention is to provide an electrical device.
[0008] In a first aspect, the present application provides a porous alumina, wherein the porous alumina is an alumina particle having a plurality of mesopores on the surface and / or inside of the particle; and the alumina particle is a quadrangular prism crystal having a thickness not less than 20% of the length of the bottom side; and the cumulative particle size D50 of 50% of the particles on the small particle size side in the cumulative particle size distribution is 0.3-2 μm; The repose angle of the porous alumina is 36.0°~38.5°.
[0009] Further, in some embodiments of the present application, the repose angle of the porous alumina is 38.1° to 38.5°; and / or The maximum particle size D of the porous alumina max Not higher than 4μm.
[0010] Further, in some embodiments of the present application, the particle size distribution of the porous alumina satisfies the following formula: SPAN1=D99 / D50<2.5; SPAN2=(D90-D50) / D10<1.5.
[0011] Furthermore, in some embodiments of the present application, the cumulative particle size D50 of 50% of the particles on the small particle size side in the cumulative particle size distribution of the porous alumina is 0.4-1.2 μm.
[0012] Furthermore, in some embodiments of the present application, the particle size distribution satisfies the following formula: SPAN1=D99 / D50<2.0; SPAN2=(D90-D50) / D10<1.2.
[0013] Furthermore, in some embodiments of the present application, the maximum particle size D of the porous alumina is max Not higher than 2μm.
[0014] Further, in some embodiments of the present application, the specific surface area of the porous alumina is 5 to 50 m 2 / g within this range; The apparent density of the porous alumina is 2-3 g / cm 3 .
[0015] Furthermore, in some embodiments of the present application, the pore volume of the porous alumina is 0.01-0.4 cm 3 / g; The particles in the porous alumina powder are at least one of the θ phase, δ phase, γ phase, and α phase, or at least one of the η phase, κ phase, χ phase, and ρ phase.
[0016] In a second aspect, the present application further provides a battery separator, which includes a substrate and a coating formed on at least one side of the substrate, wherein the porous alumina described in the first aspect is distributed in the coating.
[0017] Further, in some embodiments of the present application, the thickness uniformity δ of the coating is not higher than 0.3; The test method for thickness uniformity is: Take 6 points on the surface array of the base film with coating and obtain the thickness S of the coating at each point.n , where n is the number of the measurement point, which is a natural number in the range of 1 to 6. The average thickness S of the coating is calculated. 均 The square root of the sum of the squares of the coating differences measured at each point is calculated as follows: δ = ((S1-S 均 ) 2 + (S2-S 均 ) 2 ……(S6-S 均 ) 2 ) 1 / 2 .
[0018] Further, in some embodiments of the present application, the number of surface convex points of the coating is no higher than 1 / 100 cm2; The testing method of the number of convex points is: The base film with the coating was stretched and placed under light, and the number of black spots was observed from the back and counted. Furthermore, in some embodiments of the present application, the coating thickness in the battery separator is 1-5 μm, and the proportion of porous alumina in the coating is 90%-99% by mass.
[0019] In a third aspect, the present application further provides a battery, comprising the battery separator described in the second aspect.
[0020] In a fourth aspect, the present application also provides an electrical device, comprising the battery described in the third aspect.
[0021] The embodiments of the present application provide a porous alumina, an electronic diaphragm, a battery, and an electrical device. The repose angle and morphology of the porous alumina are controlled within a specific range, so that the dispersion of the porous alumina in the coating formed by it is good, the flatness of the coating surface is better, the convex points on the coating surface are reduced, and the damage to the battery caused by the convex points on the coating surface is avoided, and it is beneficial to improve the heat shrinkage of the diaphragm, and it is beneficial to improve the stability and reliability of the battery. In addition, the surface and interior of the alumina particles of the porous alumina provided by the present application also contain a large number of mesopores, which can provide channels for ion conduction and reduce the unit surface density of the diaphragm; at the same time, its specific surface area is controlled so that its specific surface area is at a lower level, avoiding the high surface area of the alumina particles and the high affinity with water, which makes it difficult to reduce the water content to the required content, thereby introducing water molecules into the battery that are not conducive to its reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a SEM image of the porous alumina provided for use in this application. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] [Apparent density ρ1] The apparent density ρ1 mentioned in the present application is the ratio of the mass of the material of the solid particles to the apparent volume, wherein the apparent volume is the sum of the solid volume of the solid particles and the volume of the closed pores and the volume of the open pores, which can be used to indicate the proportion of the pore volume in the particles; when the difference between the apparent density of the particles and the theoretical density is higher, the pore volume of the particles is higher; when the difference between the apparent density of the particles and the theoretical density is lower, the pore volume of the particles is lower.
[0025] [Angle of repose] The angle of repose mentioned in this application refers to the maximum angle measured when the gravity and friction between particles are balanced when the particles slide on the free slope of the powder accumulation layer in the gravitational field and are in a static state, which can be used to indicate the self-fluidity of the particles. The larger the angle of repose of the particle accumulation state, the worse the self-fluidity of the particles; the smaller the angle of repose of the particle accumulation state, the better the self-fluidity of the particles.
