High-temperature-resistant modified cyanate ester resin / carbon fiber prepreg and preparation method thereof

The modified cyanate resin was prepared by copolymerization and the addition of stabilizers, which solved the problems of low viscosity and poor stability of existing high-temperature cyanate resins, and prepared materials suitable for carbon fiber prepregs, which had high temperature stability and UV resistance. , atomic oxygen performance, suitable for extreme environments such as aerospace.

CN119039637APending Publication Date: 2024-11-29JIANGSU RUITAI FEIYU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085802.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-temperature resistant cyanate resins have low viscosity or poor stability during the preparation process, making them difficult to directly use as carbon fiber prepregs, and curing problems are prone to occur at high temperatures, which cannot meet the needs of extreme environments such as aerospace.

Method used

The brown paste-like copolymerization of phenolic cyanate monomer, bisphenol A cyanate resin and bisphenol A epoxy resin, and the epoxy-capped phenyltrimethoxysilane and stabilizer were added to prepare a brown paste copolymer. , and coat it onto carbon fibers by hot melt coating process or solvent method to prepare a modified cyanate resin/carbon fiber prepreg to ensure that the amount of glue is between 35% and 45%.

Benefits of technology

A modified cyanate resin with high softening point and moderate room temperature viscosity was obtained, which improved the room temperature storage stability and high temperature resistance of carbon fiber prepregs. The glass transition temperature reached ≥250℃, and it had good resistance to UV aging. and atomic oxygen resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985143550000021
    Figure BDA0004985143550000021
  • Figure BDA0004985143550000022
    Figure BDA0004985143550000022
  • Figure BDA0004985143550000041
    Figure BDA0004985143550000041
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant modified cyanate ester resin / carbon fiber prepreg and a preparation method thereof. The modified cyanate ester resin prepared by adopting a copolymerization method is relatively high in softening point, the room-temperature viscosity of the modified cyanate ester resin is greater than that of pure phenolic cyanate ester, and bisphenol A cyanate ester crystals are avoided, so that the modified cyanate ester resin is suitable for a carbon fiber prepreg system. According to the modified cyanate resin prepared by adopting a copolymerization method, a glyceryl ether polymer is added as a stabilizer, so that the storage stability of the high-temperature-resistant carbon fiber prepreg is improved, the defect of poor room-temperature storage stability of a phenolic cyanate prepolymer is overcome, and the room-temperature storage period of the prepreg is not less than 20 days; and the glass transition temperature Tg of the cured carbon fiber prepreg is greater than or equal to 250 DEG C. The modified cyanate ester resin / carbon fiber prepreg prepared by adopting a copolymerization method has outstanding ultraviolet aging resistance and atomic oxygen resistance, and can be used for a space expansion structure substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a high temperature resistant modified cyanate ester resin / carbon fiber prepreg and a preparation method thereof. Background Art

[0002] As a thermosetting resin, high temperature resistant cyanate ester resin has good high temperature resistance and can remain stable under high temperature conditions. The most important characteristic is that it shows good stability and heat resistance at high temperatures. This makes them suitable for applications that need to withstand high temperature environments or temperature changes. High temperature resistant cyanate ester resins usually have good chemical stability and can resist erosion and corrosion from some chemicals. These resins usually have good mechanical strength and hardness, and can maintain certain physical properties even at high temperatures. In electronic and electrical applications, high temperature resistant cyanate ester resins can also provide good electrical insulation properties. They usually maintain good dimensional and shape stability at high temperatures and are not prone to deformation or shrinkage. In the aerospace field, materials are required to be stable at extreme high temperatures. This resin is used to manufacture engine parts, spacecraft components, etc. Both phenolic cyanate ester curing materials (Tg≥300°C) and bisphenol A cyanate ester curing materials have good temperature resistance (Tg≥240°C), but phenolic cyanate ester curing materials have low viscosity and cannot be directly used as carbon fiber prepreg resins. Bisphenol A cyanate ester is a solid powder at room temperature and is not suitable for carbon fiber prepregs. Moreover, during the direct prepolymerization of phenolic cyanate ester into a viscous resin, the stability is poor and curing problems are prone to occur. The present invention aims to solve the defects of the above-mentioned cyanate ester resins, prepare a prepreg resin with appropriate viscosity by copolymerization, and add a stabilizer to improve the room temperature storage stability, thereby preparing a high temperature resistant carbon fiber prepreg (Tg≥250°C). Summary of the invention

[0003] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0004] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0005] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a high temperature resistant modified cyanate ester resin / carbon fiber prepreg.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:

[0007] Phenolic cyanate ester monomer, bisphenol A cyanate ester resin monomer and bisphenol A epoxy resin are copolymerized to obtain a brown paste copolymer;

[0008] After softening to the softening point, a stabilizer and epoxy-terminated phenyltrimethoxysilane are added, and after being evenly mixed, a modified cyanate ester resin is obtained;

[0009] The modified cyanate ester resin is coated and cured on the carbon fiber by a hot melt coating process or a solvent method to prepare a modified cyanate ester resin / carbon fiber prepreg;

[0010] Wherein, the prepreg has a dipping amount of 35% to 45%.

