Slow-release coating liquid, slow-release film and application of slow-release film in preparation of coated slow-release fertilizer
Through the combination of oxalamide, isocyanate and soybean oil, a sustained-release envelope solution is prepared and sprayed on the surface of the fertilizer, which solves the problems of poor sustained-release effect and difficulty in degradation of existing sustained-release envelope materials, and realizes the ultra-long-term nutrients of the fertilizer Release and environmentally friendly soil use.
Patent Information
- Application Number
- CN202410943987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-29
AI Technical Summary
The existing sustained-release coating materials have poor sustained-release effect and are difficult to degrade, resulting in soil pollution problems.
The sustained-release envelope solution is prepared by mixing oxalamide, isocyanate and soybean oil in a specific proportion. The sustained-release composite film is prepared by casting or spraying method, and sprayed on the surface of fertilizer particles to form a enveloped sustained-release fertilizer.
It significantly extends the nutrient release time of fertilizer, improves the utilization rate of fertilizer, and avoids soil pollution through the ease of oxalamide, while enhancing the degradation ability of the envelope material.
Smart Images

Figure CN119039076A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of slow-release coating materials, and in particular relates to a slow-release coating liquid, a slow-release film and applications in preparing coated slow-release fertilizers. Background Art
[0002] At present, the commonly used slow-release fertilizers are divided into mixed slow-release fertilizers and coated slow-release fertilizers. Mixed slow-release fertilizers are made by adding slow-release low-water-soluble substances to the fertilizers during the production process to reduce the water solubility of the fertilizers, thereby enhancing the release effect of the fertilizers. Coated slow-release fertilizers are made by coating the surface of fertilizer particles with a very thin layer of hydrophobic substances to make coated fertilizers. Water can enter the porous semi-permeable membrane, and the dissolved nutrients diffuse outside the membrane to continuously supply crops.
[0003] Among the slow-release fertilizers on the market today, the most studied and most diverse type is the coated slow-release fertilizer, which accounts for more than 95% of the slow-release fertilizers. Generally, ordinary fertilizer particles are used as the core, and a layer or even multiple layers of low-water-soluble inorganic or organic matter are coated on the surface by a special process to achieve the purpose of reducing the nutrient dissolution rate. The coating materials are mainly: 1. Inorganic coating materials (sulfur, silicate, gypsum, phosphate, etc.). The biggest advantage of inorganic coating materials is that they have a wide range of sources, but the characteristics of inorganic materials themselves determine that the slow-release effect of their coated products is not good. 2. Organic coating materials (natural polymer materials, such as natural rubber, shellac, cellulose, lignin, starch, etc.; synthetic polymer materials, such as alkyd resins, polyurethanes, thermoplastic resins, etc.; semi-synthetic polymer materials): This type of coated fertilizer is currently the fastest-growing slow-release fertilizer with the best slow / controlled release performance.
[0004] The Chinese patent application document with publication number CN105295122A discloses a method for preparing an environmentally friendly slow-release fertilizer coating material, comprising the following steps: taking natural skim latex for pretreatment, taking cassava starch to obtain modified starch for standby use; adding the modified starch to the natural skim latex and quickly mixing it, and then adding a cross-linking agent and a short-chain starch activator to react to obtain a starch-grafted modified natural skim latex emulsion, which is an environmentally friendly slow-release fertilizer coating material. The present invention adopts the pre-activated short-chain starch emulsion grafting technology, which has a simple process and a stable reaction. The obtained slow-release fertilizer coating material can not only adjust the slow-release property of the fertilizer, but also the coating has good toughness and soil degradation. However, the slow-release effect of the slow-release coating material is poor, so it needs to be further improved. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to solve the problems of poor sustained-release effect, difficult degradation of the coating material, and secondary pollution of the soil by the residual organic polymer shell in the existing sustained-release coating material.
[0006] The present invention solves the above technical problems through the following technical means:
[0007] The first aspect of the present invention provides a sustained-release coating solution, which is obtained by mixing oxalamide, isocyanate and soybean oil in a mass ratio of (3-9):(0.5-3):(0.4-2.5); the isocyanate is polyphenyl polymethylene polyisocyanate (PAPI).
