Method for preparing hexafluoro-1, 3-butadiene in one step based on continuous hydrogenation coupling strategy

By using activated carbon-based bimetallic supported catalysts to perform continuous hydrogenation reactions in a fixed bed reactor, the preparation process of hexafluoro-1,3-butadiene is simplified, and the problems of many existing process steps and rare raw materials are solved. Efficient and low-cost industrial production has been achieved.

CN119039101APending Publication Date: 2024-11-29HUBEI GUANGGANG GAS ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148137.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing hexafluoro-1,3-butadiene preparation process has long steps, requires a variety of difficult-to-obtain raw materials, and is difficult to achieve continuous production, resulting in low output per unit device and is not suitable for industrial applications.

Method used

Using a continuous hydrogenation coupling strategy, activated carbon-based bimetallic supported catalyst is used in a fixed bed reactor, and 1,1,2-trifluoro-1,2,2- Hexafluoro-1,3-butadiene is prepared by reacting trichloroethane with hydrogen.

Benefits of technology

The process steps are simplified, the raw material cost is reduced, and the efficient preparation of hexafluoro-1,3-butadiene is suitable for industrial production, with low equipment investment and high production safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002805940000031
    Figure BDA0005002805940000031
Patent Text Reader

Abstract

The invention relates to a preparation method of hexafluoro-1, 3-butadiene, in particular to a method for preparing hexafluoro-1, 3-butadiene in one step based on a continuous hydrogenation coupling strategy. The method comprises the following steps: adding a catalyst into a fixed bed reactor, firstly introducing N2 atmosphere to carry out dehydration activation on the catalyst, then raising the temperature to a reaction temperature, introducing a mixed gas of 1, 1, 2-trifluoro-1, 2, 2-trichloroethane and H2, and carrying out a continuous catalytic hydrogenation coupling reaction under normal pressure to obtain hexafluoro-1, 3-butadiene. According to the method, 1, 1, 2-trifluoro-1, 2, 2-trichloroethane is selected as a raw material, hexafluoro-1, 3-butadiene with a high additional value is prepared in one step through a continuous catalytic hydrogenation coupling strategy, the defects that in an existing process, the number of operation steps is large, raw materials are not easy to obtain and the like are effectively overcome, and maximization of economic benefits is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing hexafluoro-1,3-butadiene, and in particular to a method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy. Background Art

[0002] Hexafluorobutadiene, also known as perfluorobutadiene, is mainly used as a plasma etching medium for semiconductor products. Compared with traditional plasma etching gases such as CF4, C2F6, C3F8, c-C4F8 and NF3, hexafluorobutadiene has a faster etching rate, higher etching selectivity and aspect ratio. At present, hexafluorobutadiene has better selectivity than other etching gases and is mainly used for precision etching of critical dimensions with an etching accuracy of 100nm.

[0003] At present, there are many methods for preparing hexafluorobutadiene, mainly including the following process routes: 1) dimerization reaction of 1,2-difluorodichloroethylene and elemental fluorine; 2) addition, coupling and dechlorination of trifluorochloroethylene; 3) polymerization of tetrafluoroethylene; 4) gas phase fluorination of 1,2,3,4-tetrachlorobutane and elemental fluorine; 5) coupling of CF2=CFZnBr; 6) using 1,1,1,2-tetrafluoroethane (HFC-134a) as a raw material to synthesize CF2=CFZnCl and then coupling to obtain hexafluorobutadiene.

[0004] The Chinese invention patent with application number 202310905061.1 discloses a method for preparing hexafluorobutadiene, in which trifluorovinyl phenyl ether is reacted with hydrogen halide to generate halogenated trifluoroethylene, which is then zincated and coupled to obtain hexafluorobutadiene. This process has a long process and requires a large amount of solvent.

