Synthesis method of polyboroaluminocarbosilane containing boron and aluminum

Through the polyboron aluminum-carbosilane synthesis method that uniformly dopsy B and Al elements in ceramics, the problem of uneven distribution of sintering additives in ceramics is solved, and the high density and structural consistency of the ceramics are achieved, which is suitable for high performance Preparation of SiC ceramics.

CN119039592APending Publication Date: 2024-11-29NINGBO ZHONGXING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310616525.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing ceramic preparation methods, it is difficult to achieve uniform distribution of sintering additives on the atomic scale in ceramics, resulting in uneven density and structural structure of the ceramics, which limits its application.

Method used

A synthesis method of polyboron aluminum-carbosilane (PBACS) containing boron and aluminum is adopted to carry out cracking and rearrangement reaction in an autoclave under an inert atmosphere to generate low molecular weight polycarbonsilane, and aluminum acetylacetone is introduced on the basis of it. and boric acid, uniform doping of B and Al is achieved, forming a uniformly distributed ceramic pioneer.

Benefits of technology

It realizes uniform distribution of B and Al in ceramics, improves the density and structural consistency of the ceramics, reduces the sintering temperature and preparation cost, and is suitable for industrial batch preparation of high-performance SiC ceramics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a synthesis method of boron and aluminum-containing polyboroaluminocarbosilane, which comprises the following steps: (1) in an inert atmosphere, heating polydimethylsilane in a sealed high-pressure kettle for reaction to obtain low-molecular-weight polycarbosilane; and (2) mixing the low-molecular-weight polycarbosilane, aluminum acetylacetonate, boric acid and xylene, and carrying out heating reaction in a sealed high-pressure kettle in an inert atmosphere to obtain the boron and aluminum-containing polyboroaluminocarbosilane. According to the invention, B and Al sintering aid elements are introduced into a PCS molecular structure, so that uniform doping of B and Al in the PCS structure is realized, and a new method and approach are provided for preparation of compact SiC ceramics. The method is simple in process and suitable for industrial batch preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing a ceramic precursor, in particular to a method for synthesizing polyboroaluminocarbosilane. Background Art

[0002] High-density ceramics are in widespread and urgent demand in high-tech fields such as aerospace, and the densification of ceramics is also a research hotspot for researchers in the ceramic field around the world. At present, researchers have invented a variety of methods for preparing ceramics, such as sol-gel method, powder sintering method, carbon thermal reduction method, precursor conversion method, etc. However, the ceramics prepared by these methods have the problems of large porosity and low density, which makes the density of the prepared ceramics far from the theoretical density. In order to solve the above problems, researchers have invented many new methods, such as hot pressing sintering, spark plasma sintering, chemical vapor deposition, adding sintering aids, etc., which have played an important role in promoting the development of the ceramic field and improving the densification level of ceramics.

[0003] Adding sintering aids is an important method and effective way to improve the density level of ceramics. This method can effectively reduce the sintering preparation temperature of ceramics while effectively improving the densification level of ceramics, greatly reducing the difficulty and cost of preparation. It has become a commonly used method for preparing high-performance ceramics. At present, a variety of sintering aids have been invented, such as B, Al, SiC, BN, Al2O3 and ceramic precursor polymers. However, the biggest drawback of this method is that it is difficult to achieve uniform distribution and addition of sintering aids in ceramics at the atomic scale, resulting in uneven and inconsistent distribution of composition, structure and ingredients in the final ceramics, thereby limiting its further application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for synthesizing polyboroaluminocarbosilane containing boron and aluminum in which boron and aluminum are uniformly doped in polycarbosilane.

[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: a method for synthesizing polyboronoaluminocarbosilane (PBACS) containing boron and aluminum, comprising the following steps: (1) Under an inert atmosphere, polydimethylsilane (PDMS) is heated in a sealed autoclave to undergo cracking and rearrangement reactions to obtain low molecular weight polycarbosilane (LPCS); (2) The LPCS, aluminum acetylacetonate, boric acid and xylene are mixed, and the temperature is increased in a sealed autoclave under an inert atmosphere to perform a cracking and rearrangement reaction. After the reaction is completed, the solvent is removed to obtain PBACS.

[0006] The solvent can be removed by distillation under reduced pressure, or other methods that can remove the solvent are also feasible.