[0008] Preferably, the powder fineness of the oxamide is 100-200 mesh.
[0009] The second aspect of the present invention provides a sustained-release composite film made from the above-mentioned sustained-release coating solution.
[0010] Preferably, the sustained-release composite film is prepared by a casting method or a spraying method.
[0011] The third aspect of the present invention provides the use of the above slow-release coating solution in the preparation of coated slow-release fertilizers.
[0012] A fourth aspect of the present invention provides a coated slow-release fertilizer, which is obtained by spraying the above-mentioned slow-release coating liquid on the surface of fertilizer particles.
[0013] Preferably, the mass ratio of the fertilizer particles to the slow-release coating liquid is (88-94):(6-12).
[0014] Preferably, the fertilizer is urea or compound fertilizer.
[0015] Preferably, the spraying temperature is 70-80° C., and the spraying pressure is 8-10 MPa.
[0016] Preferably, the number of sprayed layers is one or more layers.
[0017] The advantages of the present invention are:
[0018] (1) Compared with common coating materials, the slow-release coating material produced by the method of the present invention has a stronger function of preventing nutrient release. When used in slow-release fertilizers, the fertilizers can have an ultra-long nutrient release time, thus meeting the nutrient needs of crops in the middle and late stages of growth. At the same time, compared with traditional coating materials, the fertilizer of the present invention is different in that the coating material of the present invention itself can be used as one of the nitrogen release sources to provide nutrients for crops.
[0019] (2) The present invention uses oxalamide as the main component of the coating material. Oxalamide is a high-nitrogen, low-water-soluble chemical material with the characteristics of high nitrogen content, non-toxic and tasteless, slightly soluble in water, and stable physical and chemical properties. Oxalamide raw materials are widely available. Due to its good water retention, it is wrapped on the outer surface of the fertilizer and has good slow-release properties, which can improve the utilization rate of the fertilizer. At the same time, oxalamide itself has a very high nitrogen content and can be used as a nitrogen-containing fertilizer. It is absorbed and utilized by plants, is easily degraded, and will not leave harmful substances in the soil. It is green, environmentally friendly, and pollution-free.
[0020] (3) PAPI and soybean oil are used together as raw materials to produce polyurethane. Polyurethane is a common coating material for coated fertilizers. It has the characteristics of wear resistance, water resistance, and excellent mechanical properties. However, it is difficult to degrade in the natural environment. When used in combination with oxalamide, it can enhance the performance of the fertilizer and improve its degradation ability while maintaining good slow-release performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a comparison chart of the cumulative dissolution rates of the coated slow-release fertilizers of Examples 6-8 of the present invention at different leaching times;
[0022] Figure 2 This is a comparison chart of the cumulative dissolution rates of the coated slow-release fertilizers of Examples 6, 9 and 10 of the present invention at different leaching times;
[0023] Figure 3 It is a comparison chart of the cumulative dissolution rate of the coated slow-release fertilizers of Example 6 of the present invention and Comparative Examples 1-2 at different leaching times;
[0024] Figure 4 It is a comparison chart of the mass loss rates of Examples 1-3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] A sustained-release coating liquid is prepared by mixing 6g of oxalamide, 1.64g of polyphenyl polymethylene polyisocyanate (PAPI) and 1.36g of soybean oil; wherein the fineness of the oxalamide powder is 100-200 meshes.
[0028] The sustained-release coating liquid of this embodiment is used to prepare a sustained-release composite film by a casting method, which includes the following steps: PAPI, soybean oil and oxalamide are mixed and stirred evenly in the above proportions, poured evenly on a flat template to form a film-like product with uniform thickness, dried and formed at 70-80°C, and then peeled off to obtain a composite film material.
[0029] Embodiment 2:
[0030] The difference between this embodiment and embodiment 1 is that the amount of oxamide used is 3 g, and the other steps are the same as those in embodiment 1.