[0011] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg of the present invention, wherein: the modified cyanate ester resin, measured by mass fraction, comprises:

[0012] 50%~80% phenolic cyanate ester;

[0013] 5% to 20% bisphenol A cyanate resin;

[0014] 5% to 10% bisphenol A epoxy resin;

[0015] 5% to 10% epoxy-terminated phenyltrimethoxysilane;

[0016] 0.1%~1% stabilizer;

[0017] Wherein, the stabilizer includes one or more of glycerol ether polymers, organic peroxides, organic phenol compounds, thiol compounds or organic acid compounds.

[0018] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate resin / carbon fiber prepreg of the present invention, the average molecular weight of the phenolic cyanate ester is 800 to 1000, and the structural formula is as shown in formula (I),

[0019]

[0020] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate resin / carbon fiber prepreg of the present invention, the epoxy equivalent of the bisphenol A type cyanate resin is 0.48 to 0.54, and the structural formula is shown in formula (II).

[0021]

[0022] As a preferred scheme for the preparation method of the high temperature resistant modified cyanate ester resin / carbon fiber prepreg described in the present invention, wherein: the bisphenol A type epoxy resin includes one or more of E51 and E44; the glycerol ether polymer includes one or more of polyethylene glycol glycidyl ether, polyethylene glycol monobutyl ether, and ether polyglycerol glycidyl ether.

[0023] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg of the present invention, the copolymerization temperature is 100 to 150° C., and the copolymerization time is 1 to 24 hours.

[0024] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg of the present invention, the solid content of the modified cyanate ester resin is ≥98% and the softening point is 70-90°C.

[0025] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to the present invention, the carbon fiber fabric comprises one or more of T300, T700, T1000, M40J or M55J.

[0026] As a preferred embodiment of the method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg of the present invention, the curing temperature of the prepreg is 150-200°C.

[0027] Another object of the present invention is to overcome the deficiencies in the prior art and provide a high temperature resistant modified cyanate ester resin / carbon fiber prepreg.

[0028] Beneficial effects of the present invention:

[0029] (1) The modified cyanate ester resin prepared by the copolymerization method of the present invention has a high softening point and a room temperature viscosity greater than that of pure phenolic cyanate ester, and no crystallization of bisphenol A cyanate ester occurs, so the modified cyanate ester resin is suitable for carbon fiber prepreg system.

[0030] (2) The present invention adopts a modified cyanate ester resin prepared by a copolymerization method, and adds a glycerol ether polymer as a stabilizer, thereby improving the storage stability of the high-temperature resistant carbon fiber prepreg and solving the defect of poor room temperature storage stability of the phenolic cyanate prepolymer. The room temperature storage period of the prepreg is not less than 20 days; the glass transition temperature Tg of the carbon fiber prepreg cured product is ≥250°C.

[0031] (3) The modified cyanate resin / carbon fiber prepreg prepared by the copolymerization method of the present invention has outstanding resistance to ultraviolet aging and atomic oxygen, and can be used for a space deployment structure substrate. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0033] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0034] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0035] The raw materials used in the present invention are all commercially available unless otherwise specified.

[0036] The performance of the material prepared in the embodiment of the present invention was tested as follows:

[0037] 1. Test of UV aging resistance: Use LUV-2 UV accelerated aging tester to test different prepregs for UV aging for 192 hours and then measure the ΔE value of the materials. During UV aging, the UV wavelength is 313nm, the temperature is 40℃, and the UV exposure power is 0.06kW.

[0038] 2. Atomic oxygen resistance test: Atomic oxygen effect ground simulation equipment is used to refer to the satellite orbit and the corresponding atomic oxygen flux, that is, at an orbital altitude of 400km and an operation time of 500h, the atomic oxygen flux is about 1×10 20 atoms / cm 2 , the sample was irradiated with atomic oxygen for 24 hours. The original mass of the material is m 0 , the mass change of the material before and after irradiation is Δm. During the test, the mass change of the sample at different times is used to investigate the change of the sample mass loss rate with the cumulative atomic oxygen flux. The mass loss rate calculation method is as follows:

[0039]

[0040] Example 1

[0041] This embodiment provides a method for preparing a high temperature resistant modified cyanate ester resin / carbon fiber prepreg, specifically:

[0042] 67.5% phenolic cyanate monomer (average molecular weight 800), 12.5% ​​bisphenol A cyanate resin monomer (epoxy equivalent 0.5), 7.5% bisphenol A epoxy resin E51 were copolymerized at 125°C for 6h to obtain a brown paste copolymer;

[0043] After softening to 80° C., 5% of a stabilizer (polyethylene glycol glycidyl ether) and 7.5% of epoxy-terminated phenyl trimethoxy silane were added and mixed evenly to obtain a modified cyanate ester resin;

[0044] The modified cyanate ester resin is coated on the T300 carbon fiber by a hot melt coating process and cured at 180° C. to prepare the modified cyanate ester resin / carbon fiber prepreg; the prepreg has a resin impregnation amount of 40%.

