Method for one-step preparation of solvent-free UV moisture dual-curing organosilicon conformal coating resin

This method for preparing solvent-free UV moisture dual-curing silicone conformal coating resin in one step solves the problems of complex processes and residue treatment in existing technologies, and realizes the preparation of low viscosity, environmentally friendly and high performance circuit board coatings, which are suitable for the protection of high-end electronic devices.

CN119039589APending Publication Date: 2024-11-29ZHEJIANG XINAN CHEM IND GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411260846.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing methods for preparing solvent-free UV moisture dual-curing silicone conformal coating resins are complex, the residual acrylic acid in the second step of the reaction is difficult to remove, and the generated alkyl hydroxyl groups increase viscosity, which cannot meet the protection requirements of increasingly sophisticated circuit boards.

Method used

A one-step preparation method is adopted, which involves polycondensation and de-alcoholization reaction of γ-acryloyloxypropyltrimethoxysilane, hydroxyl-terminated polysiloxane and catalyst, followed by vacuum degassing to obtain solvent-free UV moisture dual-curing organosilicon conformal coating resin, avoiding the complicated two-step process and residue treatment.

Benefits of technology

It achieves safe and reliable environmentally friendly preparation, has low resin viscosity, is easy to apply, and possesses excellent mechanical properties, electrical insulation properties, and bonding strength, making it suitable for high-end circuit board protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039589A_ABST
    Figure CN119039589A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing solvent-free UV (ultraviolet) moisture dual-curing organosilicone conformal coating resin in one step, which comprises the following steps: carrying out polycondensation dealcoholization reaction on gamma-acryloyloxy propyl trimethoxy silane, double-terminal hydroxyl polysiloxane and a catalyst, and carrying out vacuum defoaming and purification to obtain the UV moisture dual-curing organosilicone conformal coating resin. The room temperature viscosity of the prepared conformal coating resin is 1t; compared with a conventional solvent-free UV moisture dual-curing aliphatic polyester urethane acrylate system, the UV moisture dual-curing aliphatic polyester urethane acrylate system has the advantages of longer working life in the storage process due to no isocyanate group, safety and controllability, few byproducts, narrow average molecular weight distribution of the generated product, small viscosity, and good stability. The problem of troublesome post-treatment of residual raw materials is avoided, and the excessive alkoxy silane coupling agent can be directly used as an adhesion promoter for enhancing adhesion with a base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functionalized graft synthesis of organic silicon polymers, relates to the preparation of conformal coating resins, and in particular to a one-step method for preparing solvent-free UV moisture dual-curing organic silicon conformal coating resins. Background Art

[0002] Conformal coating is a special functional PCB protective coating. With the development of autonomous driving technology, the integration of controller PCB components is getting higher and higher, the design is getting more and more sophisticated, and the specifications are getting smaller and smaller, which puts more stringent requirements on the performance of the coating, such as high humidity and heat environment protection, mechanical properties and electrical properties.

[0003] UV curing is particularly suitable for thin coating systems in assembly line processes. Its rapid shaping and high cross-linking sealing strength not only have the advantages of anti-sagging and improved silicone permeability, but also improve surface properties such as gloss, surface drying time and surface drying hardness. Combined with the excellent flexibility of silicone to eliminate the stress resistance caused by curing shrinkage on precision components and improve the electrical properties of insulation and leakage short circuit, as well as flame retardancy and good circuit board wettability and low surface tension to prevent moisture, dust and corrosive gas adsorption, UV curing silicone conformal coating resin is a heat dissipation thin coating option that is more suitable for fast assembly line operations. However, there will be shadow areas on the side of the circuit board components that are not exposed to UV light, which will result in the coating not being fully cured. At the same time, based on environmental protection requirements and to solve the problem of decreased adhesion caused by full UV curing shrinkage, it is necessary to develop a preparation method for solvent-free UV moisture dual-curing silicone conformal coating resin.