[0026] The present application provides a porous alumina, such as Figure 1 As shown, there are a number of mesoporous (2-50 nm) alumina particles on the surface and / or inside of the porous alumina particles; and the alumina particles are quadrangular prism-shaped crystals with a thickness not less than 20% of the length of the bottom side; and the particle size D50 is 0.3-2 μm.
[0027] Among them, D50 is the cumulative particle size of 50% of the particles on the small particle size side in the cumulative particle size distribution; D90 is the cumulative particle size of 90% of the particles on the small particle size side in the cumulative particle size distribution; D99 is the cumulative particle size of 99% of the particles on the small particle size side in the cumulative particle size distribution; D10 is the cumulative particle size of 10% of the particles on the small particle size side in the cumulative particle size distribution; Dmax is the cumulative particle size of 99.9% of the particles on the small particle size side in the cumulative particle size distribution.
[0028] In order to provide support for the base film and reduce the heat shrinkage rate of the diaphragm, it is required that the ceramic particles used in the diaphragm coating are not easy to flow in a mutually dislocated manner when coated on the base film, which is mainly manifested in the poor self-fluidity of the ceramic particles. However, ceramic particles with poor self-fluidity are difficult to form a coating with good surface flatness on the surface of the base film due to their poor dispersibility and fluidity. It can be seen that it is difficult to have both reduced heat shrinkage of the diaphragm and good surface flatness and uniformity of distribution of ceramic particles in the coating. Based on this technical problem, the applicant found that by controlling the morphology of the alumina particles to be a tetrahedral crystal with a specific thickness not less than 20% of the length of the bottom side and the repose angle of the alumina particles within the range of 36°~38.5°, the distribution uniformity of the alumina particles in the coating formed by the alumina is good, the surface flatness of the coating is good, and the improvement of the heat shrinkage of the diaphragm is also better, which is beneficial to the optimization of the thermal properties, mechanical strength and breakdown voltage of the diaphragm, and is also beneficial to improving the reliability of the battery.
[0029] It should be noted that the "morphology of the aluminum oxide particles is a tetrahedral crystal with a specific thickness not less than 20% of the length of the bottom side" proposed in the present application should be understood as the aluminum oxide particles provided in the present application having a morphology mainly composed of tetrahedral crystals with a thickness not less than 20% of the length of the bottom side, rather than each particle in the aluminum oxide particles being a tetrahedral crystal with a thickness not less than 20% of the length of the bottom side. Exemplarily, the proportion of tetrahedral crystals with a thickness not less than 20% of the length of the bottom side in the porous aluminum oxide provided in the present application is not less than 60%, or not less than 70%, not less than 80%; preferably, the proportion of tetrahedral crystals with a thickness not less than 20% of the length of the bottom side in the porous aluminum oxide provided in the present application is not less than 90%, and more preferably not less than 95%.
[0030] The proportion of alumina particles of other morphologies in the porous alumina provided in the present application needs to be controlled within 40%, especially spherical or quasi-spherical alumina particles are preferably controlled within 5%, the total amount of needle-shaped, rod-shaped or fiber-shaped alumina particles is preferably controlled within 2%, and the total amount of needle-shaped, rod-shaped or fiber-shaped alumina particles is more preferably controlled within 1%, which is beneficial for achieving the desired dispersion of the porous alumina and the surface smoothness of the coating while maintaining the improvement of the thermal shrinkage of the porous alumina on the diaphragm.
[0031] More preferably, the ratio of the thickness (the length of the side in the Z-axis direction) to the length of the bottom side (the length of the longest side on the surface formed by the X-axis and the Y-axis) of the porous alumina provided in the present application is preferably 0.6-1.8, more preferably 0.6-0.9 or 1.2-1.8. That is, the ratio of the thickness to the bottom side of the porous alumina provided in the present application falls within the range of 0.6-1.8, and the proportion of particles is more preferred. More preferably, the ratio of the thickness to the bottom side of the porous alumina provided in the present application falls within the range of 0.6-0.9 or 1.2-1.8, and the proportion of particles is more preferred.
[0032] In order to further improve the ion conduction performance of the diaphragm, the alumina particles provided in the present application are porous alumina particles with a large number of mesopores on the surface and inside, which not only provide channels for ion conduction, but also can reduce the surface density of the coating, making the diaphragm lightweight. At the same time, the applicant also found that the pores on the surface and inside of the alumina particles provided in the present application are controlled to the size of mesopores (2~50nm), which can also be beneficial to the control of the self-fluidity of the porous alumina provided in the present application. Preferably, the pores on the surface and inside of the alumina provided in the present application are controlled to a size of 8~30nm, which is more advantageous, which is not only beneficial to the control of the self-fluidity of the porous alumina, but also more advantageous to the ion conduction speed of lithium ions in the pores, making its ion conductivity better, and the control of the specific surface area of the porous alumina, reducing the amount of binder used in the coating entering the mesopores, reducing the amount of binder used, and leaving space for the absorption and storage of the electrolyte.
[0033] The specific surface area of the porous alumina provided in this application can be controlled to be 5-50 m 2 / g, which is beneficial to control the affinity of aluminum oxide to water molecules and reduce the hydroxyl content on the surface of aluminum oxide; and the apparent density of the porous aluminum oxide is 2-3g / cm 3 , making the surface density of the coating smaller and the diaphragm significantly lighter.
