Fluorescent waterborne polyurethane with anti-counterfeiting function as well as preparation and application of fluorescent waterborne polyurethane

By introducing fluorescent chain extenders such as naphthimide derivatives and anthracene derivatives into aqueous polyurethanes, combining inorganic europium salts and organic potassium salts, fluorescent aqueous polyurethanes with anti-counterfeiting functions are prepared, and the fluorescence intensity of existing aqueous luminescent inks is solved. and the problem of insufficient stability has achieved efficient and environmentally friendly fluorescence performance improvement and versatile applications.

CN119039557AActive Publication Date: 2024-11-29SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411200510.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing aqueous luminescent inks have shortcomings in fluorescence intensity and stability, and the preparation method is not environmentally friendly, which affects its application in the fields of anti-counterfeiting and display.

Method used

Naphthalimide derivatives and anthracene derivatives are used as fluorescent chain extenders, combined with inorganic europium salts and organic potassium salts, and prepared fluorescent aqueous polyurethane with anti-counterfeiting functions through specific stirring and curing steps to form a stable emulsion and achieve fluorescent performance. enhancement and versatility.

Benefits of technology

The prepared fluorescent aqueous polyurethane has good mechanical properties, self-healing efficiency and photoluminescent performance, and has stable fluorescence performance. It is suitable for anti-counterfeiting labels and intelligent displays. It is environmentally friendly in the preparation process and is easy to obtain raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039557A_ABST
    Figure CN119039557A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of fluorescent anti-counterfeiting waterborne polyurethane, and discloses fluorescent waterborne polyurethane with an anti-counterfeiting function as well as preparation and application thereof. According to the preparation method, polycarbonate diol and diisocyanate are taken as raw materials, and two chain extenders including europium ions, potassium ions and naphthalimide derivatives and anthracene derivatives are introduced, so that the fluorescent waterborne polyurethane with an anti-counterfeiting function is obtained. The obtained fluorescent waterborne polyurethane has good mechanical performance, the tensile strength can reach 74.75 + / -3.4 MPa, the pencil hardness reaches 2H, the adhesive force is high, the flexibility is good, and meanwhile the self-repairing efficiency of 83.2% is kept; and the fluorescent material has stable fluorescence performance, has unique responsiveness to high-intensity ultraviolet light, can realize information encryption, and has certain application prospects in the aspects of anti-counterfeit labels, identification platforms, intelligent display and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fluorescent anti-counterfeiting waterborne polyurethane, and particularly relates to fluorescent waterborne polyurethane with anti-counterfeiting function and preparation and application thereof. Background Art

[0002] Waterborne polyurethane coatings have the advantages of good adhesion, good flexibility, cleanliness and pollution-free, and have great development potential. However, the unique water-based environment makes the functionalization of waterborne polyurethane difficult, limiting the application of waterborne polyurethane coatings in more fields. Therefore, realizing the functionalization of waterborne coatings is of great significance to broaden its application areas and promote the development of waterborne polyurethane coatings. Fluorescent inks have many advantages such as bright colors and simple preparation processes, and are widely used in anti-counterfeiting printing, display devices, biological imaging and other fields. Compared with inorganic luminescent inks, waterborne fluorescent inks have the advantages of high luminous efficiency, low carbon, non-toxicity and easy recycling. However, most of the waterborne luminescent inks on the market are prepared by physical blending, which has the disadvantages of reduced fluorescence intensity and poor stability. Therefore, the development of multifunctional waterborne polyurethane inks with intrinsic fluorescence is a research direction with practical significance.

[0003] Chinese invention patent publication CN107746667A discloses a method for preparing a polyurethane luminescent coating, wherein polyurethane, fluorescent powder, curing agent, defoaming agent and thickener are mixed to obtain the polyurethane luminescent coating. However, the color and fluorescent properties of the coating obtained by this method will deteriorate with the increase of the use time. This method is also not environmentally friendly and will cause pollution to the environment. Chinese invention patent publication CN110330622A discloses a fluorescent waterborne polyurethane and a method for preparing the same, wherein the fluorescent group is introduced into the system in the form of a chain extender, and the fluorescent properties can be maintained to a certain extent. Chinese invention patent publication CN116004102A discloses a waterborne polyurethane coating with fluorescent properties and a method for preparing the same, wherein the waterborne polyurethane coating has fluorescent properties, is pollution-free and non-toxic, and is easy to promote and apply. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing fluorescent waterborne polyurethane with anti-counterfeiting function.