[0004] There are methods for preparing solvent-free UV moisture dual-curing silicone conformal coating resins on the market, mainly: 1) using a two-step preparation process, but the residual acrylic acid in the second step is difficult to remove. This process uses alkoxysilane two-step moisture curing to generate silicon-oxygen-silicon bonds to improve the spatial strength of the coating and the bonding strength with the substrate PCB. The bonding strength with the glass fiber substrate PCB increases with the extension of moisture curing time, and it is not necessary to add radiation-curing alkoxysilane coupling agents to the coating formula.

[0005] 2) Conventional solvent-free UV moisture dual-curing silicone segmented polyurethane acrylate process. This process uses segmented silicone to improve the flexibility of the coating to eliminate the high and low temperature impact stress resistance generated by the passage of current. The adhesion to the substrate PCB is improved through the urethane bond in the segmented polyurethane and the urea bond in the polyurea generated by the two-step moisture curing. Since the bonding strength to the glass fiber substrate PCB is not enough, additional radiation-cured alkoxy silane coupling agents are needed to be added to the coating formula to enhance the bonding strength of the substrate.

[0006] In addition, from the perspective of system stability, the two-step preparation process has much better storage stability than the latter due to the absence of isocyanate groups that are highly sensitive to water vapor.

[0007] In view of the two-step method for preparing solvent-free UV moisture dual-curing silicone conformal coating resin, firstly, the process is complicated and the residual acrylic acid in the second step reaction is difficult to post-process; secondly, the second step of ring-opening grafting will generate alkyl hydroxyl groups that increase the viscosity of the system. In order to meet the increasingly sophisticated environmental protection, mechanical and electrical performance requirements of circuit boards, while trying to control the average molecular weight and viscosity of the silicone conformal coating resin to improve the wetting and penetration of semiconductor components, it is necessary to develop a safe, reliable and easy to post-process one-step method for preparing solvent-free UV moisture dual-curing silicone conformal coating resin. Summary of the invention

[0008] The present invention solves the problem that the two-step method for preparing solvent-free UV moisture dual-curing organic silicon conformal coating resin is complicated, the residual acrylic acid in the second step reaction is difficult to post-process, and the alkyl hydroxyl group that increases the viscosity is generated, thereby providing a one-step method for preparing solvent-free UV moisture dual-curing organic silicon conformal coating resin. The method of the present invention is safe and reliable, easy to operate, and the room temperature viscosity of the prepared resin is less than 100 cP, environmentally friendly and solvent-free, and the coating construction is convenient. It has many advantages of organic silicon, such as excellent mechanical properties that can completely eliminate the stress resistance caused by the high and low temperature impact generated before and after the current of the components on the circuit board passes, excellent electrical insulation performance to prevent leakage short circuit, excellent wetting penetration bonding strength with glass fiber substrate circuit board, and high crosslinking density and strength of UV resin and gloss of the sealing layer. The organic silicon conformal coating resin prepared by the present invention can be used in the circuit board protection fields such as high-end PCB industrial electronics, automotive electronics, consumer electronics, aerospace electronics and military electronics.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] The present invention provides a one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, the method comprising the following steps:

[0011] 1) Prepare raw materials: γ-acryloxypropyltrimethoxysilane, hydroxyl-terminated polysiloxane, catalyst, partial radiation-curable defoamer and inhibitor;

[0012] 2) adding γ-acryloxypropyltrimethoxysilane, hydroxyl-terminated polysiloxane and a catalyst into a reaction container, heating and stirring to a first temperature, monitoring changes in the hydroxyl value in the reaction system during the reaction, and adding an inhibitor and a partially radiation-curable defoamer when it is monitored that the silanol groups in the reaction system are completely consumed, heating to a second temperature and stirring evenly, and evacuating until degassing is complete to obtain a solvent-free UV moisture dual-curing silicone conformal coating resin.

[0013] As a preferred embodiment of the present invention, the raw materials include, by weight: 2.5 to 4 parts of γ-acryloxypropyltrimethoxysilane, 1 part of hydroxyl-terminated polysiloxane, 0.01 to 0.1 parts of catalyst, 0.1 to 0.2 parts of partial radiation curing defoamer and 0.005 to 0.02 parts of polymerization inhibitor. The radiation curing defoamer is preferably: one or a combination of two or more of Evonik Deco 270, 2300, 2200N, 2250, and 2500.