[0034] Preferably, the maximum particle size D of the porous alumina provided in the present application is max It can also be controlled within the range of no more than 4 μm, which is more conducive to the diaphragm coating to reduce the number of surface protrusions of the diaphragm coating and further optimize the surface flatness of the coating. In addition, the particle size distribution of the porous alumina provided in the present application preferably also satisfies: SPAN1=D99 / D50<2.5; SPAN2=(D90-D50) / D10<1.5.
[0035] The porous alumina has a narrow particle size distribution, which is more conducive to improving the distribution uniformity and surface flatness of the porous alumina of the coating, and is also conducive to the retention of ion transmission channels in the coating, and is more conducive to the optimization of the ion conductivity of the diaphragm.
[0036] In addition, the porous alumina provided by the present application has a more obvious technical effect in thin coatings with a coating thickness of less than 2 μm. When the porous alumina provided by the present application is applied to thin coatings with a coating thickness of no more than 2 μm, the particle size D50 of the porous alumina is preferably 0.4 to 1.2 μm, the angle of repose is preferably 38.1° to 38.5°, and the maximum particle size D max The surface flatness of the membrane coating formed by porous alumina within this range is better than 2μm, and its optimization of the thermal shrinkage of the membrane is more obvious. In addition, due to the thin coating thickness, the membrane formed based on this porous alumina has a low surface density and the membrane is more lightweight.
[0037] On this basis, the particle size distribution of the porous alumina provided in the present application can be further controlled within the range of: SPAN1=D99 / D50<2.0, SPAN2=(D90-D50) / D10<1.2, which is more conducive to improving the surface flatness and optimizing the heat shrinkage rate of the diaphragm coating.
[0038] In addition, the applicant has also found that further controlling the cumulative particle size D50 of 50% of the particles on the small particle size side in the porous alumina cumulative particle size distribution of the porous alumina provided in the present application and the product of the specific surface area BET and the apparent density ρ of the porous alumina can further optimize the diaphragm of the coating formed by the alumina provided in the present application, so that it is better in the surface hydroxyl content of the porous alumina particles and the surface density of the coating when it is used in the diaphragm coating. Among them, the product of the particle size D50 of the porous alumina and the specific surface area BET and the apparent density ρ needs to satisfy the following formula: 15<D50╳BET╳ρ<75 When the product of the particle size D50 of the porous alumina provided in the present application, the specific surface area BET, and the apparent density ρ is controlled within this range, the surface hydroxyl content of the alumina can reach 5 / nm 2 Below, and the membrane formed by the coating can reduce the unit area density of the coating with a solid content (alumina particle content in the coating) of 93% to 4g / (m 2 ·μm), the unit surface density of the formed coating can even be reduced to 2g / (m 2 ·μm).
[0039] Preferably, the product of the particle size D50 of the porous alumina, the specific surface area BET, and the apparent density ρ satisfies the following formula: 20<D50╳BET╳ρ<60 More preferably, for porous alumina particles within different particle size ranges, the product of the particle size D50 of the porous alumina and the specific surface area BET and the apparent density ρ is within a corresponding range, which is more conducive to the optimization of its coating surface density, ion conductivity and coating performance. For example, when the particle size D50 of porous alumina is 0.3~0.4μm and its SPAN1=D99 / D50<2.0, SPAN2=(D90-D50) / D10<1.2, its D50╳BET╳ρ value is preferably in the range of 19~25, and the surface uniformity value δ of its coating can be controlled within 0.2; and when the particle size D50 of porous alumina is 0.8~1.0 and its SPAN1=D99 / D50<2.2, SPAN2=(D90-D50) / D10<1.2, its D50╳BET╳ρ value is preferably in the range of 48~55, and the surface uniformity value δ of its coating can be controlled within 0.3.
[0040] The porous alumina provided in this application has a pore volume of 0.02-0.4 cm 3 / g, preferably 0.05-0.2cm 3 / g.
[0041] In the porous alumina provided in the present application, the particles in the porous alumina are at least one of α-alumina, θ-alumina, and δ-alumina. It is preferred that γ-alumina is not included, or the content of γ-alumina in the porous alumina provided in the present application is not more than 5% by mass, so as to improve the chemical stability of the porous alumina and reduce the activity.
[0042] In the porous alumina powder provided in the present application, the particles in the porous alumina powder are at least one of the θ phase, δ phase, γ phase, α phase or at least one of the η phase, κ phase, χ phase, ρ phase.
[0043] It should be noted that when the porous alumina powder includes γ-phase alumina, it includes at least one of δ-phase, η-phase, κ-phase, χ-phase, and ρ-phase alumina in addition to the γ-phase alumina; when the porous alumina powder includes α-phase alumina, the content of α-alumina in the porous alumina powder is not higher than 5%, and more preferably not higher than 2%.