[0005] Another object of the present invention is to provide fluorescent waterborne polyurethane with anti-counterfeiting function prepared by the above method.

[0006] Another object of the present invention is to provide an application of the fluorescent waterborne polyurethane with anti-counterfeiting function in anti-counterfeiting labels, identification platforms or smart displays.

[0007] The purpose of the present invention is achieved through the following solutions:

[0008] A method for preparing fluorescent waterborne polyurethane with anti-counterfeiting function comprises the following steps:

[0009] 1) mixing polycarbonate diol and diisocyanate, adding a catalyst, and continuing to stir to obtain a prepolymer;

[0010] 2) adding a fluorescent chain extender and 1,4-butanediol to the prepolymer and stirring to obtain an intermediate product containing a fluorescent group;

[0011] 3) adding a hydrophilic chain extender to the intermediate product containing a fluorescent group and stirring to obtain an intermediate product containing a hydrophilic group;

[0012] 4) adding benzidine to the intermediate product containing a hydrophilic group and stirring;

[0013] 5) adding triethylamine to the solution obtained in step 4) for neutralization;

[0014] 6) Adding an inorganic europium salt, an organic potassium salt and water to the solution obtained in step 5), stirring to obtain an emulsion, and curing to obtain a fluorescent waterborne polyurethane with anti-counterfeiting function.

[0015] In step 1), the polycarbonate diol is at least one of PCDL1000 and PCDL2000.

[0016] In step 1), the diisocyanate is at least one of hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), and toluene diisocyanate (TDI).

[0017] In step 1), the molar ratio of the diisocyanate to the polycarbonate diol is 2 to 3:1.

[0018] Step 1) The catalyst is at least one of stannous octoate, stannous oleate and dibutyltin dilaurate; the usage ratio of the catalyst to polycarbonate diol is 1 drop: 4-6 mmol.

[0019] Step 1) The polycarbonate diol is subjected to a dehydration treatment before mixing and stirring, specifically, the polycarbonate diol is placed in a vacuum and dehydrated at 110-120° C. for 1-3 hours to remove water and other small molecules in the polycarbonate diol for standby use.

[0020] Step 1) The mixing and stirring temperature is 80-90° C., the mixing and stirring time is 0.5-1.5 h, and the continued stirring time is 2.5-4 h.

[0021] The mixing and stirring in step 1) is carried out under N2 or Ar atmosphere.

[0022] Step 2) The fluorescent chain extender is a naphthalene imide derivative BAT and an anthracene derivative ADO, and the structural formula is as follows:

[0023]

[0024] The naphthalene imide derivative is prepared by the following steps:

[0025] The naphthylic anhydride and aminodiol are reacted at 80°C for 12 to 24 hours, the solvent is removed, washed, and dried to obtain an intermediate; the intermediate is reacted with aminoindole in dimethyl sulfoxide at 80°C for 12 to 24 hours, centrifuged, impurities are removed, and dried to obtain a naphthylimide derivative (BAT);

[0026] The anthracene derivative is prepared by the following steps:

[0027] Potassium carbonate, anthracene bromide and alcohol amine are mixed and stirred in dimethyl sulfoxide, reacted at 80° C. for 4 to 5 hours, filtered, impurities removed and dried to obtain a light yellow anthracene derivative (ADO).

[0028] The molar ratio of the fluorescent chain extender in step 2) to 1,4-butanediol and the polycarbonate diol in step 1) is 0.25-4.25:0.25-4.25:50.

[0029] Step 2) The molar ratio of the naphthalene imide derivative to the anthracene derivative in the fluorescent chain extender is 0.25:0.5-4.

[0030] The stirring time in step 2) is 2 to 3 hours.

[0031] Step 3) The hydrophilic chain extender is at least one of 2,2-dihydroxymethylpropionic acid, 2,2-dihydroxymethylbutyric acid, and sodium ethylenediaminesulfonate.