[0005] The Chinese invention patent with application number 201610568871.2 discloses a method for preparing hexafluorobutadiene using iodine and chlorine as raw materials, wherein iodine and chlorine react to produce iodine monochloride, iodine monochloride reacts with trifluorochloroethylene in the presence of a metal complex ion solution to produce 1,2-dichloro-2-iodo-1,1,2-trifluoroethane, 1,2-dichloro-2-iodo-1,1,2-trifluoroethane is catalyzed by zinc powder in a metal complex ion solution to produce 1,2,3,4-tetrachloro-1,1,2,3,4,4-hexachlorobutane, and further reacts to produce hexafluoro-1,3-butadiene. This process route requires the use of a metal ion complex solution, which is expensive and not easy to industrialize.

[0006] In summary, the current hexafluorobutadiene preparation process is mainly based on the polymerization and preparation of various halogenated hydrocarbon intermediates, and then the target product hexafluoro-1,3-butadiene is obtained after metal dehalogenation. The raw materials required for these preparation processes are not easy to obtain, and the synthesis route is long, it is difficult to achieve continuous production, the output per unit device is low, and it is not easy to apply industrially. Therefore, how to improve the reaction process and create a new industrial route is the research focus of the synthesis of hexafluorobutadiene. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, which has simple process raw materials and a short synthesis route.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, comprising the following steps: adding a catalyst to a fixed bed reactor, first introducing an N2 atmosphere to remove water and activate the catalyst, and then heating it to a reaction temperature, introducing a mixed gas of 1,1,2-trifluoro-1,2,2-trichloroethane (CF2ClCFCl2, CFC-113) and H2 to carry out a continuous catalytic hydrogenation coupling reaction under normal pressure to obtain hexafluoro-1,3-butadiene.

[0009] The beneficial effects of the present invention are as follows: the present invention selects 1,1,2-trifluoro-1,2,2-trichloroethane with high ozone depletion potential and high greenhouse effect potential as a raw material, and prepares high value-added hexafluoro-1,3-butadiene in one step through a continuous catalytic hydrogenation coupling strategy, effectively overcoming the shortcomings of the existing process such as multiple operating steps and difficulty in obtaining raw materials, thereby achieving maximum economic benefits. DETAILED DESCRIPTION

[0010] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes.

[0011] A method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy comprises the following steps: adding a catalyst into a fixed bed reactor, first introducing an N2 atmosphere to remove water and activate the catalyst, then heating to a reaction temperature, introducing a mixed gas of 1,1,2-trifluoro-1,2,2-trichloroethane and H2 to carry out a continuous catalytic hydrogenation coupling reaction under normal pressure (0.1013 MPa) to obtain hexafluoro-1,3-butadiene.

[0012] The synthesis process of the present invention is shown in formula (1):

[0013]

[0014] From the above description, it can be seen that the beneficial effects of the present invention are: the present invention uses 1,1,2-trifluoro-1,2,2-trichloroethane as a raw material, and prepares hexafluoro-1,3-butadiene in one step through a continuous catalytic hydrogenation coupling strategy, and the operation steps are simple. 1,1,2-Trifluoro-1,2,2-trichloroethane has high ozone depletion potential and high greenhouse effect potential, the raw material is easy to obtain, the processing value is high, it is suitable for industrial production, and the economic benefit is maximized; the reaction process is a gas-solid phase catalytic reaction, the operating pressure is normal pressure, which is convenient for continuous production, the equipment investment is low and the production safety is high.

[0015] Furthermore, the catalyst is an activated carbon-based bimetallic supported catalyst.

[0016] Furthermore, the carrier of the activated carbon-based bimetallic supported catalyst is activated carbon; the first metal in the activated carbon-based bimetallic supported catalyst is any one of Co, Ni and Cu, and the second metal is any one of Ru, Pd and Pt.

[0017] Preferably, the first metal in the activated carbon-based bimetallic supported catalyst is Co or Ni, and the second metal is Pd.

[0018] Furthermore, the loading amount of the first metal in the activated carbon-based bimetallic supported catalyst is 5-40wt%, and the loading amount of the second metal is 0.05-3wt%.

[0019] Preferably, the loading amount of the first metal in the activated carbon-based bimetallic supported catalyst is 5-15 wt %, and the loading amount of the second metal is 0.2-1 wt %.