[0044] That is, the porous alumina powder provided in the present application can be any one of the pure phase of θ-alumina and mixed phase alumina with other phases, the pure phase of δ-alumina and mixed phase alumina with other phases, the pure phase of η-alumina and mixed phase alumina with other phases, the pure phase of κ-alumina and mixed phase alumina with other phases, the pure phase of χ-alumina and mixed phase alumina with other phases, the pure phase of ρ-alumina and mixed phase alumina with other phases, the mixed phase alumina of γ-alumina and other phases, and the mixed phase alumina of α-alumina and other phases. Preferably, the porous alumina powder is preferably the pure phase of θ-alumina and mixed phase alumina with other phases, the pure phase of δ-alumina and mixed phase alumina with other phases, the pure phase of η-alumina and mixed phase alumina with other phases, the pure phase of κ-alumina and mixed phase alumina with other phases, the pure phase of χ-alumina and mixed phase alumina with other phases, and the pure phase of ρ-alumina and mixed phase alumina with other phases. Furthermore, in order to improve the porous alumina provided in the present application, the content of γ-alumina in the porous alumina provided in the present application is preferably lower, such as lower than 10% or lower than 8%, so as to improve the chemical stability of the porous alumina and reduce the activity.
[0045] In some embodiments, the content of metal elements in the porous alumina powder is: the content of metal elements in the porous alumina powder is: sodium ion content: 0-300ppm; calcium ion content: 0-300ppm; iron ion content: 0-200ppm; silicon ion content: 0-300ppm; cobalt ion content: 0-50ppm; copper ion content: 0-50ppm; zinc ion content: 0-50ppm; lead ion content: 0-50ppm; chromium ion content: 0-50ppm; nickel ion content: 0-50ppm; zirconium ion content: 0-3000ppm; tin ion content: 0-50ppm.
[0046] More preferably, the sum of the contents of metal elements in the porous alumina powder is not higher than 5000 ppm. More preferably, the sum of the contents of iron, cobalt, chromium, zinc and nickel in the porous alumina powder is not higher than 500 ppm, so as to avoid the side reactions of the impurity elements with the electrolyte and the positive and negative electrodes during the charge and discharge process of the battery, increase the consumption of the electrolyte, generate gas and reduce the ion conductivity, which is conducive to reducing the damage of these impurities to the battery.
[0047] The sum of the contents of metal elements such as iron, cobalt, chromium, zinc and nickel in the porous alumina provided by the present application is relatively low. The reason may be that the porous alumina particles provided by the present application are mainly single crystal particles, and the integrity of the crystal particles is relatively high; and in the preparation process, the porous formation is not formed by granulation, but by the escape of water molecules in the crystal particles and the displacement of atoms during the crystal phase change process; making it difficult for metal elements to embed into the porous alumina particles and attach to the surface of the single crystal particles, making it easier for other metal ions in ionic state to remain in the reaction system and be removed by cleaning or demagnetization and impurity removal.
[0048] Preferably, the porous alumina provided in the present application is directly prepared from raw materials without compounding, sorting and mixing of multiple porous aluminas.
[0049] [Method for preparing porous alumina] The porous alumina provided in the present application can be an intermediate obtained by controlling the growth of aluminum hydroxide or aluminum ions through a hydrothermal reaction with crystal seeds as crystal nuclei, and the porous alumina particles with a specific morphology, a specific particle size range and a specific repose angle can be obtained by adjusting the pH value of the system after the hydrothermal reaction and before drying, and then controlling the temperature curve of the calcination process in the presence of a barrier agent after drying and crushing.
[0050] In this preparation method, the seed crystal used is alumina monohydrate with a particle size not exceeding 80 nm, and the content of water of crystallization of the intermediate obtained is preferably controlled at 1-1.2, and the purity of the alumina monohydrate crystals in the intermediate is controlled at more than 99% through a hydrothermal process and a pH adjustment process, and the particle size of the grown intermediate satisfies D50 of 0.3-2 μm, and its morphology is mainly tetrahedral crystals with a specific thickness not less than 20% of the length of the bottom side.
[0051] In order for those skilled in the art to better understand and implement the present application, an example of the preparation method of the porous alumina is provided below: Preparation method: Step (1): providing aluminum hydroxide, seed crystals and pure water, mixing aluminum hydroxide, additives and pure water, grinding for 30 min to 60 min, immediately adding seed crystals, mixing and simultaneously heating to 60° C. to 80° C., stirring for reaction for 1 h to 3 h; then heating to 150° C. to 200° C., keeping the temperature for reaction for 4 h to 48 h, to obtain an intermediate; controlling the reaction pressure to be 1.4 to 3.7 MPa; Step (2): adjusting the pH value of the system, and drying the intermediate powder by infrared microwave drying after filter pressing to form an intermediate powder, wherein the free water content in the intermediate powder is controlled to be no higher than 0.2%, and the crystal water content is controlled to be no higher than 1.2 water molecules; Step (3): adding a barrier agent, mixing the intermediate evenly, calcining at 600°C to 1200°C for 0.5 to 5 hours, and jet milling to obtain porous alumina.
[0052] In the system formed by aluminum hydroxide, additives and pure water, the amount of additive added is 0.01~1% by mass fraction; the amount of aluminum hydroxide added is 10~30% by mass fraction. The amount of seed added is 0.01~0.2% of this system. It should be noted that the particle size of the seed is not higher than 80nm; if alcohol is added to the additive, the amount of alcohol added is not less than 30% of the dispersant and not more than 60% of the dispersant.