[0045] Example 2

[0046] The difference between this embodiment and embodiment 1 is that the impregnation amount of the prepreg is adjusted to 35%, and the rest of the preparation process is the same as that of embodiment 1 to obtain the prepreg.

[0047] Example 3

[0048] The difference between this embodiment and embodiment 1 is that the impregnation amount of the prepreg is adjusted to 45%, and the rest of the preparation process is the same as that of embodiment 1 to obtain the prepreg.

[0049] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 1.

[0050] Table 1

[0051] Example 1 Example 2 Example 3 Glass transition temperature Tg(℃) 350 300 310 Room temperature storage period (days) >70 >70 >70 ΔE 7.5 8 8.3 Mass loss rate (%) 0.56 0.98 0.71

[0052] It can be seen from the above table that adjusting the amount of prepreg has a significant effect on the performance of the prepreg, which is due to the interaction between the resin and the fiber and the change in the resin content. When the amount of impregnation increases, the ratio of fiber to resin will increase, which may cause excessive resin during curing, resulting in an overly dense or uneven cross-linked structure between the resins, affecting the performance of the resin. A reduction in the amount of impregnation may result in insufficient bonding between the resin and the fiber, thereby affecting the strength and heat resistance of the prepreg. According to the results in the above table, the best technical effect can be obtained when the amount of impregnation in the present invention is 40%.

[0053] Example 4

[0054] The present embodiment is different from the embodiment 1 in that the bisphenol A epoxy resin is adjusted to 5% and the phenolic cyanate ester is adjusted to 70%. The rest of the preparation process is the same as that of the embodiment 1 to obtain a prepreg.

[0055] Example 5

[0056] The present embodiment is different from the embodiment 1 in that the bisphenol A epoxy resin is adjusted to 10% and the phenolic cyanate ester is adjusted to 65%. The rest of the preparation process is the same as that of the embodiment 1 to obtain a prepreg.

[0057] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 2.

[0058] Table 2

[0059] Example 1 Example 4 Example 5 Glass transition temperature Tg(℃) 350 280 300 Room temperature storage period (days) >70 >70 >70 ΔE 7.5 9.5 8.8 Mass loss rate (%) 0.56 1.13 0.80

[0060] It can be seen from the above table that adjusting the content of bisphenol A epoxy resin has a significant effect on the performance of the prepreg. This is because bisphenol A epoxy resin acts as a modifier in the formula. Changes in the content of bisphenol A epoxy resin will affect the crosslinking density and structure of the prepolymer, further leading to poor performance of the resin under high temperature conditions. When the content of bisphenol A epoxy resin is too high, it may cause the crosslinking density of the resin system to be too high, making the crosslinking structure between the resins too dense or uneven; it may also cause poor interfacial bonding between the resin and the fiber. According to the results in the above table, the best technical effect can be obtained when the content of bisphenol A epoxy resin in the present invention is 7.5%.

[0061] Example 6

[0062] The difference between this embodiment and embodiment 1 is that the copolymerization temperature is adjusted to 100° C., and the rest of the preparation process is the same as that of embodiment 1 to obtain a prepreg.

[0063] Example 7

[0064] The difference between this embodiment and embodiment 1 is that the copolymerization temperature is adjusted to 150° C., and the rest of the preparation process is the same as that of embodiment 1 to obtain a prepreg.

[0065] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 3.

[0066] Table 3

[0067] Example 1 Example 6 Example 7 Glass transition temperature Tg(℃) 350 260 250 Room temperature storage period (days) >70 >70 >70 ΔE 7.5 8.3 9.9 Mass loss rate (%) 0.56 0.96 0.92

[0068] As can be seen from the above table, adjusting the copolymerization temperature has a significant effect on the performance of the prepreg, because changes in the copolymerization temperature may affect the curing rate and degree of the resin. A higher copolymerization temperature may cause the resin to cure faster, but it may also cause incomplete curing or curing defects, thereby reducing the performance of the prepreg. According to the results in the above table, the best technical effect can be obtained when the copolymerization temperature in the present invention is 125°C.