[0014] As a preferred embodiment of the present invention, in step 2), the first temperature is 30°C to 60°C, and the reaction time is 2h to 8h.

[0015] As a preferred embodiment of the present invention, in step 2), the sampling time interval is 1 hour, and the sampling times are 2 to 6 times.

[0016] Preferably, the sampling times are 3 to 4 times.

[0017] As a preferred embodiment of the present invention, the reaction time is 4 h to 5 h.

[0018] As a preferred solution of the present invention, the vacuum degree is -80 kPa to -90 kPa.

[0019] Preferably, the vacuum degree is -80 kPa to -84 kPa.

[0020] As a preferred embodiment of the present invention, in step 2), the second temperature is 50°C.

[0021] As a preferred embodiment of the present invention, the catalyst includes one of stannous 2-ethylhexanoate, stannous octoate, tin neodecanoate, dibutyltin diacetate, dibutyltin dilaurate, tetrabutyl titanate, tetraisopropyl titanate, tetraethyl titanate, or a composite catalyst with a chelated titanium compound.

[0022] As a preferred embodiment of the present invention, the polymerization inhibitor includes 2,5-di-tert-butyl-p-phenol or 2,6-di-tert-butyl-p-cresol.

[0023] As a preferred embodiment of the present invention, the molecular weight of the hydroxyl-terminated polysiloxane is 500-2000.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) The one-step preparation method of the present invention is safe and controllable, with few by-products, a narrow average molecular weight distribution of the generated product, low viscosity, and no problem of troublesome post-processing of residual raw materials. Excess alkoxysilane coupling agent can be directly used as an adhesion promoter to enhance adhesion to the substrate. Due to the presence of long-chain dimethylsiloxane in the main chain, the surface energy is low, and the resistance to external moisture, corrosive gas, dust and ultraviolet aging is strong. At the same time, due to the low system viscosity and non-silicon diluent, the chip coating has high fullness, slow flow wettability, and high performance consistency at all positions of the coating. The system is solvent-free and adopts an automated flow coating process, which is environmentally friendly and efficient.

[0026] 2) The main structure of the solvent-free UV moisture dual-curing silicone conformal coating resin prepared by the one-step method of the present invention is a silicone segment, which has low surface tension to resist the adhesion of moisture, dust and corrosive gases, good antistatic insulation and flame retardant properties, and excellent mechanical and electrical properties to meet the increasingly sophisticated circuit board component protection requirements.

[0027] 3) The one-step method for preparing the solvent-free UV moisture dual-curing silicone conformal coating resin of the present invention has a higher alkoxy silicon functionality and can form a stronger bonding performance with the glass fiber substrate of the circuit board during the moisture curing process.

[0028] 4) The solvent-free UV moisture dual-curing silicone conformal coating resin prepared by the method of the present invention has a small average molecular weight, can better wet the semiconductor components soldered on the circuit board and form a protective coating with uniform distribution and consistent thickness, while meeting the national environmental protection policy and meeting the requirements of the fast assembly line production process, having good storage stability, and flexible and changeable application formulas to meet the requirements of different places and different application fields; when used in the subsequent coating application process, it does not require more diluting monomers, has a high coating fullness, has good wettability to the chip, and has high performance consistency at all positions of the coating.

[0029] 5) The solvent-free UV moisture dual-curing silicone conformal coating resin prepared by the method of the present invention can be used in circuit board protection fields such as high-end PCB industrial electronics, automotive electronics, consumer electronics, aerospace electronics and military electronics. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0031] Figure 1 It is a reaction principle diagram of the present invention.

[0032] Figure 2 It is the infrared spectrum of the product after the condensation reaction of Example 1. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention provides a one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, see Figure 1 The present invention carries out polycondensation dealcoholization reaction on gamma-acryloxypropyltrimethoxysilane, bihydroxyl polysiloxane and a catalyst, and obtains UV moisture dual-curing organic silicon conformal coating resin after vacuum degassing and purification.

[0035] The solvent-free UV moisture dual-curing silicone conformal coating resin of the present invention can be used in the subsequent application process to adjust the conventional indicators such as glass transition temperature, wetting, dispersing and defoaming properties, surface tension and gloss required by the later coating by using some UV monomers and additives.