[0032] The molar ratio of the hydrophilic chain extender in step 3) to the diisocyanate in step 1) is 1:10 to 2:5.

[0033] Step 3) The stirring temperature is 70-80° C. and the stirring time is 1.5-2.5 h.

[0034] Step 4) the benzidine is at least one of o-tolidine, m-tolidine and 3,3'-dimethoxybenzidine.

[0035] The molar ratio of the benzidine in step 4) to the diisocyanate in step 1) is 1:10 to 2:5.

[0036] Step 4) The stirring temperature is 40-50° C. and the stirring time is 2.5-3.5 h.

[0037] The molar ratio of the triethylamine in step 5) to the hydrophilic chain extender in step 3) is 1:1.

[0038] Step 5) The neutralization temperature is room temperature; the stirring time of the neutralization is 0.5 to 1 h.

[0039] Step 6) The inorganic europium salt is at least one of europium nitrate, europium carbonate, europium acetate, and europium sulfate.

[0040] Step 6) The organic potassium salt comprises at least one of potassium acetate, potassium propionate, potassium lactate and potassium citrate.

[0041] The molar ratio of the inorganic europium salt and the organic potassium salt in step 6) to the benzidine in step 4) is 0.25:1.25 to 10:20.

[0042] Step 6) The amount of water used is such that the solid content of the emulsion is 35wt% to 40wt%.

[0043] Step 6) The stirring temperature is 25-35° C.; the stirring speed is 1000 r / min-1500 r / min; and the stirring time is 0.5-1 h.

[0044] Step 6) The curing is specifically to coat the emulsion on a substrate and solidify it into a shape or to pour the emulsion into a mold and air-dry it to solidify it.

[0045] The substrate is one of 50# steel plate, epoxy plate, bakelite plate, PC plate, glass plate and acrylic plate.

[0046] The curing conditions for the coating on the substrate are baking at 100-130°C in a blast oven for 0.1-0.5h; the air-drying curing conditions are air-drying at room temperature for 24h-72h, and then baking at 80-100°C in a blast oven for 6-12h.

[0047] The fluorescent waterborne polyurethane with anti-counterfeiting function prepared by the above method.

[0048] The fluorescent water-based polyurethane with anti-counterfeiting function is used in anti-counterfeiting labels, identification platforms or smart displays.

[0049] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0050] 1. The present invention introduces a naphthylimide-based chain extender (BAT) and anthracene-based chain extender (ADO) into a waterborne polyurethane (WPU) to prepare a fluorescent waterborne polyurethane (FWPU) with stable emulsion performance and can be printed on a variety of substrates with simple mixing. The obtained fluorescent waterborne polyurethane has good mechanical properties and excellent self-healing efficiency, and has excellent flexibility and excellent adhesion on a variety of substrates (ISO grade 0). Due to the introduction of cations to construct a non-covalent physical cross-linking network based on double cation-π interactions, the tensile properties of FWPU reach 74.75±3.4MPa, the hardness reaches 2H, and the self-healing efficiency is maintained at 83.2%.

[0051] 2. The present invention introduces naphthalene imide derivatives, anthracene derivatives and europium ions, so that the obtained fluorescent water-based polyurethane has excellent photoluminescence properties. Encrypted information can be input into the polyurethane using high-intensity 254nm ultraviolet light, and double information encryption can be achieved with 365nm information input. It has certain application prospects in anti-counterfeiting labels, identification platforms, smart displays, etc.

[0052] 3. Fluorescence performance and anti-counterfeiting applications of FWPU: FWPU can achieve a variety of colors, and its fluorescence has excellent stability (water resistance, acid and alkali resistance, heat resistance and light resistance), and has a unique responsiveness to high-intensity ultraviolet light. This feature can be used to input information and patterns on FWPU, encrypt information, and use FWPU to prepare information primitives to form an information matrix to express information. In addition, FWPU emulsion only needs to add a small amount of defoamer and thickener to be used as an excellent water-based fluorescent ink, and combined with screen printing technology, it can be printed on a variety of substrates.

[0053] 4. The synthesis conditions of the present invention are mild, the preparation process is simple, and the raw materials are easily available. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 It is the stress-strain curve diagram of each embodiment and comparative example.

