Anti-fouling release film and preparation method thereof

By using chitosan-modified titanium dioxide, siloxane-modified polyurethane acrylate and fluorocarbon surfactant in the release film, the problem of insufficient anti-fouling ability of the existing release film is solved, and the film is significantly improved Anti-fouling performance and service life.

CN119039638APending Publication Date: 2024-11-29ZHEJIANG DAHUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166525.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing release film has insufficient anti-fouling ability and is easily contaminated by oil, water stains and other stains, affecting its aesthetics and functional service life.

Method used

Using a combination of chitosan-modified titanium dioxide, silicone-modified polyurethane acrylate and fluorocarbon surfactant, the hydrophilic and photocatalytic properties are improved by modifying titanium dioxide, and silicone-modified polyurethane acrylate enhances stain resistance. , and the film's stain resistance is improved by fluorocarbon surfactant treatment.

Benefits of technology

It significantly improves the anti-fouling ability of the release film, enhances its hydrophilic and photocatalytic properties, improves the surface smoothness and anti-fouling properties, and extends the service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of release films, and particularly discloses an anti-fouling release film and a preparation method thereof. The anti-fouling release film comprises a base layer and a treatment layer, and the base layer is prepared from, by weight, 50-80 parts of polypropylene, 5-8 parts of flexibilizer, 3-8 parts of elasticity regulator, 2-5 parts of release agent, 5-10 parts of chitosan modified titanium dioxide, 5-8 parts of siloxane modified polyurethane acrylate and 3-5 parts of smoothing agent; the raw material of the treatment layer comprises a fluorocarbon surfactant. The release film disclosed by the invention has a relatively good anti-pollution effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of release films, and in particular to an anti-fouling release film and a preparation method thereof. Background Art

[0002] Release film refers to a film with distinguishable surface. It is non-sticky or slightly sticky when in contact with specific materials under limited conditions. Common release films are made of base resin, toughening agent, elasticity regulator, and release agent. They have good tensile strength and toughness, and are easy to peel off. However, they are not resistant to stains, making them easily contaminated by oil stains, water stains, etc., which not only affects the appearance, but also may damage their functionality and service life. Summary of the invention

[0003] In order to improve the anti-fouling ability of a release film, the present application provides an anti-fouling release film and a preparation method thereof.

[0004] In the first aspect, the present application provides an anti-fouling release film, which adopts the following technical solution: An anti-fouling release film comprises a base layer and a treatment layer. The raw materials of the base layer comprise the following components in parts by weight: 50 to 80 parts of polypropylene, 5 to 8 parts of a toughening agent, 3 to 8 parts of an elasticity regulator, 2 to 5 parts of a release agent, 5 to 10 parts of chitosan-modified titanium dioxide, 5 to 8 parts of siloxane-modified polyurethane acrylate, and 3 to 5 parts of a lubricant; the raw materials of the treatment layer comprise a fluorocarbon surfactant.

[0005] By adopting the above technical scheme, chitosan is used to modify titanium dioxide to improve the dispersion performance of titanium dioxide. Titanium dioxide can improve the hydrophilicity of the film and also has certain photocatalytic properties, which can decompose some substances on the surface of the film, thereby improving the anti-fouling performance; Siloxane-modified polyurethane acrylate has good anti-fouling performance, and the addition of a lubricant can improve the smoothness of the base surface. Finally, through the treatment of fluorocarbon surfactants, the anti-fouling ability of the release film is improved.

[0006] In a specific embodiment, the preparation method of chitosan-modified titanium dioxide comprises the following steps: dispersing titanium dioxide in water to form a dispersion; Adding chitosan to the acetic acid aqueous solution, stirring evenly to dissolve the chitosan, and obtaining a chitosan solution; Adding the dispersion into the chitosan solution, stirring evenly to obtain a mixed solution; Add glutaraldehyde to the mixed solution, stir evenly, let it stand, add sodium hydroxide solution, soak, filter, wash, dry and grind to obtain modified titanium dioxide.

[0007] By adopting the above technical scheme, titanium dioxide is first dispersed to obtain a dispersion liquid, then chitosan is dissolved in an acetic acid aqueous solution to obtain a chitosan solution, and finally the dispersion liquid is added to the chitosan solution, stirred and mixed evenly, glutaraldehyde is added to react, allowed to stand, sodium hydroxide solution is added, soaked, filtered, washed, dried, and ground to obtain modified titanium dioxide with good dispersibility.