[0053] The alcohol used here can be one or more of common alcohol solvents such as ethanol, propanol, n-butanol, isobutanol, amyl alcohol, isopentanol, etc.
[0054] After the intermediate is obtained, the pH value of the intermediate slurry is adjusted to 7.2-8.3, preferably 7.5-8.0, with an organic acid, and the intermediate slurry is dried by infrared microwave drying. The drying method can also be spray drying. When spray drying is adopted, a disintegration step is also included after spray drying and before calcination, and the dried particles are dispersed into a particle size D50 of 0.3-2 μm by air jet milling or grinding.
[0055] When infrared microwave drying is used, the intermediate powder after drying does not need to be broken up or crushed, and can directly enter the calcination process, saving costs and improving the morphological integrity of the product. In addition, in order to achieve a good dispersion effect, when infrared microwave drying is used, the slurry is first filtered into a filter cake with a free water content of not less than 65%, and then broken into small pieces of filter cake, and then heated to a temperature of not less than 150°C by infrared light irradiation, treated for 8-15 minutes, and then cooled to 80-100°C, and treated with microwave heating for 3-10 minutes, and then heated to above 150°C by microwave heating until the small filter cake automatically explodes into powder. Similarly, the intermediate powder formed by segmented drying using the infrared microwave drying process has a low water content, which can reach a water content (free water) of not more than 0.2%, and in this process, the appearance of the particles is not damaged by grinding or ball milling, and the integrity is better. Moreover, since there is no high-temperature spraying process and the process of automatic explosion into powder, the crystal particles in the obtained powder are less agglomerated, and the single crystal dispersion of the product is better.
[0056] The intermediate prepared by the method also has a crystalline water content of no more than 1.2 water molecules in terms of the number of crystalline molecules, preferably 1 to 1.2 crystalline water molecules, and a mainly quadrangular prism-shaped morphology, with a particle size mainly distributed in the range of 0.3 to 2 μm.
[0057] In step (3), a small amount of a barrier agent that can be decomposed into gas at a relatively low temperature is added, and the decomposition temperature of the barrier agent is not higher than 450°C, more preferably not lower than 50°C and not higher than 100°C. Exemplarily, the barrier agent can be ammonium bicarbonate, ammonium carbonate, ammonium nitrate, preferably ammonium carbonate; the amount of the barrier agent is 0.01% to 0.1% by mass of the dried intermediate powder obtained in step (2). The barrier agent can be added in the drying stage or in the calcination stage. When it is added in the calcination stage, it can also reduce the adhesion of particles to the wall of the container used for calcination during the calcination process. The temperature curve of the calcination process is preferably: rapidly heating to at least 300°C at a heating rate of not less than 8°C / min, reducing the heating rate (heating rate is not higher than 2°C / min) and then heating to the holding temperature, and then sintering for 0.5h to 5h to obtain the product, so as to promote the single crystal morphology of the porous alumina particles to be maintained, and the pore size and pore volume to be controlled.
[0058] In this preparation method, the inventors found that directly adjusting the acidity of the slurry after the reaction can promote the consistency of the crystal structure and particle size of the product and the pore size distribution. The reason may be that directly adjusting the acidity after the reaction can curb the formation of alumina trihydrate, so that the intermediate obtained has higher purity, and a large number of defects appear on the intermediate, providing biased guidance for the subsequent formation and development of pores.
[0059] In a second aspect, the present application further provides a battery separator, which includes a substrate and a coating formed on at least one side of the substrate, wherein the porous alumina described in the first aspect is distributed in the coating.
[0060] Wherein, the thickness uniformity δ of the coating layer formed based on the porous alumina is not higher than 0.3.
[0061] Preferably, the number of surface convex points of the coating formed based on the porous alumina can be as low as no more than 1 / m 2, and its heat shrinkage can be reduced to within 2.2% in MD (transverse direction) and within 2.7% in TD (vertical direction). For porous alumina suitable for thin coatings (coating thickness within 2μm), when its particle size is within 0.4~1.2μm and Dmax is within 2μm, SPAN1≤2, SPAN2≤1.2, and the repose angle is within the range of 36°~38.5°, the heat shrinkage of the coating formed based on the porous alumina can be optimized to less than 1.9% in MD (transverse direction) and within 1.4% in TD (vertical direction), and the thickness uniformity of the coating can be optimized to within 0.27. More preferably, when the porous alumina has a particle size within the range of 0.4-0.8 μm and Dmax within 2 μm, SPAN1≤2, SPAN2≤1.2, and an angle of repose within the range of 38.5°-40.5°, the heat shrinkage of the coating formed based on the porous alumina can be optimized to less than 1.2% in MD (transverse direction) and within 1.1% in TD (longitudinal direction), and the thickness uniformity of the coating can be optimized to within 0.2.
[0062] Wherein, the testing method of thickness uniformity is: Take 6 points on the surface array of the base film with coating and obtain the thickness S of the coating at each point. n , where n is the number of the measurement point, which is a natural number in the range of 1 to 6. The average thickness S of the coating is calculated. 均 The square root of the sum of the squares of the differences between the coating thickness measured at each point is calculated as follows: δ = ((S1-S 均 ) 2 + (S2-S 均 ) 2 ……( S6-S 均 ) 2 ) 1 / 2 .