[0055] Figure 2 This is a graph showing the fluorescence performance of Example 1 after being placed under pH=7, pH=13, pH=1, and 100°C conditions for 240 hours.

[0056] Figure 3 This is a comparison diagram of Example 1 placed in an open-air natural environment for 15 days under 254nm irradiation.

[0057] Figure 4 It is a schematic diagram of polyurethane information input in Example 1 of dual anti-counterfeiting application and a diagram of different information expressions of polyurethane in Example 1 under the excitation of ultraviolet light of different wavelengths.

[0058] Figure 5 It is a schematic diagram of preparing information elements by utilizing the responsiveness of the polyurethane of Example 1 to long-term irradiation with 254nm ultraviolet light, and a diagram of different information expressions of the matrix composed of the information elements at 365nm and 254nm.

[0059] Figure 6 These are information expression pictures of the polyurethane of Example 1 under visible light, 254nm and 365nm, and display pictures of various pattern information input on the polyurethane of Example 1 using 254nm ultraviolet light.

[0060] Figure 7 It is the carbon nuclear magnetic resonance spectrum of BAT and ADO of the present invention.

[0061] Figure 8 It is the hydrogen nuclear magnetic resonance spectrum of BAT and ADO of the present invention. DETAILED DESCRIPTION

[0062] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0063] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0064] The parts mentioned in the following preparations are all molar parts, wherein "1 part" means "1 mmol".

[0065] Preparation of naphthalene imide derivatives (BAT):

[0066]

[0067] 1) Weigh 30 parts of 4-bromo-1,8-naphthoic anhydride in a single-necked flask, then add 90 parts of 2-amino-1,3-propanediol and 120 mL of ethanol. After reflux heating at 80°C for 12 hours, a rotary evaporator is used to remove excess ethanol. Finally, wash with deionized water three times and vacuum dry at 50°C for 12 hours to obtain a light yellow powder intermediate.

[0068] 2) Weigh 5 parts of the light yellow powder intermediate into a single-necked flask, add 5.1 parts of 3-(2-aminoethyl)indole and dimethyl sulfoxide (10 mL), and reflux at 80°C for 12 hours. After the reaction is completed, pour the solution into 200 mL of deionized water to obtain an orange-red suspension. The suspension is divided into centrifuge tubes, centrifuged at high speed, and the supernatant is poured off to obtain an orange-red solid. The crude product is recrystallized from ethanol 1 to 2 times, dried at 50°C for 6 hours, and ground to obtain an orange-red powder BAT.

[0069] Preparation of anthracene derivatives (ADO):

[0070]

[0071] 123.01 parts of potassium carbonate, 72.9 parts of diethanolamine, 3.61 parts of potassium iodide and 30 mL of DMSO were added to a flask and stirred thoroughly. Then 12.17 parts of 9-(bromomethyl)anthracene were dissolved in 30 mL of DMSO and placed in the original reaction vessel, and 3 to 10 mL of DMSO were added to adjust the reaction rate. The reaction was carried out at 80°C for 4 hours, and the obtained solution was poured into a large amount of water to obtain a suspension with light yellow flocs. The suspension was filtered using a G4 sand core funnel, washed with water, dried, recrystallized with ethanol, and finally dried in a vacuum chamber for 12 hours to obtain light yellow powder ADO.

[0072] Example 1

[0073] A fluorescent waterborne polyurethane with anti-counterfeiting function, the synthesis steps of which are as follows:

[0074] (1) 50 parts of polycarbonate diol (PCDL1000) with a molecular weight of 1000 were evacuated at 120°C, and the water was removed for 2 hours, and then the heating was turned off; after the temperature dropped to 80°C, 105 parts of isophorone diisocyanate (IPDI) were added, mixed and stirred in a N2 atmosphere, and reacted for 1 hour, and then 10 drops of catalyst dibutyltin dilaurate (DBTDL) were added, and the stirring reaction was continued for 3 hours to obtain a prepolymer.

[0075] (2) 3.75 parts of 1,4-butanediol (BDO), 0.25 parts of a naphthyl imide derivative (BAT) and 0.5 parts of anthracene derivative (ADO) were added to the prepolymer obtained in step (1), and a small amount of butanone was added to dilute it. The reaction was continued by stirring for 3 hours to obtain an intermediate product containing a fluorescent group.