[0069] Comparative Example 1

[0070] The difference between this comparative example and Example 1 is that the bisphenol A epoxy resin is adjusted to 0, the phenolic cyanate monomer is adjusted to 75%, and the rest of the preparation process is the same as Example 1 to prepare a prepreg.

[0071] Comparative Example 2

[0072] This comparative example provides an existing method for preparing a cyanate ester resin / carbon fiber prepreg, specifically:

[0073] The raw materials were weighed according to the molar ratio of E51 and phenolic cyanate ester of 1:2, placed in a beaker, heated and stirred in an oil bath at 100°C until melted, poured into a mold pre-coated with a release agent, degassed in a vacuum drying oven at 100°C for 15 minutes, and then placed in an electronic oven for heating. The modified cyanate ester resin was coated on T300 carbon fiber by a hot melt coating process, and cured by a process of 150°C 1h + 180°C / 2h + 200°C / 3h, and the post-curing process was 250°C / 4h, finally obtaining a cyanate ester resin / carbon fiber prepreg.

[0074] The performance of the material obtained in the above comparative example was tested, and the comparison results with those of Example 1 are shown in Table 4.

[0075] Table 4

[0076] Example 1 Comparative Example 1 Comparative Example 2 Glass transition temperature Tg(℃) 350 200 260 Room temperature storage period (days) >70 30 45 ΔE 7.5 >12 11.6 Mass loss rate (%) 0.56 3.71 2.58

[0077] It can be seen from the above table that, compared with the unmodified cyanate resin / carbon fiber prepreg and the existing prepreg, the modified cyanate resin prepared by the copolymerization method of the present invention has a higher softening point and a room temperature viscosity greater than that of pure phenolic cyanate, and no crystallization of bisphenol A cyanate occurs, and is suitable for the carbon fiber prepreg system.

[0078] In summary, the present invention adopts a modified cyanate ester resin prepared by a copolymerization method, adds a glycerol ether polymer as a stabilizer, improves the storage stability of the high-temperature resistant carbon fiber prepreg, solves the defect of poor room temperature storage stability of the phenolic cyanate prepolymer, and the room temperature storage period of the prepreg is not less than 20 days; the glass transition temperature Tg of the carbon fiber prepreg cured product is ≥250°C.

[0079] The modified cyanate resin / carbon fiber prepreg prepared by the copolymerization method of the present invention has outstanding ultraviolet aging resistance and atomic oxygen resistance performance, and can be used for a space deployment structure substrate.

[0080] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a high temperature resistant modified cyanate ester resin / carbon fiber prepreg, characterized in that: include, Phenolic cyanate ester monomer, bisphenol A cyanate ester resin monomer and bisphenol A epoxy resin are copolymerized to obtain a brown paste copolymer; After softening to the softening point, a stabilizer and epoxy-terminated phenyltrimethoxysilane are added, and after being evenly mixed, a modified cyanate ester resin is obtained; The modified cyanate ester resin is coated and cured on the carbon fiber by a hot melt coating process or a solvent method to prepare a modified cyanate ester resin / carbon fiber prepreg; Wherein, the prepreg has a dipping amount of 35% to 45%.

2. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 1, characterized in that: The modified cyanate ester resin, measured by mass fraction, includes: 50%~80% phenolic cyanate ester; 5% to 20% bisphenol A cyanate resin; 5% to 10% bisphenol A epoxy resin; 5% to 10% epoxy-terminated phenyltrimethoxysilane; 0.1%~1% stabilizer; Wherein, the stabilizer includes one or more of glycerol ether polymers, organic peroxides, organic phenol compounds, thiol compounds or organic acid compounds.

3. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 2, characterized in that: The average molecular weight of the phenolic cyanate ester is 800 to 1000, and the structural formula is as shown in formula (I).

4. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 2, characterized in that: The bisphenol A cyanate resin has an epoxy equivalent of 0.48 to 0.54 and a structural formula as shown in formula (II).

5. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 2, characterized in that: The bisphenol A epoxy resin includes one or more of E51 and E44; the glycerol ether polymer includes one or more of polyethylene glycol glycidyl ether, polyethylene glycol monobutyl ether, and ether polyglycerol glycidyl ether.

6. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 1, characterized in that: The copolymerization temperature is 100-150° C., and the copolymerization time is 1-24 hours.

7. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 1, characterized in that: The solid content of the modified cyanate ester resin is ≥98%, and the softening point is 70-90°C.

8. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 1, characterized in that: The carbon fiber fabric includes one or more of T300, T700, T1000, M40J or M55J.

9. The method for preparing the high temperature resistant modified cyanate ester resin / carbon fiber prepreg according to claim 1, characterized in that: The curing temperature of the prepreg is 150-200°C.

10. The high temperature resistant modified cyanate ester resin / carbon fiber prepreg prepared by the preparation method according to any one of claims 1 to 9.