[0063] The thickness uniformity δ represents the standard deviation of the thickness of the coating at each position on the diaphragm compared to the average value, which can be used to indicate the uniformity of the thickness of the coating formed on the diaphragm.
[0064] The testing method of the number of convex points is: The base film with the coating was stretched and placed under light, and the number of black spots was observed from the back and counted.
[0065] The number of bumps is tested based on the principle that powder agglomeration / large particles will cause light to be blocked and appear as black spots. It can be used to indicate the number of bumps on the coating surface. The more bumps there are, the poorer the thickness uniformity of the coating is, and the poorer the dispersion of the aluminum oxide particles in the coating is. The more bumps there are, the more reliability the battery has.
[0066] Preferably, the coating thickness in the battery separator is 1-5 μm, and the proportion of porous aluminum oxide in the coating is 90%-99% by mass.
[0067] In a third aspect, the present application further provides a battery, comprising the battery structure described in the second aspect.
[0068] In a fourth aspect, the present application further provides an electric device, comprising the battery described in the third aspect. The electric device may be an electric vehicle, an aircraft, an aircraft, a mobile phone, a tablet computer, a handheld game console, a portable digital device (such as a digital camera), a smart home, a smart wearable (such as a smart bracelet, a smart watch, smart glasses), or any other electric device that can use an ion battery.
[0069] In order to facilitate those skilled in the art to understand the innovation of the present application, some preferred embodiments are provided below in conjunction with the accompanying drawings to illustrate the above technical solution.
[0070] Fabrication of porous alumina Example 1 Step (1): providing aluminum hydroxide, seed crystals, and pure water, mixing aluminum hydroxide and pure water, grinding for 40 minutes, immediately adding seed crystals, mixing and simultaneously heating to 65°C, stirring and reacting for 2 hours; then heating to 170°C, keeping the temperature for 10 hours to obtain an intermediate; controlling the reaction pressure to 2 MPa; Step (2): adjusting the pH value of the system to 7.8, and filtering the slurry into a filter cake with a free water content of not less than 65%, and breaking it into small pieces of filter cake, and then heating it to a temperature of not less than 150° C. by infrared light irradiation, treating it for 10 minutes, and then cooling it to 80° C., and treating it with microwaves for 8 minutes, and then heating it to more than 150° C. by microwaves, until the small filter cakes automatically explode into powder; Step (3): add ammonium carbonate barrier agent with a mass fraction of 0.05% and a mass percentage of 100% of alumina, mix well with the intermediate, and then quickly heat up to 300°C at a heating rate of 8°C / min, reduce the heating rate to 2°C / min and then heat up to 1100°C, then keep warm and sinter for 3h, and after air flow milling, obtain sample 1 of porous alumina.
[0071] Example 2 Step (1): provide aluminum hydroxide, seed crystals, and pure water, mix aluminum hydroxide and pure water, grind for 50 minutes, immediately add seed crystals, mix and simultaneously heat to 65°C, stir and react for 2 hours; then heat to 170°C, keep warm and react for 10 hours to obtain an intermediate; control the reaction pressure to 2 MPa; Step (2): adjusting the pH value of the system to 7.8, and filtering the slurry into a filter cake with a free water content of not less than 65%, and breaking it into small pieces of filter cake, and then heating it to a temperature of not less than 150° C. by infrared light irradiation, treating it for 10 minutes, and then cooling it to 80° C., and treating it with microwaves for 8 minutes, and then heating it to more than 150° C. by microwaves, until the small filter cakes automatically explode into powder; Step (3): add ammonium carbonate barrier agent with a mass fraction of 0.05% and a mass percentage of 100% of alumina, mix well with the intermediate, and then quickly heat up to 300°C at a heating rate of 8°C / min, reduce the heating rate to 2°C / min, and then heat up to the insulation temperature, and then sinter at this temperature for 3 hours. After air flow milling, obtain sample 2 of porous alumina.
[0072] Example 3 Step (1): provide aluminum hydroxide, seed crystals, and pure water, mix aluminum hydroxide and pure water, grind for 50 minutes, immediately add seed crystals, mix and simultaneously heat to 65°C, stir and react for 3 hours; then heat to 170°C, keep warm and react for 15 hours to obtain an intermediate; control the reaction pressure to 2MPa; Step (2): adjusting the pH value of the system to 7.8, and filtering the slurry into a filter cake with a free water content of not less than 65%, and breaking it into small pieces of filter cake, and then heating it to a temperature of not less than 150° C. by infrared light irradiation, treating it for 10 minutes, and then cooling it to 80° C., and treating it with microwaves for 8 minutes, and then heating it to more than 150° C. by microwaves, until the small filter cakes automatically explode into powder; Step (3): add ammonium carbonate barrier with a mass fraction of 0.03% and a mass percentage of 100% of alumina, mix well with the intermediate, and then quickly heat up to 300°C at a heating rate of 8°C / min, reduce the heating rate to 2°C / min, and then heat up to the insulation temperature, and then sinter at this temperature for 3 hours. After air flow milling, obtain sample 3 of porous alumina.