[0008] In a specific embodiment, the mass fraction of titanium dioxide in the dispersion is 1%-3%; the mass fraction of chitosan in the chitosan solution is 0.1%-0.5%; and the weight ratio of the dispersion to the chitosan solution in the mixed solution is 1:(8-10).

[0009] By adopting the above technical solution, the ratio of titanium dioxide to chitosan is further limited, and the modification effect of titanium dioxide is improved.

[0010] In a specific embodiment, the preparation method of the siloxane-modified polyurethane acrylate comprises the following steps: Under the protection of nitrogen, terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole are stirred and mixed uniformly, and then isophorone diisocyanate is added dropwise at 60-80° C. to react to obtain siloxane-modified polyurethane acrylate.

[0011] By adopting the above technical scheme and utilizing the above method, the polysiloxane molecular structure containing terminal hydroxyl groups is introduced into polyurethane acrylate, so that the prepared siloxane-modified polyurethane acrylate has a better anti-fouling effect.

[0012] In a specific embodiment, the weight ratio of the terminal hydroxyl polydimethylsiloxane, the pentaerythritol triacrylate, the dibutyltin dodecanoate, and the p-hydroxyanisole is 1:(18.9-19.0):(0.01-0.03):(0.03-0.05).

[0013] By adopting the above technical scheme, the ratio of terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole is further limited, so that the raw materials can react better and the performance of the prepared siloxane-modified polyurethane acrylate is improved. In a specific embodiment, the lubricant comprises a mixture of precipitated silica and talc.

[0014] By adopting the above technical solution, the surfaces of precipitated silica and talcum powder are smooth and have low oil absorption, and the porous structure of precipitated silica can improve the anti-transmission effect of the prepared release film.

[0015] In a second aspect, the present application provides a method for preparing an anti-fouling release film, which adopts the following technical solution: A method for preparing an anti-fouling release film comprises the following steps: Preparation of the base layer: polypropylene, toughening agent, elasticity regulator, release agent, chitosan-modified titanium dioxide, siloxane-modified polyurethane acrylate, and lubricant are stirred and mixed uniformly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast, and stretched to obtain a base layer; Surface treatment: add fluorocarbon surfactant to water, stir evenly to obtain a treatment solution; place the base layer in the treatment solution for surface treatment, take it out, wash it, dry it, and obtain an anti-fouling release film.

[0016] By adopting the above technical scheme, the raw materials such as polypropylene, toughening agent, elasticity regulator, release agent, chitosan modified titanium dioxide, siloxane modified polyurethane acrylate, and lubricant are first mixed, melt-extruded, cast, and stretched to obtain a base layer, and finally the base layer is immersed in a treatment liquid for surface treatment to obtain a release film with good anti-fouling effect.

[0017] In a specific embodiment, in the surface treatment step, the weight fraction of the fluorocarbon surfactant in the treatment liquid is 1-3%.

[0018] In a specific possible implementation manner, in the surface treatment step, the base layer is placed in a treatment liquid, heated in a water bath at 20-30° C. for 50-70 min, taken out, cleaned, and dried to obtain an anti-fouling release film.

[0019] By adopting the above technical solution, the content of fluorocarbon surfactant in the treatment liquid and the temperature and time of surface treatment are further limited, thereby improving the treatment effect on the base layer.

[0020] In summary, the present application includes at least one of the following beneficial technical effects: 1. In this application, chitosan is used to modify titanium dioxide to improve the dispersion performance of titanium dioxide. Titanium dioxide can improve the hydrophilicity of the film and also has certain photocatalytic properties, which can decompose some substances on the surface of the film, thereby improving the anti-fouling performance; Siloxane-modified polyurethane acrylate has good anti-fouling performance, and the addition of a lubricant can improve the smoothness of the surface of the base layer. Finally, the anti-fouling ability of the release film is improved by treating it with a fluorocarbon surfactant; 2. The lubricant in the present application is a mixture of precipitated silica and talcum powder. The surfaces of the precipitated silica and talcum powder are smooth and have low oil absorption. The porous structure of the precipitated silica can improve the anti-transmission effect of the prepared release film. 3. The method in the present application first mixes the raw materials such as polypropylene, toughening agent, elasticity regulator, release agent, chitosan-modified titanium dioxide, siloxane-modified polyurethane acrylate, and lubricant, melt-extrudes, casts, and stretches to obtain a base layer, and finally immerses the base layer in a treatment liquid for surface treatment to obtain a release film with good anti-fouling effect. DETAILED DESCRIPTION

[0021] The present application is further described in detail below with reference to the embodiments.