[0036] The solvent-free UV moisture dual-curing silicone conformal coating resin prepared by the method of the present invention has a room temperature viscosity of <100 cP, is environmentally friendly and solvent-free, and is easy to apply and construct. Compared with conventional solvent-free UV moisture dual-curing aliphatic polyester polyurethane acrylate systems, it has a longer applicability period during storage due to the absence of isocyanate groups.

[0037] The conformal coating prepared using the resin of the present invention can be directly used in the assembly line coating process of circuit boards. The first step of UV curing fixes the sealing layer to prevent it from sagging, and the secondary moisture curing improves the sealing strength of the silicon coating and improves the shortcomings of the silicon coating such as high air permeability and poor resistance to penetration of moisture corrosive gases. The shadow areas generated by the high and low sides of the components that are not exposed to UV light can also be completely coated and protected through the second step of moisture curing.

[0038] The resin obtained by the method of the present invention has many advantages of organic silicon, such as excellent mechanical properties that can completely eliminate the stress resistance caused by high and low temperature impacts generated before and after the current passes through the components on the circuit board, excellent electrical insulation performance, leakage short circuit prevention, excellent wetting penetration bonding strength with glass fiber substrate circuit boards, and high cross-linking density and strength of UV resin and gloss of the sealing layer.

[0039] In the present invention, the radiation curing defoamer is preferably: one or a combination of two or more of Evonik Deco 270, 2300, 2200N, 2250, and 2500.

[0040] Example 1

[0041] This embodiment provides a one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, comprising:

[0042] 1) Take 68g of γ-acryloxypropyltrimethoxysilane, 70g of hydroxyl-terminated polysiloxane (molecular weight 600, hydroxyl content 5.1%), 1.3g of tetraisopropyl titanate catalyst, heat and stir to 40 degrees Celsius, react under stirring, monitor the changes of hydroxyl groups in the system during the reaction, and take samples for infrared testing during the process; in addition, before sampling during the process, a gentle heating method should be maintained, and the small molecule alcohol in the system should be removed by nitrogen. During the process, the vacuum can be appropriately increased to quickly remove the small molecule alcohol generated in the reaction system. After 2 hours of reaction, samples are taken to monitor the reaction of silanol groups. If the silanol groups are not completely reacted, the above operation is continued until the silanol groups in the reaction system are completely consumed. The reaction time is 5 hours; continue stirring to reduce the temperature of the reaction bottle liquid to room temperature, sample and test the viscosity 30.24cP, the molecular weight test Mn=1536, and the product viscosity doubles, which can be considered to be sufficient condensation reaction. Figure 2 It can be seen that the product after the reaction appears 1730cm -1 The characteristic peaks of carbonyl (C=O) and 1170 cm -1 and 1250cm -1 The peaks at the bottom are the symmetric stretching vibration and antisymmetric stretching vibration peaks of the CO bond, which also proves that the acrylate group is successfully connected to both ends of the polysiloxane. Figure 2 There are still some hydroxyl groups in the reaction, which is mainly due to the sampling during the reaction, and there may be residual alcohol in the system that has not been removed. Figure 2 There are still hydroxyl peaks remaining in the resin, but this does not prevent the resin from being formulated into coatings and its subsequent use.

[0043] After the reaction is completed, 0.69g of inhibitor 2,6-di-tert-butyl-p-cresol is added, and 5.6g of radiation-curable defoamer is added, wherein the radiation-curable defoamer is Evonik Deco 2300 and 270 of Germany, and the mass ratio of Evonik Deco 2300 and 270 of Germany is 1:1. After stirring evenly at 50 degrees Celsius, vacuum degassing is complete to obtain solvent-free UV moisture dual-curing silicone conformal coating resin.