[0073] Example 4 Step (1): provide aluminum hydroxide, seed crystals, and pure water, mix aluminum hydroxide and pure water, grind for 40 minutes, immediately add seed crystals, mix and simultaneously heat to 65°C, stir and react for 3 hours; then heat to 170°C, keep warm and react for 15 hours to obtain an intermediate; control the reaction pressure to 2MPa; Step (2): adjusting the pH value of the system to 7.8, and filtering the slurry into a filter cake with a free water content of not less than 65%, and breaking it into small pieces of filter cake, and then heating it to a temperature of not less than 150° C. by infrared light irradiation, treating it for 10 minutes, and then cooling it to 80° C., and treating it with microwaves for 8 minutes, and then heating it to more than 150° C. by microwaves, until the small filter cakes automatically explode into powder; Step (3): add ammonium carbonate barrier agent with a mass fraction of 0.03% and a mass percentage of 100% of alumina, mix well with the intermediate, and then quickly heat up to 300°C at a heating rate of 8°C / min, reduce the heating rate to 2°C / min, and then heat up to the insulation temperature, and then sinter at this temperature for 3 hours. After air flow milling, obtain sample 4 of porous alumina.
[0074] Comparative Example 1 Compared with Example 1, the mixing and grinding time of aluminum hydroxide and pure water in this comparative example is 30 minutes; the remaining steps are the same as those in Example 1, and a comparative sample 1 is obtained.
[0075] Comparative Example 2 Compared with Example 2, the mixing and grinding time of aluminum hydroxide and pure water in this comparative example is 35 minutes; the remaining steps are the same as those in Example 1, and comparative sample 2 is obtained.
[0076] Comparative Example 3 Compared with Example 3, the mixing and grinding time of aluminum hydroxide and pure water in this comparative example is 35 minutes; the remaining steps are the same as those in Example 3, and comparative sample 3 is obtained.
[0077] Comparative Example 4 Compared with Example 4, the mixing and grinding time of aluminum hydroxide and pure water in this comparative example is 30 minutes; the remaining steps are the same as those in Example 4, and comparative sample 4 is obtained.
[0078] [Testing of porous alumina] The obtained porous alumina was subjected to particle size distribution test, specific surface area test, apparent density test, repose angle test and morphology characterization. The specific test methods are as follows: 1. Particle size distribution test The results were obtained by using Malvern 3000 laser particle size analyzer.
[0079] 2. Specific surface area test Obtained by testing with a Microscope Surface Area Analyzer.
[0080] 3. Repose angle test Obtained by testing with a powder properties instrument.
[0081] 4. Morphological Characterization Characterized by SEM scanning electron microscope.
[0082] The test results are shown in Table 1.
[0083] Table 1
[0084] The aluminum oxide particles obtained in the above examples and comparative examples are prepared into slurries, and the slurries are coated on the cut base films, respectively, and dried to obtain diaphragm samples. The slurry preparation and slurry coating film forming method are as follows: (1) Take 350g of porous alumina powder and 650g of deionized water and stir for 10 minutes; (2) Add 10.5 g of dispersant SF8 and continue stirring for 10 min; (3) Add 5.25 g of emulsifier lauryl alcohol polyoxyethylene ether and continue stirring for 10 min; (4) Add 17.5 g of acrylic emulsion BM900-B and continue stirring for 30 min to obtain a coating slurry; (5) The slurry was coated on the surface of the PE diaphragm on an online rod coater and dried in a forced air oven at 40°C for 10 min to obtain a coated diaphragm.
[0085] The base film is a 9 μm thick PE film purchased from Suzhou Jieli New Energy Materials Co., Ltd. The dispersant is SF8 purchased from San Nopco, Japan The binder is BM900-B purchased from Zeon, Japan Lauryl alcohol polyoxyethylene ether was purchased from Nantong Haian Chemical.
[0086] The viscosity of the slurry was measured, and the diaphragm was weighed, the thickness, heat shrinkage, water content, and number of bumps were measured, and the thickness uniformity and coating surface density of the diaphragm were calculated.
[0087] The specific testing methods are as follows: 1. Thickness uniformity The membrane was cut into 20×50cm membranes, and 6 points were taken on the membrane in an equilateral triangle with a side length of 10cm, and three equilateral triangles were taken at different positions on the membrane; considering that the coating was not produced on the equipment, the thickness of the coating fluctuated greatly on both sides in the horizontal direction, so only two points far from the edge were selected in the horizontal direction, a total of 6 points, and the square root value δ of the sum of the squares of the difference between the data points and the mean point was counted and calculated. The specific calculation formula is as follows: δ = ((S1-S 均 ) 2 + (S2-S 均 ) 2 ……(S6-S 均 ) 2 ) 1 / 2 The thickness of the diaphragm and the base film was measured using a German Mahr thickness tester.
[0088] 2. Thermal shrinkage measurement Measured according to 6.6.2 of standard GB / T36363-2018.
[0089] 3. Moisture content measurement The moisture content of the membrane was measured using a Karl Fischer titrator.
[0090] 4. Viscosity measurement It was measured using a NJD-5 rotational viscometer.