[0007] PBACS can be prepared by adopting the above technical solution.

[0008] Preferably, in step (1), the temperature of the cracking and rearrangement reaction is 300-650°C, more preferably 350-600°C.

[0009] By adopting the above technical solution, a better cracking and rearrangement effect is achieved.

[0010] Preferably, in step (1), the cleavage and rearrangement reaction time is 1 to 20 hours, more preferably 2 to 15 hours.

[0011] By adopting the above technical solution, a better cracking and rearrangement effect is achieved.

[0012] Preferably, in step (1), the ratio of PDMS mass to autoclave volume is 95-105 g:1 L.

[0013] By adopting the above technical solution, a suitable reaction pressure can be provided, and a better cracking and rearrangement effect can be achieved.

[0014] Preferably, in step (1), the heating rate is 5 to 100°C / min, more preferably 10 to 70°C / min.

[0015] Generally, the above technical solution is faster and more efficient under the premise of safety. A lower heating rate is safer but will extend the overall synthesis time. The most suitable heating rate may vary according to the size of the autoclave and can be adjusted appropriately according to actual conditions. When using a new autoclave, you can start the test at a lower rate.

[0016] Preferably, in step (1), the inert atmosphere is a nitrogen atmosphere.

[0017] Inert gases are used to provide an environment that does not participate in chemical reactions, and other atmospheres that can achieve this effect are also possible.

[0018] The cracking reaction principle of step (1) is as follows: -[Si(CH3)2] n -→-[(H or CH3)Si(CH3)-CH2] n -. The LPCS prepared in step (1) of the present invention is solid; LPCS has a higher molecular weight than liquid LLPCS (low molecular weight liquid polycarbosilane), and the structure of the subsequent product can be better controlled; although LLPCS has a lower molecular weight, it is liquid, so the subsequent process is simpler; LPCS and LLPCS each have their own advantages. In the present invention, it is more appropriate to use LPCS as the product of step (1).

[0019] Preferably, in step (2), the temperature of the cracking and rearrangement reaction is 300-700°C, more preferably 320-600°C.

[0020] By adopting the above technical solution, a better cracking and rearrangement effect is achieved.

[0021] Preferably, in step (2), the cleavage and rearrangement reaction time is 1 to 20 hours, more preferably 2 to 15 hours.

[0022] By adopting the above technical solution, a better cracking and rearrangement effect is achieved.

[0023] Preferably, in step (2), the weight ratio of LPCS to xylene is 20-80:100, more preferably 25-70:100.

[0024] By adopting the above technical solution, a better cracking and rearrangement effect is achieved.

[0025] Preferably, in step (2), the ratio of the mass of xylene to the volume of the autoclave is 35-45 g:1 L.

[0026] By adopting the above technical solution, a suitable reaction pressure can be provided, and a better cracking and rearrangement effect can be achieved.

[0027] Preferably, in step (2), the weight ratio of aluminum acetylacetonate to LPCS is 1-8:100, more preferably 1-6:100.

[0028] By adopting the above technical solution, the aluminum content in the product can be controlled, and the above range is adopted to make the obtained PBACS have a better sintering effect; it can also be adjusted according to actual needs, which mainly affects the product performance and has little effect on the success rate of synthesizing PBACS.

[0029] Preferably, in step (2), the weight ratio of boric acid to LPCS is 0.1-2:100, more preferably 0.1-1.8:100.

[0030] By adopting the above technical solution, the boron content in the product can be controlled, and the above range is adopted to make the obtained PBACS have a better sintering effect; it can also be adjusted according to actual needs, which mainly affects the product performance and has little effect on the success rate of synthesizing PBACS.

[0031] Preferably, in step (2), the heating rate is 5 to 100°C / min, more preferably 10 to 70°C / min.

[0032] Generally, the above technical solution is faster and more efficient under the premise of safety. A lower heating rate is safer but will extend the overall synthesis time. The most suitable heating rate may vary according to the size of the autoclave and can be adjusted appropriately according to actual conditions. When using a new autoclave, you can start the test with a lower rate and try to increase the heating rate in subsequent tests.

[0033] Preferably, in step (2), the inert atmosphere is a nitrogen atmosphere.