[0022] All raw materials in the examples can be obtained from commercial sources, among which the fluorocarbon surfactant has a CAS number of 151772-58-6.

[0023] Preparation Example Preparation Example 1 Preparation Example 1 provides a method for preparing chitosan-modified titanium dioxide, comprising the following steps: Dispersing titanium dioxide in water and performing ultrasonic dispersion for 25 minutes to form a dispersion; wherein the mass fraction of titanium dioxide in the dispersion is 1%; Add chitosan to an aqueous solution of acetic acid with a volume fraction of 1%, stir evenly, dissolve the chitosan, and obtain a chitosan solution; wherein the mass fraction of chitosan in the chitosan solution is 0.1%; Add the dispersion into the chitosan solution and stir evenly to obtain a mixed solution; wherein the weight ratio of the dispersion to the chitosan solution in the mixed solution is 1:8; Add glutaraldehyde to the mixed solution, stir for 1 hour, let stand for 8 hours, add an appropriate amount of 0.1 mol / L sodium hydroxide solution, soak until the mixed solution becomes a gel, filter, wash, dry and grind to obtain modified titanium dioxide.

[0024] Preparation Example 2 Preparation Example 2 provides a method for preparing chitosan-modified titanium dioxide, comprising the following steps: Dispersing titanium dioxide in water and ultrasonically dispersing for 25 minutes to form a dispersion; wherein the mass fraction of titanium dioxide in the dispersion is 2%; Add chitosan to an acetic acid aqueous solution with a volume fraction of 1%, stir evenly, dissolve the chitosan, and obtain a chitosan solution; wherein the mass fraction of chitosan in the chitosan solution is 0.3%; Adding the dispersion into the chitosan solution and stirring evenly to obtain a mixed solution; wherein the weight ratio of the dispersion to the chitosan solution in the mixed solution is 1:9; Add glutaraldehyde to the mixed solution, stir for 1 hour, let stand for 8 hours, add an appropriate amount of 0.1 mol / L sodium hydroxide solution, soak until the mixed solution becomes a gel, filter, wash, dry and grind to obtain modified titanium dioxide.

[0025] Preparation Example 3 Preparation Example 3 provides a method for preparing chitosan-modified titanium dioxide, comprising the following steps: Dispersing titanium dioxide in water and performing ultrasonic dispersion for 25 minutes to form a dispersion; wherein the mass fraction of titanium dioxide in the dispersion is 3%; Add chitosan to an acetic acid aqueous solution with a volume fraction of 1%, stir evenly, dissolve the chitosan, and obtain a chitosan solution; wherein the mass fraction of chitosan in the chitosan solution is 0.5%; Adding the dispersion into the chitosan solution and stirring evenly to obtain a mixed solution; wherein the weight ratio of the dispersion to the chitosan solution in the mixed solution is 1:10; Add glutaraldehyde to the mixed solution, stir for 1 hour, let stand for 8 hours, add an appropriate amount of 0.1 mol / L sodium hydroxide solution, soak until the mixed solution becomes a gel, filter, wash, dry and grind to obtain modified titanium dioxide.

[0026] Preparation Example 4 Preparation Example 4 provides a method for preparing siloxane-modified polyurethane acrylate, comprising the following steps: Under the protection of nitrogen, terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole are stirred and mixed evenly, and then the temperature begins to rise. At 60°C, isophorone diisocyanate is added dropwise, and then the reaction is carried out at 80°C to obtain siloxane-modified polyurethane acrylate; wherein the weight ratio of terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole is 1:18.9:0.01:0.03; and the molar ratio of terminal hydroxyl polydimethylsiloxane to isophorone diisocyanate is 6:5.

[0027] Preparation Example 5 Preparation Example 5 provides a method for preparing siloxane-modified polyurethane acrylate, comprising the following steps: Under the protection of nitrogen, terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole are stirred and mixed evenly, and then the temperature begins to rise. At 60°C, isophorone diisocyanate is added dropwise, and then the reaction is carried out at 80°C to obtain siloxane-modified polyurethane acrylate; wherein the weight ratio of terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole is 1:18.95:0.02:0.04; and the molar ratio of terminal hydroxyl polydimethylsiloxane to isophorone diisocyanate is 6:5.