[0020] The loading amount of the first metal refers to the percentage of the mass of the first metal to the mass of the activated carbon-based bimetallic supported catalyst; the loading amount of the second metal refers to the percentage of the mass of the second metal to the mass of the activated carbon-based bimetallic supported catalyst.

[0021] Furthermore, the preparation method of the activated carbon-based bimetallic supported catalyst includes the following steps: dissolving any one of RuCl3, (NH4)2PdCl4 and (NH4)2PtCl6, and the nitrate hydrate of the first metal in deionized water, then adding activated carbon and stirring, and obtaining the activated carbon-based bimetallic supported catalyst after drying and calcining.

[0022] From the above description, it can be seen that the catalyst used in the preparation method of the present invention is a supported activated carbon-based catalyst, which is simple to prepare, has good repeatability, is easy to scale up production, and is convenient for industrial application.

[0023] Furthermore, when the activated carbon-based bimetallic supported catalyst is a 5Co-0.2Pd / AC catalyst, the preparation method includes the following steps: 12.35 parts by weight of cobalt nitrate hexahydrate and 0.27 parts by weight of (NH4)2PdCl4 are weighed and dissolved in deionized water, and then 50 parts by weight of activated carbon are added, stirred for 6 hours, placed in a forced air drying oven at 120°C for 12 hours, and then calcined at 500°C in a N2 atmosphere for 4 hours to obtain a 5Co-0.2Pd / AC catalyst.

[0024] Furthermore, the particle size of the catalyst is 20 to 40 meshes.

[0025] Furthermore, the space velocity of the continuous catalytic hydrogenation coupling reaction is 150 to 1200 h -1 , the reaction temperature is 400-700°C.

[0026] Furthermore, the space velocity of the continuous catalytic hydrogenation coupling reaction is 300 to 900 h -1 , the reaction temperature is 450-600℃.

[0027] Furthermore, the reaction temperature of water removal activation was 300°C, the N2 flow rate was 50 mL / min, and the water removal activation time was 2 h.

[0028] Furthermore, the feed volume ratio of 1,1,2-trifluoro-1,2,2-trichloroethane to H2 is 1:3 to 1:15.

[0029] Furthermore, the feed volume ratio of 1,1,2-trifluoro-1,2,2-trichloroethane to H2 is 1:6 to 1:10.

[0030] Embodiment 1 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0031] Weigh 12.35 g of cobalt nitrate hexahydrate and 0.27 g of (NH4)2PdCl4 and dissolve them in 100 mL of deionized water, then add 50 g of activated carbon and stir for 6 h. Then, dry the mixture in a forced air drying oven at 120°C for 12 h, and then calcine it at 500°C in a N2 atmosphere for 4 h to obtain a 5Co-0.2Pd / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0032] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 5Co-0.2Pd / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 450 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:6, and the space velocity of catalytic hydrogenation coupling was 300 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 61%, the selectivity of the target product hexafluoro-1,3-butadiene was 87%, and the catalyst remained stable after 30 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0033] Embodiment 2 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0034] Weigh 38 g of copper nitrate trihydrate and 1.54 g of RuCl3 and dissolve them in 100 mL of deionized water, then add 25 g of activated carbon and stir for 6 h. Then, dry the mixture in a forced air drying oven at 120°C for 12 h, and then calcine it at 500°C in a N2 atmosphere for 4 h to obtain a 40Cu-3Ru / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0035] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 40Cu-3Ru / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 700 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:15, and the space velocity of catalytic hydrogenation coupling was 1200 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 54%, the selectivity of the target product hexafluoro-1,3-butadiene was 77%, and the catalyst remained stable after 25 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0036] Embodiment 3 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0037] Weigh 12.35 g of cobalt nitrate hexahydrate and 0.057 g of (NH4)2PtCl6 and dissolve them in 100 mL of deionized water, then add 50 g of activated carbon and stir for 6 hours. Then, dry the mixture in a forced air drying oven at 120°C for 12 hours, and then calcine it at 500°C in a N2 atmosphere for 4 hours to obtain a 5Co-0.05Pt / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0038] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 5Co-0.05Pt / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 400 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:3, and the space velocity of catalytic hydrogenation coupling was 150 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 56%, the selectivity of the target product hexafluoro-1,3-butadiene was 81%, and the catalyst remained stable after 35 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0039] Embodiment 4 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0040] 18.58 g of nickel nitrate hexahydrate and 0.67 g of (NH4)2PdCl4 were weighed and dissolved in 100 mL of deionized water, and then 25 g of activated carbon was added thereto. After stirring for 6 hours, the mixture was placed in a forced air drying oven at 120°C for 12 hours, and then calcined at 500°C in a N2 atmosphere for 4 hours to obtain a 15Ni-1Pd / AC catalyst, which was then granulated into tablets to obtain a catalyst with a particle size of 20 to 40 mesh.