[0034] Inert gases are used to provide an environment that does not participate in chemical reactions, and other atmospheres that can achieve this effect are also possible.

[0035] The reaction in step (2) involves the self-crosslinking and cleavage rearrangement of LPCS, as well as the bridging of the intermediate products with Al and B respectively; in the final product, Al and B mainly exist in the form of Al-O-Si, Al-OC, BO-Si, BOC and the bridges between them. After the reaction in step (2), the B and Al elements are uniformly doped in the PCS structure, and the density of the ceramics prepared by the obtained PBACS as a precursor reaches a high level.

[0036] Preferably, the preparation method of PDMS comprises: adding dichlorodimethylsilane to a reaction solvent containing metallic sodium particles under inert gas protection while stirring, condensing and refluxing, collecting the precipitate after the reaction is completed, washing and drying.

[0037] The method uses dichlorodimethylsilane as a monomer and synthesizes PDMS through sodium condensation. The obtained PDMS is in the form of white powder.

[0038] More preferably, in the method for preparing PDMS, the reaction temperature is 60-85° C., and further preferably 65-75° C. This temperature condition can promote the reaction.

[0039] More preferably, in the preparation method of PDMS, the molar ratio of metallic sodium to dichlorodimethylsilane is 2.02-2.1:1.

[0040] This reaction is a Na condensation reaction, the principle is relatively simple, the reaction equation is: n(CH3)2SiCl2+2nNa=[(CH3)2Si] n +2nNaCl, The theoretical reaction molar ratio of dichlorodimethylsilane and metallic Na is 1:2; in the actual experimental operation process, a slight excess of metallic Na is used to ensure that all dichlorodimethylsilane participates in the reaction to increase the yield of the target product, which is also a necessary operating method in the organic synthesis process.

[0041] More preferably, in the method for preparing PDMS, the reaction time is 5 to 30 hours, and further preferably 10 to 25 hours. With this reaction time, the reaction yield is higher.

[0042] More preferably, in the method for preparing PDMS, the particle size of the metal sodium particles is less than 3 mm. When the volume of the metal sodium particles is too large, the specific surface area is small and the reaction rate will be reduced.

[0043] More preferably, in the method for preparing PDMS, the reaction solvent is toluene and / or n-hexane. The above reaction solvents have a better reaction effect.

[0044] More preferably, in the method for preparing PDMS, the stirring speed is 100-500 r / min. Stirring promotes uniform distribution of substances in the system and makes the reaction more uniform. The speed can be selected according to actual conditions.

[0045] More preferably, in the method for preparing PDMS, the inert gas is one or both of nitrogen and argon. The inert gas is used to provide an environment that does not participate in chemical reactions, and other atmospheres that can achieve this effect are also feasible.

[0046] The obtained PBACS is used as a precursor and is cracked at high temperature (such as 1400-1900°C, keeping warm for 30-300 minutes) under the protection of inert gas to obtain sintered SiC ceramics containing B and Al elements.

[0047] Principle of the invention: The precursor conversion method has become an important method for preparing ceramic materials due to the advantages of controllable and designable precursor composition structure, uniform distribution, good processability, low ceramic conversion temperature, and uniform composition structure and performance of ceramic products. The present invention combines the precursor conversion method with the addition of sintering aids, introduces B and Al sintering aid elements into the PCS molecular structure, and realizes uniform doping of B and Al in the PCS structure. After inorganic conversion, B and Al can be evenly distributed in the ceramic matrix at the atomic scale, and high-density SiC ceramics can be prepared.

[0048] Beneficial effects of the invention: The invention introduces B and Al sintering aid elements into the PCS molecular structure, realizes uniform doping of B and Al in the PCS structure, and provides a new method and approach for the preparation of dense SiC ceramics. The method is simple in process and suitable for industrial batch preparation. DETAILED DESCRIPTION

[0049] The present invention will be further described below with reference to the embodiments.

[0050] The raw materials used in the examples of the present invention are all obtained through conventional commercial channels. Example 1

[0051] The synthesis method of the polyboroaluminocarbosilane containing boron and aluminum in this embodiment comprises the following steps: (1) Place 100 g of PDMS in a 1 L autoclave, evacuate and replace with N2, and then seal. Heat the autoclave to 420 °C at a rate of 20 °C / min and keep it warm for 10 h. After the reaction is completed, LPCS can be obtained with a softening point of 62 °C.