[0028] Preparation Example 6 Preparation Example 6 provides a method for preparing siloxane-modified polyurethane acrylate, comprising the following steps: Under the protection of nitrogen, terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole are stirred and mixed evenly, and then the temperature begins to rise. At 60°C, isophorone diisocyanate is added dropwise, and then the reaction is carried out at 80°C to obtain siloxane-modified polyurethane acrylate; wherein the weight ratio of terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole is 1:19.0:0.03:0.05; and the molar ratio of terminal hydroxyl polydimethylsiloxane to isophorone diisocyanate is 6:5. Example

[0029] Example 1 Embodiment 1 provides a method for preparing an anti-fouling release film, comprising the following steps: Preparation of base layer: 50kg of polypropylene, 5kg of toughening agent, 3kg of elasticity regulator, 2kg of release agent, 5kg of chitosan-modified titanium dioxide in Preparation Example 1, 5kg of siloxane-modified polyurethane acrylate in Preparation Example 4, and 3kg of lubricant are stirred and mixed to obtain a mixture; then the mixture is added to an extruder, melt-extruded, cast, and stretched to obtain a base layer with a thickness of 40 microns; wherein the toughening agent is POE material; the elasticity regulator is styrene-butadiene rubber; the release agent is siloxane release agent TP-200E; the lubricant is a mixture of precipitated silica and talcum powder, and the weight ratio of precipitated silica to talcum powder is 1:2; Surface treatment: Add fluorocarbon surfactant to water, stir evenly to obtain a treatment liquid; the weight fraction of the fluorocarbon surfactant in the treatment liquid is 2%; place the base layer in the treatment liquid, heat it in a water bath at 20°C for 70 minutes, take it out, wash it, and dry it to obtain an anti-fouling release film.

[0030] Example 2 The difference between Example 2 and Example 1 is that the chitosan-modified titanium dioxide is the chitosan-modified titanium dioxide in Preparation Example 2; the remaining steps are consistent with Example 1.

[0031] Example 3 The difference between Example 3 and Example 1 is that the chitosan-modified titanium dioxide is the chitosan-modified titanium dioxide in Preparation Example 3; the remaining steps are consistent with Example 1.

[0032] Example 4 The difference between Example 4 and Example 2 is that the siloxane-modified polyurethane acrylate is the siloxane-modified polyurethane acrylate in Preparation Example 5; the remaining steps are consistent with Example 2.

[0033] Example 5 The difference between Example 5 and Example 2 is that the siloxane-modified polyurethane acrylate is the siloxane-modified polyurethane acrylate in Preparation Example 6; the remaining steps are consistent with Example 2.

[0034] Example 6 The difference between Example 6 and Example 4 is that, in preparation of the base layer, 65 kg of polypropylene, 6.5 kg of toughening agent, 5.5 kg of elasticity regulator, 3.5 kg of release agent, 7.5 kg of chitosan-modified titanium dioxide in Preparation Example 2, 6.5 kg of siloxane-modified polyurethane acrylate in Preparation Example 5, and 4 kg of lubricant are stirred and mixed uniformly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast, and stretched to obtain a base layer; the remaining steps are consistent with Example 4.

[0035] Example 7 The difference between Example 7 and Example 4 is that, in preparation of the base layer, 80 kg of polypropylene, 8 kg of toughening agent, 8 kg of elasticity regulator, 5 kg of release agent, 10 kg of chitosan-modified titanium dioxide in Preparation Example 2, 8 kg of siloxane-modified polyurethane acrylate in Preparation Example 5, and 5 kg of lubricant are stirred and mixed uniformly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast, and stretched to obtain a base layer; the remaining steps are consistent with Example 4.

[0036] Example 8 The difference between Example 8 and Example 6 is that the lubricant is precipitated silica; the remaining steps are consistent with Example 6.

[0037] Example 9 The difference between Example 9 and Example 6 is that the lubricant is talcum powder; the remaining steps are consistent with Example 6.

[0038] Example 10 The difference between Example 10 and Example 6 is that, in surface treatment, a fluorocarbon surfactant is added to water and stirred evenly to obtain a treatment liquid; wherein the weight fraction of the fluorocarbon surfactant in the treatment liquid is 2%; the base layer is placed in the treatment liquid, heated in a water bath at 25°C for 60 minutes, taken out, washed, and dried to obtain an anti-fouling release film; and the remaining steps are consistent with Example 6.