[0041] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of granulated 15Ni-1Pd / AC catalyst was first loaded, and 50 mL / min of N2 was introduced and heated to 300°C for dehydration and activation treatment for 2 h. Then the temperature was raised to 600°C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:10, and the space velocity of catalytic hydrogenation coupling was 900 h -1, the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 62%, the selectivity of the target product hexafluoro-1,3-butadiene was 86%, and the catalyst remained stable after 30 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0042] Embodiment 5 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0043] Weigh 12.34 g of cobalt nitrate hexahydrate and 0.33 g of (NH4)2PdCl4 and dissolve them in 100 mL of deionized water, then add 25 g of activated carbon and stir for 6 hours. Then, dry the mixture in a forced air drying oven at 120°C for 12 hours, and then calcine it at 500°C in a N2 atmosphere for 4 hours to obtain a 10Co-0.5Pd / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0044] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 10Co-0.5Pd / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 500 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:8, and the space velocity of catalytic hydrogenation coupling was 600 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 60%, the selectivity of the target product hexafluoro-1,3-butadiene was 88%, and the catalyst remained stable after 25 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0045] Embodiment 6 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0046] 19.82 g of nickel nitrate hexahydrate and 1.07 g of (NH4)2PdCl4 were weighed and dissolved in 100 mL of deionized water, and then 50 g of activated carbon was added thereto. After stirring for 6 h, the mixture was placed in a forced air drying oven at 120°C for 12 h, and then calcined at 500°C in a N2 atmosphere for 4 h to obtain a 8Ni-0.8Pd / AC catalyst, which was then granulated into tablets to obtain a catalyst with a particle size of 20 to 40 mesh.

[0047] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 8Ni-0.8Pd / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 550 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:9, and the space velocity of catalytic hydrogenation coupling was 700 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 61%, the selectivity of the target product hexafluoro-1,3-butadiene was 86%, and the catalyst remained stable after 40 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0048] Embodiment 7 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0049] Weigh 22.81 g of copper nitrate trihydrate and 0.668 g of (NH4)2PdCl4 and dissolve them in 100 mL of deionized water, then add 50 g of activated carbon and stir for 6 hours. Then, dry the mixture in a forced air drying oven at 120°C for 12 hours, and then calcine it at 500°C in a N2 atmosphere for 4 hours to obtain a 12Cu-0.5Pd / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0050] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 12Cu-0.5Pd / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300°C for dehydration and activation treatment for 2 h. Then the temperature was raised to 600°C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:8, and the space velocity of catalytic hydrogenation coupling was 800 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 60%, the selectivity of the target product hexafluoro-1,3-butadiene was 84%, and the catalyst remained stable after 35 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0051] Embodiment 8 of the present invention is: a method for preparing hexachloro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, the steps are as follows:

[0052] Weigh 24.77 g of nickel nitrate hexahydrate and 0.8 g of (NH4)2PdCl4 and dissolve them in 100 mL of deionized water, then add 50 g of activated carbon and stir for 6 h. Then, dry the mixture in a forced air drying oven at 120°C for 12 h, and then calcine it at 500°C in a N2 atmosphere for 4 h to obtain a 10Ni-0.6Pd / AC catalyst. Then, press the catalyst into tablets with a particle size of 20 to 40 mesh.