[0052] (2) Dissolve 10 g of LPCS, 0.2 g of aluminum acetylacetonate, and 0.1 g of boric acid in 40 g of xylene and place in a 1 L autoclave. After evacuating and replacing with N2, seal the autoclave and heat it to 450 °C at a rate of 15 °C / min and keep it warm for 10 h. After the reaction is completed, cool the system to room temperature and distill the product under reduced pressure to remove the solvent to obtain PBACS.

[0053] The preparation method of the PDMS is: 200g of metal sodium was placed in a 5000ml three-necked flask equipped with mechanical stirring and condensation reflux device. The sodium particles were smaller than 3mm in size, and 2000ml of toluene was added. Under the protection of high purity N2, the system temperature was raised to 70°C and the stirring speed was 250 r / min. Then the dichlorodimethylsilane monomer was added to the system (the molar ratio of sodium metal to monomer was 2.05); the reaction was completed after 25 hours. The precipitate was removed by separation and filtration. The obtained precipitate was washed with alcohol, water and dried to obtain PDMS.

[0054] 2 g of the obtained PBACS was placed in a crucible and placed in a sintering furnace. Under Ar protection, the furnace temperature was raised to 1800 °C at a heating rate of 10 °C / min and kept at this temperature for 1 h to obtain a sintered SiC ceramic containing B and Al elements. The density was measured to be 3.02 g / cm 3 , high level of densification. Example 2

[0055] The synthesis method of the polyboroaluminocarbosilane containing boron and aluminum in this embodiment comprises the following steps: (1) Place 100 g of PDMS in a 1 L autoclave, evacuate and replace with N2, and then seal. Heat the autoclave to 420 °C at a rate of 20 °C / min and keep it warm for 10 h. After the reaction is completed, LPCS can be obtained with a softening point of 62 °C.

[0056] (2) Dissolve 10 g of LPCS, 0.2 g of aluminum acetylacetonate, and 0.1 g of boric acid in 40 g of xylene and place in a 1 L autoclave. After evacuating and replacing with N2, seal the autoclave and heat it to 450 °C at a rate of 15 °C / min and keep it warm for 10 h. After the reaction is completed, cool the system to room temperature and distill the product under reduced pressure to remove the solvent to obtain PBACS.

[0057] The preparation method of the PDMS is: 200g of metallic sodium is placed in a 5000ml three-necked flask equipped with a mechanical stirrer and a condensation reflux device. The particle size of the sodium particles is less than 3mm. 2000ml of toluene is added. Under the protection of high-purity N2, the system temperature is raised to 70°C and the stirring speed is 250r / min. Then dichlorodimethylsilane monomer is added to the system (the molar ratio of metallic sodium to monomer is 2.10); the reaction ends after 25h. The precipitate is separated and filtered to remove it. The precipitate is washed with alcohol, washed with water, and dried to obtain PDMS.

[0058] 2 g of the obtained PBACS was placed in a crucible and placed in a sintering furnace. Under Ar protection, the furnace temperature was raised to 1600 °C at a heating rate of 10 °C / min and kept at this temperature for 1 h to obtain a sintered SiC ceramic containing B and Al elements. The density was measured to be 2.9 g / cm 3 , high level of densification. Example 3

[0059] The synthesis method of the polyboroaluminocarbosilane containing boron and aluminum in this embodiment comprises the following steps: (1) Place 100 g of PDMS in a 1 L autoclave, evacuate and replace with N2, and then seal. Heat the autoclave to 420 °C at a rate of 20 °C / min and keep it warm for 10 h. After the reaction is completed, LPCS can be obtained with a softening point of 62 °C.

[0060] (2) Dissolve 10 g of LPCS, 0.1 g of aluminum acetylacetonate, and 0.1 g of boric acid in 40 g of xylene and place in a 1 L autoclave. After evacuating and replacing with N2, seal the autoclave and heat it to 450 °C at a rate of 15 °C / min and keep it warm for 10 h. After the reaction is completed, cool the system to room temperature and distill the product under reduced pressure to remove the solvent to obtain PBACS.