[0031] Embodiment 3:
[0032] The difference between this embodiment and embodiment 1 is that the amount of oxamide used is 9 g, and the other steps are the same as those in embodiment 1.
[0033] Embodiment 4:
[0034] The difference between this embodiment and embodiment 1 is that the amount of PAPI used is 0.55 g, the amount of soybean oil used is 0.45 g, and the other steps are the same as those in embodiment 1.
[0035] Embodiment 5:
[0036] The difference between this embodiment and embodiment 1 is that the amount of PAPI used is 2.73 g, the amount of soybean oil used is 2.27 g, and the other steps are the same as those in embodiment 1.
[0037] Embodiment 6:
[0038] A coated slow-release fertilizer is prepared from the slow-release coating solution of Example 1 and 91 g of common urea. The preparation method comprises the following steps:
[0039] (1) Urea slurry is granulated through a fluidized bed to produce large urea particles.
[0040] (2) Add a mixed solution of oxalamide, PAPI and soybean oil into a spraying device and spray it evenly on the surface of large urea particles to produce a nitrogen-containing chemical material coated fertilizer.
[0041] The spraying temperature is 70-80°C, the spraying pressure is 8-10MPa, and a small amount of spraying is performed and then a second spraying is performed after solidification. This process is repeated several times until the surface of the urea particles is completely covered with the slow-release coating liquid.
[0042] The coated slow-release fertilizer obtained in this example and common urea (blank control CK) were subjected to a reverse sand column leaching experiment, and the method was as follows: 100 g of glass beads were sequentially loaded into the leaching device, and then equal amounts of coated fertilizer and common urea were spread on the glass beads in each leaching tube, and then covered with 40 g of dry glass beads, and water was added at a frequency of 20 ml / 3 min for reverse leaching. Sampling was performed once every 20 ml, and the urea content in the water sample was determined, and the dissolution rate was calculated. The calculation formula is:
[0043] Qn=Wn / W0*100%
[0044] Q=∑Wn / W0*100%
[0045] Wherein, Wn is the single dissolution amount (g), W0 is the initial mass, Qn is the single dissolution rate, and Q is the cumulative dissolution rate.
[0046] Embodiment 7:
[0047] The difference between this embodiment and embodiment 6 is that the "sustained-release coating solution of embodiment 1" is changed to "coating solution of embodiment 2", the amount of urea used is changed to 94 g, and the other steps are the same as those of embodiment 6.
[0048] Embodiment 8:
[0049] The difference between this embodiment and embodiment 6 is that the "sustained-release coating solution of embodiment 1" is changed to "coating solution of embodiment 3", the amount of urea used is changed to 88 g, and the other steps are the same as those of embodiment 6.
[0050] Embodiment 9:
[0051] The difference between this embodiment and embodiment 6 is that the "sustained-release coating solution of embodiment 1" is changed to the "coating solution of embodiment 4", the amount of urea used is changed to 93 g, and the other steps are the same as those of embodiment 6.
[0052] Embodiment 10:
[0053] The difference between this embodiment and embodiment 6 is that the "sustained-release coating solution of embodiment 1" is changed to the "coating solution of embodiment 5", the amount of urea used is changed to 89 g, and the other steps are the same as those of embodiment 6.
[0054] Comparative Example 1:
[0055] The difference between the sustained-release coating solution of this comparative example and that of Example 1 is that oxalamide is not added, and the other components and proportions are the same as those of Example 1. The preparation steps of the sustained-release composite film of this comparative example are also the same as those of Example 1.
[0056] The coated slow-release fertilizer of this comparative example is prepared from the slow-release coating liquid of this comparative example and 97g of ordinary urea, and the preparation method and experimental method are the same as those of Example 6.
[0057] Comparative Example 2:
[0058] The difference between the sustained-release coating solution of this comparative example and that of Example 1 is that PAPI and soybean oil are not added, and the amount of urea used is changed to 94 g. The preparation steps of the sustained-release composite film of this comparative example are the same as those of Example 1.