[0053] In a fixed bed reactor equipped with an online detection system for GC-MS, 10 mL of 10Ni-0.6Pd / AC catalyst after tableting was first loaded, and 50 mL / min of N2 was introduced and heated to 300 °C for dehydration and activation treatment for 2 h. Then the temperature was raised to 500 °C, N2 was turned off, and the gas was switched to a mixture of CFC-113 and H2 for continuous catalytic hydrogenation coupling reaction. The volume ratio of CFC-113 to H2 was 1:8, and the space velocity of catalytic hydrogenation coupling was 600 h -1 , the reaction pressure was normal pressure. After GC-MS online detection, the conversion rate of CFC-113 was 63%, the selectivity of the target product hexafluoro-1,3-butadiene was 85%, and the catalyst remained stable after 30 hours (i.e., the conversion rate of the reactants and the selectivity of the target product remained basically unchanged).

[0054] In summary, the method for preparing hexachloro-1,3-butadiene in one step based on the continuous hydrogenation coupling strategy provided by the present invention has the following advantages:

[0055] (1) CFC-113 with high ozone depletion potential and high greenhouse effect potential is selected as the raw material. The raw material is cheap and easy to obtain, and is suitable for industrial production.

[0056] (2) High value-added hexafluoro-1,3-butadiene is prepared in one step through a continuous catalytic hydrogenation coupling strategy, which effectively overcomes the disadvantage of the existing process with many operating steps.

[0057] (3) The gas-solid phase catalytic reaction process is adopted, and the operating pressure is normal pressure, which is convenient for continuous production and has a larger production capacity.

[0058] (4) The catalyst preparation method is simple, has good reproducibility, and is convenient for industrial application.

[0059] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the specification of the present invention, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy, characterized in that: The following steps are involved: A catalyst is added to a fixed bed reactor, and N2 atmosphere is first introduced to remove water from the catalyst for activation. The temperature is then raised to the reaction temperature, and a mixed gas of 1,1,2-trifluoro-1,2,2-trichloroethane and H2 is introduced to carry out a continuous catalytic hydrogenation coupling reaction under normal pressure to obtain hexafluoro-1,3-butadiene.

2. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The catalyst is an activated carbon-based bimetallic supported catalyst.

3. The method for preparing hexafluoro-1,3-butadiene in one step based on the continuous hydrogenation coupling strategy according to claim 2, characterized in that: The carrier of the activated carbon-based bimetallic supported catalyst is activated carbon; the first metal in the activated carbon-based bimetallic supported catalyst is any one of Co, Ni and Cu, and the second metal is any one of Ru, Pd and Pt.

4. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 2 or 3, characterized in that: The loading amount of the first metal in the activated carbon-based bimetallic supported catalyst is 5-40 wt %, and the loading amount of the second metal is 0.05-3 wt %.

5. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 2 or 3, characterized in that: The preparation method of the activated carbon-based bimetallic supported catalyst comprises the following steps: dissolving any one of RuCl3, (NH4)2PdCl4 and (NH4)2PtCl6, and a nitrate hydrate of the first metal in deionized water, then adding activated carbon and stirring, and obtaining the activated carbon-based bimetallic supported catalyst after drying and calcining.

6. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The particle size of the catalyst is 20 to 40 meshes.

7. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The space velocity of the continuous catalytic hydrogenation coupling reaction is 150 to 1200 h -1 , the reaction temperature is 400-700°C.

8. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The space velocity of the continuous catalytic hydrogenation coupling reaction is 300 to 900 h -1 , the reaction temperature is 450-600℃.

9. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The volume ratio of the 1,1,2-trifluoro-1,2,2-trichloroethane to H2 is 1:3 to 1:

15.

10. The method for preparing hexafluoro-1,3-butadiene in one step based on a continuous hydrogenation coupling strategy according to claim 1, characterized in that: The feed volume ratio of 1,1,2-trifluoro-1,2,2-trichloroethane to H2 is 1:6 to 1:10.