[0061] The preparation method of the PDMS is: 200g of metallic sodium is placed in a 5000ml three-necked flask equipped with a mechanical stirrer and a condensation reflux device. The particle size of the sodium particles is less than 3mm. 2000ml of toluene is added. Under the protection of high-purity N2, the system temperature is raised to 70°C and the stirring speed is 250r / min. Then dichlorodimethylsilane monomer is added to the system (the molar ratio of metallic sodium to monomer is 2.05); the reaction ends after 25h. The precipitate is separated and filtered to remove it. The precipitate is washed with alcohol, washed with water, and dried to obtain PDMS.

[0062] 2 g of the obtained PBACS was placed in a crucible and placed in a sintering furnace. Under Ar protection, the furnace temperature was raised to 1800 °C at a heating rate of 10 °C / min and kept at this temperature for 1 h to obtain a sintered SiC ceramic containing B and Al elements. The density was measured to be 2.97 g / cm 3 , high level of densification.

Claims

1. A method for synthesizing polyboroaluminocarbosilane containing boron and aluminum, characterized in that: The following steps are involved: (1) In an inert atmosphere, polydimethylsilane is heated in a sealed autoclave to undergo a cracking and rearrangement reaction to obtain a low molecular weight polycarbosilane; (2) The low molecular weight polycarbosilane, aluminum acetylacetonate, boric acid and xylene are mixed, and the temperature is increased in a sealed autoclave under an inert atmosphere to carry out a cracking and rearrangement reaction. After the reaction is completed, the solvent is removed to obtain a polyboroaluminocarbosilane containing boron and aluminum.

2. The method for synthesizing polyboroaluminocarbosilane containing boron and aluminum according to claim 1, characterized in that: In step (1), the temperature of the cracking and rearrangement reaction is 300-650° C.; and the time of the cracking and rearrangement reaction is 1-20 h.

3. The method for synthesizing polyboroaluminocarbosilane containing boron and aluminum according to claim 1 or 2, characterized in that: In step (1), the ratio of the mass of polydimethylsilane to the volume of the autoclave is 95-105 g:1 L.

4. The method for synthesizing a polyboroaluminocarbosilane containing boron and aluminum according to any one of claims 1 to 3, characterized in that: In step (1), the heating rate is 5-100°C / min; and the inert atmosphere is a nitrogen atmosphere.

5. The method for synthesizing a polyboroaluminocarbosilane containing boron and aluminum according to any one of claims 1 to 4, characterized in that: In step (2), the temperature of the cracking and rearrangement reaction is 300-700° C.; and the time of the cracking and rearrangement reaction is 1-20 h.

6. The method for synthesizing a polyboroaluminocarbosilane containing boron and aluminum according to any one of claims 1 to 5, characterized in that: In step (2), the weight ratio of the low molecular weight polycarbosilane to xylene is 20-80:100; and the ratio of the mass of xylene to the volume of the autoclave is 35-45 g:1 L.

7. The method for synthesizing a polyboroaluminocarbosilane containing boron and aluminum according to any one of claims 1 to 6, characterized in that: In step (2), the weight ratio of aluminum acetylacetonate to low molecular weight polycarbosilane is 1-8:100; the weight ratio of boric acid to low molecular weight polycarbosilane is 0.1-2:100; the heating rate is 5-100°C / min; and the inert atmosphere is a nitrogen atmosphere.

8. The method for synthesizing a polyboroaluminocarbosilane containing boron and aluminum according to any one of claims 1 to 7, characterized in that: The preparation method of polydimethylsilane comprises: adding dichlorodimethylsilane into a reaction solvent with metal sodium particles protected by an inert gas while stirring, condensing and refluxing, collecting the precipitate after the reaction is completed, washing and drying.

9. The method for synthesizing polyboroaluminocarbosilane containing boron and aluminum according to claim 8, characterized in that: In the preparation method of polydimethylsilane, the reaction temperature is 60-85° C.; the molar ratio of metallic sodium to dichlorodimethylsilane is 2.02-2.1:1; and the reaction time is 5-30 hours.

10. The method for synthesizing polyboroaluminocarbosilane containing boron and aluminum according to claim 8 or 9, characterized in that: In the preparation method of polydimethylsilane, the particle size of the metal sodium particles is less than 3 mm; the reaction solvent is toluene and / or n-hexane; the stirring speed is 100-500 r / min; and the inert gas is one or both of nitrogen and argon.