[0076] (3) The temperature was lowered to 70° C., and 30 parts of 2,2-bis(hydroxymethyl)butyric acid (DMBA) were added to the reaction solution obtained in step (2), and the reaction was carried out for 1.5 hours to obtain an intermediate product containing a hydrophilic group.

[0077] (4) The temperature was lowered to 50° C. again, 20 parts of m-tolidine (mT) were added, and the reaction was continued for 3 h to obtain an intermediate product containing a hydrophilic group.

[0078] (5) Add 30 parts of triethylamine to the reaction solution obtained in step (4) for neutralization, cool to room temperature, and stir thoroughly for 0.5 h.

[0079] (6) Dissolve 0.25 parts of europium nitrate and 5 parts of potassium acetate in deionized water. After dissolution, add the ion water solution into the system to make the solid content of the emulsion 38wt%. Adjust the speed of the agitator to 1500r / min, stir at high speed for 0.5h to obtain an emulsion; pour the emulsion into a mold, place it at room temperature for 24h, and then place it in a forced air oven at 100°C for 5h to obtain a fluorescent waterborne polyurethane.

[0080] Comparative Example 1

[0081] The difference from Example 1 is that potassium acetate is not added in step (6).

[0082] Comparative Example 2

[0083] The difference from Example 1 is that europium nitrate and potassium acetate are not added in step (6).

[0084] Comparative Example 3

[0085] The difference from Comparative Example 2 is that in step (2), 3.25 parts of 1,4-butanediol (BDO), 0.25 parts of naphthaleneimide derivative (BAT) and 1 part of anthracene derivative (ADO) are added to the prepolymer obtained in step (1).

[0086] Comparative Example 4

[0087] The difference from Comparative Example 2 is that in step (2), 2.25 parts of 1,4-butanediol (BDO), 0.25 parts of a naphthaleneimide derivative (BAT) and 2 parts of anthracene derivative (ADO) are added to the prepolymer obtained in step (1).

[0088] Comparative Example 5

[0089] The difference from Comparative Example 2 is that in step (2), 0.25 parts of 1,4-butanediol (BDO), 0.25 parts of naphthaleneimide derivative (BAT) and 4 parts of anthracene derivative (ADO) are added to the prepolymer obtained in step (1).

[0090] Comparative Example 1 is a fluorescent waterborne polyurethane emulsion without adding an organic potassium salt, and Comparative Examples 2-5 are fluorescent waterborne polyurethane emulsions without adding an inorganic europium salt and an organic potassium salt, and only the ratio of the two fluorescent chain extenders, naphthaleneimide derivative (BAT) and anthracene derivative (ADO), is changed.

[0091] The mechanical properties of the polyurethanes obtained in the above examples and comparative examples were tested, and the results are shown in Table 1.

[0092] Table 1 Mechanical properties of various embodiments and comparative examples

[0093]

[0094] The emulsions obtained in the examples and comparative examples were coated on different substrates respectively and baked in a forced air oven at 120° C. for 0.1 h to obtain fluorescent waterborne polyurethane attached to the substrates. Adhesion grade test was then performed.

[0095] Table 2 Adhesion grades of various embodiments and comparative examples on different substrates

[0096]

[0097] By comparing the polyurethane obtained in Example 1 with the comparative example, the tensile strength and pencil hardness of the polyurethane are greatly improved, indicating that Eu 3+ and K + The introduction of , constructs a non-covalent physical cross-linking network based on dual cation-π interaction. The introduction of cation-π action further increases the intermolecular force, promotes the aggregation of hard segments, and increases the degree of microphase separation, thereby greatly improving the mechanical properties of polyurethane, but the reduction of segment mobility is not conducive to the self-repair of polyurethane, so the self-repair efficiency of polyurethane obtained in Example 1 is lower than that of the comparative example. All polyurethanes obtained in the embodiments and comparative examples have a pencil hardness of more than HB, and the hardness is moderate, and can provide clearly visible lines and patterns on the surfaces of many substrates, which are suitable for drawing, marking and other purposes. By comparing the polyurethanes obtained in comparative examples 2-5, it is found that with the increase in the content of the two fluorescent chain extenders, that is, the increase in rigid side chains, the tensile properties of polyurethane are improved, and the pencil hardness is also improved, indicating that the increase of rigid side chains in the system not only increases the hard segment content of the polymer, but also enhances the interaction between molecular chains, the mobility of the polymer segments decreases, and the polyurethane exhibits better mechanical properties. The flexibility and adhesion of each embodiment and comparative example on various substrates are good, indicating that the introduction of rigid groups and cations has little effect on the flexibility and adhesion of polyurethane.