[0039] Embodiment 11 The difference between Example 11 and Example 6 is that, in surface treatment, a fluorocarbon surfactant is added to water and stirred evenly to obtain a treatment liquid; wherein the weight fraction of the fluorocarbon surfactant in the treatment liquid is 2%; the base layer is placed in the treatment liquid, heated in a water bath at 30°C for 50 minutes, taken out, washed, and dried to obtain an anti-fouling release film; and the remaining steps are consistent with Example 6.

[0040] Comparative Example Comparative Example 1 Comparative Example 1 provides a method for preparing a release film, comprising the following steps: Preparation of base layer: 50kg of polypropylene, 5kg of toughening agent, 3kg of elasticity regulator and 2kg of release agent are stirred and mixed evenly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast and stretched to obtain a release film with a thickness of 40 microns; the toughening agent is POE material; the elasticity regulator is styrene-butadiene rubber; and the release agent is silicone release agent TP-200E.

[0041] Comparative Example 2 Comparative Example 2 provides a method for preparing a release film, comprising the following steps: Preparation of the base layer: 50 kg of polypropylene, 5 kg of toughening agent, 3 kg of elasticity regulator, 2 kg of release agent, and 5 kg of chitosan-modified titanium dioxide in Preparation Example 1 were stirred and mixed uniformly to obtain a mixture; the mixture was then added to an extruder, melt-extruded, cast, and stretched to obtain a release film with a thickness of 40 microns; wherein the toughening agent was POE material; the elasticity regulator was styrene-butadiene rubber; and the release agent was silicone release agent TP-200E.

[0042] Comparative Example 3 Comparative Example 3 provides a method for preparing a release film, comprising the following steps: Preparation of the base layer: 50 kg of polypropylene, 5 kg of toughening agent, 3 kg of elasticity regulator, 2 kg of release agent, and 5 kg of the silicone-modified polyurethane acrylate in Preparation Example 4 were stirred and mixed uniformly to obtain a mixture; the mixture was then added to an extruder, melt-extruded, cast, and stretched to obtain a release film with a thickness of 40 microns; wherein the toughening agent was POE material; the elasticity regulator was styrene-butadiene rubber; and the release agent was silicone release agent TP-200E.

[0043] Comparative Example 4 Comparative Example 4 provides a method for preparing a release film, comprising the following steps: Preparation of base layer: 50kg of polypropylene, 5kg of toughening agent, 3kg of elasticity regulator, 2kg of release agent and 3kg of lubricant are stirred and mixed evenly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast, and stretched to obtain a release film with a thickness of 40 microns; the toughening agent is POE material; the elasticity regulator is styrene-butadiene rubber; the release agent is silicone release agent TP-200E; the lubricant is a mixture of precipitated silica and talcum powder, and the weight ratio of precipitated silica to talcum powder is 1:2.

[0044] Comparative Example 5 Comparative Example 5 provides a method for preparing a release film, comprising the following steps: Preparation of base layer: 50kg of polypropylene, 5kg of toughening agent, 3kg of elasticity regulator and 2kg of release agent are stirred and mixed evenly to obtain a mixture; then the mixture is added to an extruder, melt-extruded, cast and stretched to obtain a base layer with a thickness of 40 microns; wherein the toughening agent is POE material; the elasticity regulator is styrene-butadiene rubber; the release agent is silicone release agent TP-200E; surface treatment: fluorocarbon surfactant is added to water, stirred evenly to obtain a treatment liquid; wherein the weight fraction of the fluorocarbon surfactant in the treatment liquid is 2%; the base layer is placed in the treatment liquid, heated in a water bath at 20°C for 70 minutes, taken out, cleaned and dried to obtain a release film.

[0045] Performance test of anti-fouling performance: write on the release film with an oil-based pen and then wipe it to observe the wiping effect, which can be wiped off, wiped but leaving slight marks, difficult to wipe off, and very difficult to wipe off; and test the oil contact angle of the release film. The larger the oil contact angle, the better the anti-fouling effect of the release film.