[0044] The test data of the resin prepared in Example 1 after being formulated into a coating are as follows:

[0045] Medium pressure mercury lamp 70mW / cm 2Surface drying time: 30 seconds, medium pressure mercury lamp 40mW / cm 2 After 60 seconds of curing and 7 days of curing at 22 degrees Celsius and 55% relative humidity, the properties are as follows: Thermal expansion coefficient 2.39×10 -4 K -1 (ISO 11359-2), thermal conductivity 0.15W / (m·K) (ISO 8302), glass transition temperature -45℃, water adsorption coefficient at 23℃ for 24 hours is 0 (ISO 62), elongation 15% (ISO 37), tensile strength 70psi (ISO 37), tear strength 0.8N / mm (ISO 34-1), Shore hardness 70 (ISO868), UV curing depth >0.9mm, dielectric constant 3.15 at 1kHz (IEC 60250), volume resistivity 2×10 14 Ω·cm(IEC60093), surface resistance 8×10 16 Ω(IEC60093), dielectric breakdown strength 18kV / mm(IEC-60243-1).

[0046] Example 2

[0047] This embodiment provides a one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, comprising:

[0048] Take 70g of γ-acryloxypropyltrimethoxysilane, 100g of hydroxyl-terminated polysiloxane (molecular weight 2000, hydroxyl content 1.6%), 1.7g of tetraisopropyl titanate catalyst, heat and stir to 50 degrees Celsius, react under stirring, monitor the changes of hydroxyl groups in the system during the reaction, and take samples for infrared testing during the process; in addition, before sampling during the process, a gentle heating method should be maintained, and small molecule alcohols in the system should be removed by nitrogen. During the process, vacuum can be appropriately drawn to increase the vacuum degree to quickly remove the small molecule alcohols generated in the reaction system, and the above operation is repeated until the silanol groups in the reaction system are completely consumed, and the reaction time is 5 hours;

[0049] Continue stirring to lower the temperature of the liquid in the reaction bottle to room temperature. Take a sample and test the viscosity, which is 65.03 cP. The product viscosity doubles, indicating that the condensation reaction is sufficient. The molecular weight test Mn=2488.

[0050] After the reaction is completed, 0.85g of inhibitor 2,6-di-tert-butyl-p-cresol is added, and 8.5g of radiation-curing defoamer is added. The radiation-curing defoamer added is Evonik Deco 2300 and 270 of Germany. The mass ratio of Evonik Deco 2300 and 270 of Germany is 1:1. After stirring evenly at 50 degrees Celsius, vacuum degassing is completed to obtain solvent-free UV moisture dual-curing silicone conformal coating resin.

[0051] The test data of the resin of Example 2 after being formulated into a coating are as follows:

[0052] Medium pressure mercury lamp 70mW / cm 2 Surface drying time: 30 seconds, medium pressure mercury lamp 40mW / cm 2 After 60 seconds of curing and 7 days of curing at 22 degrees Celsius and 55% relative humidity, the properties are as follows: Thermal expansion coefficient 2.45×10 -4 K -1 (ISO 11359-2), thermal conductivity 0.15W / (m·K) (ISO 8302), glass transition temperature -45℃, water adsorption coefficient at 23℃ for 24 hours is 0 (ISO 62), elongation 15% (ISO 37), tensile strength 70psi (ISO 37), tear strength 0.8N / mm (ISO 34-1), Shore hardness 70 (ISO868), UV curing depth >0.9mm, dielectric constant 3.3 at 1kHz (IEC 60250), volume resistivity 2×10 14 Ω·cm(IEC60093), surface resistance 8×10 16 Ω(IEC60093), dielectric breakdown strength 20kV / mm(IEC-60243-1).

[0053] Example 3

[0054] This embodiment provides a one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, comprising:

[0055] Take 82g of γ-acryloxypropyltrimethoxysilane, 100g of hydroxyl-terminated polysiloxane (molecular weight 1000, hydroxyl content 2.9%), 1.8g of tetraisopropyl titanate catalyst, heat and stir to 45 degrees Celsius, react under stirring, monitor the changes of hydroxyl groups in the system during the reaction, and take samples for infrared testing during the process; in addition, before sampling during the process, a gentle heating method should be maintained, and small molecule alcohols in the system should be removed by nitrogen. During the process, vacuum can be appropriately drawn to increase the vacuum degree to quickly remove the small molecule alcohols generated in the reaction system. Repeat the above operation until the silanol groups in the reaction system are completely consumed, and the reaction time is 5 hours; continue stirring to reduce the temperature of the reaction bottle liquid to room temperature, take samples for testing, and the viscosity is 56.3cP and the molecular weight is 1448.