[0091] 5. Bump count detection The membrane was cut into 20×50 cm membranes, placed under light, and observed from the back to count the number of black spots.
[0092] The test results are shown in Table 2.
[0093] Table 2
[0094] The measured values of the coating thickness used to calculate the δ value are shown in Table 3: Table 3
[0095] As can be seen from the above table, the particle size D50 and repose angle of the porous alumina with a specific morphology provided by this solution can be controlled within the range of 36°~38.5°. The structural consistency of the alumina is high, its particle size distribution is uniform, the apparent density and specific surface area are also low, and the viscosity of the slurry formed by it is also low. The dispersion of alumina in the slurry is excellent, and the fluidity of the slurry is good. The alumina particles in the diaphragm coating formed by the slurry coating formed by the porous alumina are also evenly distributed, the surface density of the diaphragm coating is low, the thermal shrinkage rate is lower, and the uniformity of the membrane surface thickness is also significantly optimized; there are very few or almost no convex points on the membrane surface.
[0096] In addition, for thin coatings (coatings with a thickness of no more than 2 μm), when alumina with a narrower particle size distribution, a lower particle size D50, and a repose angle in the range of 38.1°~38.5° is used, the coating formed can more significantly improve the shrinkage rate of the diaphragm and its apparent performance is also better.
[0097] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A porous alumina, characterized in that: The porous alumina is an alumina particle having a plurality of mesopores on the surface and / or inside of the particle; and the alumina particle is a quadrangular prism crystal having a thickness not less than 20% of the length of the bottom side; and the cumulative particle size D50 of 50% of the particles on the small particle size side in the cumulative particle size distribution is 0.3-2 μm; The repose angle of the porous alumina is 36.0°~38.5°.
2. The porous alumina according to claim 1, characterized in that: The angle of repose of the porous alumina is 38.1° to 38.5°; and / or The maximum particle size D of the porous alumina max Not higher than 4μm.
3. The porous alumina according to claim 1 or 2, characterized in that: The particle size distribution of the porous alumina satisfies the following formula: SPAN1=D99 / D50<2.5; SPAN2=(D90-D50) / D10<1.
5.
4. The porous alumina according to claim 1 or 2, characterized in that: The cumulative particle size D50 of 50% of particles on the small particle size side in the cumulative particle size distribution of the porous alumina is 0.4 to 1.2 μm.
5. The porous alumina according to claim 4, characterized in that: Its particle size distribution satisfies the following formula: SPAN1=D99 / D50<2.0; SPAN2=(D90-D50) / D10<1.
2.
6. The porous alumina according to claim 4, characterized in that The maximum particle size D of porous alumina max Not higher than 2μm.
7. The porous alumina according to claim 1, characterized in that: The specific surface area of the porous alumina is 5 to 50 m 2 / g within this range; The apparent density of the porous alumina is 2-3 g / cm 3 .
8. The porous alumina according to claim 1, characterized in that The pore volume of the porous alumina is 0.01-0.4 cm 3 / g; The particles in the porous alumina powder are at least one of the θ phase, δ phase, γ phase, and α phase, or at least one of the η phase, κ phase, χ phase, and ρ phase.
9. A battery separator, characterized in that: The battery separator comprises a substrate and a coating formed on at least one side of the substrate, wherein the porous alumina according to any one of claims 1 to 8 is distributed in the coating.
10. The battery separator according to claim 9, characterized in that: The thickness uniformity δ of the coating is not higher than 0.3; The test method for thickness uniformity is: Take 6 points on the surface array of the base film with coating and obtain the thickness S of the coating at each point. n , where n is the number of the measurement point, which is a natural number in the range of 1 to 6. The average thickness S of the coating is calculated. 均 The square root of the sum of the squares of the coating differences measured at each point is calculated as follows: δ=((S1-S 均 ) 2 +(S2-S 均 ) 2 ……( S6-S 均 ) 2 ) 1 / 2 。 11. The battery separator according to claim 9, characterized in that: The number of convex points on the surface of the coating is not higher than 1 / 100cm 2 ; The testing method of the number of convex points is: The base film with the coating was stretched and placed under light, and the number of black spots was observed from the back and counted.
12. The battery separator according to any one of claims 9 to 11, characterized in that: The coating thickness in the battery separator is 1-5 μm, and the proportion of porous aluminum oxide in the coating is 90%-99% by mass.
13. A battery, characterized in that: A battery separator comprising the battery separator according to any one of claims 9 to 12.
14. An electrical device, characterized in that: Comprising the battery of claim 13.
Citation Information
Patent Citations
Easily dispersed aluminum oxide for ceramic membrane of lithium battery and preparation method thereof
CN109516782A
Nano aluminum oxide diaphragm coating and preparation method thereof
CN114512764A
Lithium ion battery ceramic coating slurry, coating diaphragm and preparation method thereof
CN116283346A
Alumina and slurry containing the same, and alumina porous film using the same, laminated separator, nonaqueous electrolyte secondary battery and method for manufacturing nonaqueous electrolyte secondary battery
US20180351147A1
Cited By
Porous aluminum oxide powder for lithium-ion battery and preparation method therefor, battery separator, battery, and electric device
WO2026091476A1