[0098] The fluorescence performance of the coating of Example 1 was evaluated after being placed under pH=7, pH=13, pH=1, and 100°C for 240 hours and in an open-air natural environment for 15 days. It was found that the fluorescence of the coating did not change significantly. Figure 2 , Figure 3 As shown, it exhibits good water resistance, acid and alkali resistance, heat resistance and light resistance, and has excellent fluorescence stability.

[0099] like Figure 4Through a specific mold (a black template with a hollowed-out part that allows ultraviolet light to pass through, thereby controlling the fixed area of ​​the polyurethane to be "input with information"), different information can be effectively input into the material under 365nm and 254nm ultraviolet light. Under visible light, the polyurethane in the embodiment encrypts the information, making it completely unreadable. Under 254nm ultraviolet light, the information "E" can be effectively read, and then the information "F" can be successfully read under 450nm blue light. The information of the two is combined to finally obtain the effective information "EF", realizing the double encryption of information.

[0100] The encrypted information input by 254nm ultraviolet light is highly read-only. The information cannot be read under 365nm ultraviolet light, 450nm blue light, and visible light. Only under 254nm ultraviolet light can the information be clearly output. Figure 5 In (a), two information primitives are prepared, one of which is the polyurethane of Example 1 without any treatment, and the other is irradiated with 254nm ultraviolet light to prepare information primitives. The two information primitives are combined into a certain information matrix to complete the input and composition of information. The two information primitives are indistinguishable under the irradiation of a conventional anti-counterfeiting 365nm ultraviolet flashlight, but under the irradiation of 254nm ultraviolet light, they can be successfully decrypted - the output information "L" and "H", as shown in FIG. Figure 5 (b). Using this feature combined Figure 4 The specific mold mentioned in (a) can complete more complex pattern input, such as Figure 6 In (a), the dolphin pattern can be input into the polyurethane, and Figure 6 (b) shows the polyurethane samples of Example 1 with more expression patterns.

[0101] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing fluorescent waterborne polyurethane with anti-counterfeiting function, characterized in that: The following steps are involved: 1) mixing polycarbonate diol and diisocyanate, adding a catalyst, and continuing to stir to obtain a prepolymer; 2) adding a fluorescent chain extender and 1,4-butanediol to the prepolymer and stirring to obtain an intermediate product containing a fluorescent group; 3) adding a hydrophilic chain extender to the intermediate product containing a fluorescent group and stirring to obtain an intermediate product containing a hydrophilic group; 4) adding benzidine to the intermediate product containing a hydrophilic group and stirring; 5) adding triethylamine to the solution obtained in step 4) for neutralization; 6) Adding an inorganic europium salt, an organic potassium salt and water to the solution obtained in step 5), stirring to obtain an emulsion, and curing to obtain a fluorescent waterborne polyurethane with anti-counterfeiting function.

2. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: Step 1) The polycarbonate diol is at least one of PCDL1000 and PCDL2000; Step 1) the diisocyanate is at least one of hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate and toluene diisocyanate; Step 1) The molar ratio of the diisocyanate to the polycarbonate diol is 2 to 3:1; Step 1) The catalyst is at least one of stannous octoate, stannous oleate and dibutyltin dilaurate; the usage ratio of the catalyst to polycarbonate diol is 1 drop: 4-6 mmol.

3. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: Step 1) The polycarbonate diol is subjected to a dehydration treatment before mixing and stirring, specifically, the polycarbonate diol is placed in a vacuum and dehydrated at 110-120° C. for 1-3 hours to remove water and other small molecules in the polycarbonate diol for standby use; Step 1) The mixing and stirring temperature is 80-90°C, the mixing and stirring time is 0.5-1.5h, and the continued stirring time is 2.5-4h; The mixing and stirring in step 1) is carried out under N2 or Ar atmosphere.

4. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: Step 2) The fluorescent chain extender is a naphthalene imide derivative BAT and an anthracene derivative ADO, and the structural formula is as follows:

5. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 4, characterized in that: The naphthalene imide derivative is prepared by the following steps: The naphthylic anhydride and aminodiol are reacted at 80°C for 12 to 24 hours, the solvent is removed, washed, and dried to obtain an intermediate; the intermediate is reacted with aminoindole in dimethyl sulfoxide at 80°C for 12 to 24 hours, centrifuged, impurities are removed, and dried to obtain a naphthylimide derivative; The anthracene derivative is prepared by the following steps: Potassium carbonate, anthracene bromide and alcohol amine are mixed and stirred in dimethyl sulfoxide, reacted at 80°C for 4-5 hours, filtered, impurities removed and dried to obtain a light yellow anthracene derivative.

6. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: The molar ratio of the fluorescent chain extender in step 2) to 1,4-butanediol and the polycarbonate diol in step 1) is 0.25-4.25:0.25-4.25:50; Step 2) the molar ratio of the naphthalimide derivative to the anthracene derivative in the fluorescent chain extender is 0.25:0.5-4; The stirring time in step 2) is 2 to 3 hours.

7. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: Step 3) the hydrophilic chain extender is at least one of 2,2-dimethylol propionic acid, 2,2-dimethylol butyric acid, and sodium ethylenediamine sulfonate; The molar ratio of the hydrophilic chain extender in step 3) to the diisocyanate in step 1) is 1:10 to 2:5; Step 3) the stirring temperature is 70-80°C and the stirring time is 1.5-2.5h; Step 4) the benzidine is at least one of o-tolidine, m-tolidine and 3,3'-dimethoxybenzidine; The molar ratio of the benzidine in step 4) to the diisocyanate in step 1) is 1:10 to 2:5; Step 4) The stirring temperature is 40-50° C. and the stirring time is 2.5-3.5 h.

8. The method for preparing the fluorescent waterborne polyurethane with anti-counterfeiting function according to claim 1, characterized in that: The molar ratio of the triethylamine in step 5) to the hydrophilic chain extender in step 3) is 1:1; Step 5) The neutralization temperature is room temperature; the stirring time of the neutralization is 0.5 to 1 h; Step 6) the inorganic europium salt is at least one of europium nitrate, europium carbonate, europium acetate, and europium sulfate; Step 6) the organic potassium salt comprises at least one of potassium acetate, potassium propionate, potassium lactate and potassium citrate; The molar ratio of the inorganic europium salt and the organic potassium salt in step 6) to the benzidine in step 4) is 0.25:1.25 to 10:20; Step 6) The amount of water used is such that the solid content of the emulsion is 35wt% to 40wt%; Step 6) the stirring temperature is 25-35°C; the stirring time is 0.5-1h; Step 6) The curing is specifically to coat the emulsion on a substrate and solidify it into a shape or to pour the emulsion into a mold and air-dry it to solidify it.

9. Fluorescent waterborne polyurethane with anti-counterfeiting function prepared by the method according to any one of claims 1 to 8.

10. Use of the fluorescent waterborne polyurethane with anti-counterfeiting function as claimed in claim 9 in anti-counterfeiting labels, identification platforms or smart displays.

Citation Information

Patent Citations

  • Fluorescent dye, preparation method and application thereof

    CN102115610A

  • Fluorescent waterborne polyurethane based on chromophore in dihydric alcohol and preparation method thereof

    CN103254396A

  • Fluorochrome monomer, copolymeric fluorescent polyurethane emulsion and fluorescent polyurethane-acrylic ester copolymer emulsion as well as preparation methods thereof

    CN105601567A

  • Rare earth metal coordination-modified waterborne polyurethane luminous resin and preparation method thereof

    CN107814895A

  • Transparent waterborne polyurethane emulsion based on cation-pi interaction as well as preparation and application of transparent waterborne polyurethane emulsion

    CN117700666A