[0056] After the reaction is completed, 0.91g of inhibitor 2,6-di-tert-butyl-p-cresol is added, and 9.1g of radiation-curing defoaming agent is added. The added radiation-curing defoaming agent is Evonik Deco 2300 and 270 of Germany. The mass ratio of Evonik Deco 2300 and 270 of Germany is 1:1. After stirring evenly at 50 degrees Celsius, vacuum degassing is complete to obtain the desired one-step preparation of solvent-free UV moisture dual-curing silicone conformal coating resin.

[0057] The test data of the resin prepared in Example 3 after being formulated into a coating are as follows:

[0058] Medium pressure mercury lamp 70mW / cm 2 Surface drying time: 30 seconds, medium pressure mercury lamp 40mW / cm 2 After 60 seconds of curing and 7 days of curing at 22 degrees Celsius and 55% relative humidity, the properties are as follows: Thermal expansion coefficient 2.50×10 -4 K -1 (ISO 11359-2), thermal conductivity 0.15W / (m·K) (ISO 8302), glass transition temperature -45℃, water adsorption coefficient at 23℃ for 24 hours is 0 (ISO 62), elongation 15% (ISO 37), tensile strength 70psi (ISO 37), tear strength 0.8N / mm (ISO 34-1), Shore hardness 70 (ISO868), UV curing depth>0.9mm, dielectric constant 3.2 at 1kHz (IEC 60250), volume resistivity 2×10 14 Ω·cm(IEC60093), surface resistance 8×10 16 Ω(IEC60093), dielectric breakdown strength 19kV / mm(IEC-60243-1).

[0059] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin, characterized in that: The method comprises the following steps: 1) Prepare raw materials: γ-acryloxypropyltrimethoxysilane, hydroxyl-terminated polysiloxane, catalyst, partial radiation-curable defoamer and inhibitor; 2) adding γ-acryloxypropyltrimethoxysilane, hydroxyl-terminated polysiloxane and a catalyst into a reaction container, heating and stirring to a first temperature, monitoring changes in the hydroxyl value in the reaction system during the reaction, and adding an inhibitor and a partial radiation-curable defoamer when it is detected that the silanol groups in the reaction system are completely consumed, stirring evenly and evacuating until degassing is complete to obtain a solvent-free UV moisture dual-curing silicone conformal coating resin.

2. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: The raw materials include, by weight: 2.5 to 4 parts of gamma-acryloxypropyltrimethoxysilane, 1 part of hydroxyl-terminated polysiloxane, 0.01 to 0.1 parts of catalyst, 0.1 to 0.2 parts of partially radiation-curable defoamer and 0.005 to 0.02 parts of polymerization inhibitor.

3. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: In step 2), the first temperature is 30°C to 60°C, and the reaction time is 2h to 8h.

4. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: In step 2), the sampling time interval is 1 hour, and the sampling times are 2 to 6 times.

5. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 4, characterized in that: The reaction time is 4h to 5h.

6. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: The vacuum degree is -80 kPa to -90 kPa.

7. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: In step 2), the second temperature is 50°C.

8. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: The catalyst includes one of stannous 2-ethylhexanoate, stannous octoate, tin neodecanoate, dibutyltin diacetate, dibutyltin dilaurate, tetrabutyl titanate, tetraisopropyl titanate, tetraethyl titanate, or a composite catalyst with a chelated titanium compound.

9. The method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin in one step according to claim 1, characterized in that: The polymerization inhibitor includes 2,5-di-tert-butyl-p-phenol or 2,6-di-tert-butyl-p-cresol.

10. A one-step method for preparing a solvent-free UV moisture dual-curing silicone conformal coating resin according to any one of claims 1 to 9, characterized in that: The molecular weight of the hydroxyl-terminated polysiloxane is 500-2000.

Citation Information

Cited By

  • Light and moisture dual-curing organic silicon resin as well as synthesis method and application thereof