[0059] The coated slow-release fertilizer of this comparative example is prepared from the slow-release coating liquid of this comparative example and 94 g of ordinary urea, and the preparation method and experimental method are the same as those of Example 6.
[0060] The experimental test results of the above examples 6-10 and comparative examples 1-2 are as follows: Figures 1 to 3 As shown:
[0061] like Figure 1 As shown, by comparison, it can be seen that, compared with the blank control group, Examples 6 to 8 significantly reduce the release rate of nutrients, which proves that the slow-release coating liquid of the present invention effectively prevents the rapid release of fertilizer nutrients. By comparing Examples 6, 7 and 8, it can be seen that, while keeping the same amount of curing agent, too much or too little oxalamide addition will affect the slow-release performance of the coated fertilizer.
[0062] from Figure 2 It can be seen that, while keeping the amount of oxamide added unchanged, changing the amount of curing agent has a significant effect on the performance of the fertilizer. When the amount of curing agent used is small, the coating layer thickness is low, the concentration of oxamide in the coating material increases, and the waterproof performance decreases, so the slow-release performance decreases more significantly. When the amount of curing agent used is large, the water barrier performance is improved and the nutrient release rate decreases, but due to the low oxamide content, the rate is higher than Example 6.
[0063] from Figure 3 It can be seen that without the addition of oxamide, the nutrient release rate of the fertilizer increases. If there is no curing agent, using oxamide as the coating material alone will reduce the slow-release performance because the oxamide particles are not tightly connected to each other.
[0064] The mass loss rate of the sustained-release composite films prepared in Examples 1-3 and Comparative Example 1 was experimentally tested:
[0065] At the same time, the film was buried in the soil to a depth of 8 cm and the soil moisture content was maintained at 25%. Samples were taken every 30 days, washed with deionized water, dried and weighed (test results are shown in Table 1). Figure 4 The mass loss rate is calculated as follows:
[0066]
[0067] Where W1 is the mass loss rate in the soil, M1 is the initial mass of the film (g), and M2 is the mass of the film when it is sampled from the soil (g).
[0068] pass Figure 4 It can be seen that when oxamide is not added to the membrane material in Comparative Example 1, the polyurethane material formed by PAPI and soybean oil alone decomposes slowly. However, the decomposition speed of Examples 1 to 3 with oxamide added is significantly improved, and the decomposition speed of the coating material is slow in the early and middle stages, while the decomposition is more thorough in the later stages.
[0069] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A sustained-release coating solution, It is characterized in that The invention is prepared by mixing oxalamide, isocyanate and soybean oil in a mass ratio of (3-9):(0.5-3):(0.4-2.5); the isocyanate is polyphenyl polymethylene polyisocyanate PAPI.
2. The sustained-release coating solution according to claim 1, It is characterized in that The powder fineness of the oxamide is 100-200 meshes.
3. A sustained-release composite film prepared using the sustained-release coating solution according to any one of claims 1 to 2.
4. The sustained-release composite film according to claim 3, It is characterized in that It is prepared by casting or spraying.
5. Use of the slow-release coating liquid according to any one of claims 1 to 2 in the preparation of coated slow-release fertilizers.
6. A coated slow-release fertilizer, It is characterized in that The method is obtained by spraying the slow-release coating liquid according to any one of claims 1 to 2 on the surface of fertilizer particles.
7. The coated slow-release fertilizer according to claim 6, It is characterized in that The mass ratio of the fertilizer particles to the slow-release coating liquid is (88-94):(6-12).
8. The coated slow-release fertilizer according to claim 6, It is characterized in that The number of spraying layers is one or more layers.
9. The coated slow-release fertilizer according to claim 6, It is characterized in that The fertilizer is urea or compound fertilizer.
10. The coated slow-release fertilizer according to claim 6, It is characterized in that The spraying temperature is 70-80° C., and the spraying pressure is 8-10 MPa.
Citation Information
Cited By
Fertilizer for promoting rooting and fruit swelling of crops and preparation method thereof
CN120271382A