[0046] Table 1 Performance test results of release film sample Oil contact angle (°) Wiping effect Example 1 10.30 Can be wiped off Example 2 10.60 Can be wiped off Example 3 10.50 Can be wiped off Example 4 10.92 Can be wiped off Example 5 10.73 Can be wiped off Example 6 11.51 Can be wiped off Example 7 11.18 Can be wiped off Example 8 11.02 Can be wiped off Example 9 11.05 Can be wiped off Example 10 12.40 Can be wiped off Embodiment 11 12.15 Can be wiped off Comparative Example 1 <10 Difficult to wipe off Comparative Example 2 <10 Hard to wipe off Comparative Example 3 <10 Hard to wipe off Comparative Example 4 <10 Hard to wipe off Comparative Example 5 <10 Hard to wipe off Combining Example 1 and Comparative Examples 1-5, the release film in Example 1 has the best anti-fouling effect. It can be seen that the composite release film in the present application, the titanium dioxide in the base layer can improve the hydrophilicity of the film, and also has certain photocatalytic properties, which can decompose some substances on the surface of the film; the siloxane-modified polyurethane acrylate has good anti-fouling properties, and the addition of a lubricant can improve the smoothness of the base layer surface, and finally through the treatment with a fluorocarbon surfactant, the anti-fouling ability of the release film is improved.

[0047] In combination with Examples 1-3, the release film in Example 2 has the best anti-fouling effect. It can be seen that when preparing chitosan-modified titanium dioxide, the ratio of titanium dioxide to chitosan in Preparation Example 2 is optimal, so that the release film has the best anti-fouling effect.

[0048] Combining Example 2, Example 4 and Example 5, the anti-fouling effect of the release film in Example 4 is the best. It can be seen that when preparing siloxane-modified polyurethane acrylate, the ratio of terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole in Preparation Example 5 is optimal, so that the obtained siloxane-modified polyurethane acrylate has good anti-fouling performance.

[0049] Combining Example 4, Example 6 and Example 7, the anti-fouling effect of the release film in Example 6 is the best. It can be seen that when preparing the base layer, increasing the amount of raw materials used, the anti-fouling performance of the base layer shows a trend of first increasing and then decreasing.

[0050] Combining Example 6, Example 8 and Example 9, the anti-fouling effect of the release film in Example 6 is the best. It can be seen that when preparing the base layer, the lubricant is preferably a mixture of precipitated silica and talcum powder. The combination of the two improves the anti-fouling effect of the prepared release film.

[0051] Combining Example 6, Example 10 and Example 11, the release film in Example 10 has the best anti-fouling effect. It can be seen that when the base layer is surface-treated with the treatment liquid, the surface treatment conditions in Example 10 are the best, thereby obtaining a release film with the best anti-fouling effect.

[0052] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-fouling release film, characterized in that: It comprises a base layer and a treatment layer, wherein the raw materials of the base layer comprise the following components in parts by weight: 50-80 parts of polypropylene, 5-8 parts of a toughening agent, 3-8 parts of an elasticity regulator, 2-5 parts of a release agent, 5-10 parts of chitosan-modified titanium dioxide, 5-8 parts of siloxane-modified polyurethane acrylate, and 3-5 parts of a lubricant; and the raw materials of the treatment layer comprise a fluorocarbon surfactant.

2. The anti-fouling release film according to claim 1, characterized in that: The preparation method of chitosan modified titanium dioxide comprises the following steps: dispersing titanium dioxide in water to form a dispersion; Adding chitosan to the acetic acid aqueous solution, stirring evenly to dissolve the chitosan, and obtaining a chitosan solution; Adding the dispersion into the chitosan solution, stirring evenly to obtain a mixed solution; Add glutaraldehyde to the mixed solution, stir evenly, let it stand, add sodium hydroxide solution, soak, filter, wash, dry and grind to obtain modified titanium dioxide.

3. The anti-fouling release film according to claim 2, characterized in that: The mass fraction of titanium dioxide in the dispersion is 1%-3%; the mass fraction of chitosan in the chitosan solution is 0.1%-0.5%; and the weight ratio of the dispersion to the chitosan solution in the mixed solution is 1:(8-10).

4. The anti-fouling release film according to claim 1, characterized in that: The preparation method of the siloxane-modified polyurethane acrylate comprises the following steps: Under the protection of nitrogen, terminal hydroxyl polydimethylsiloxane, pentaerythritol triacrylate, dibutyltin dodecanoate and p-hydroxyanisole are stirred and mixed uniformly, and then isophorone diisocyanate is added dropwise at 60-80° C. to react to obtain siloxane-modified polyurethane acrylate.

5. The anti-fouling release film according to claim 4, characterized in that: The weight ratio of the terminal hydroxyl polydimethylsiloxane, the pentaerythritol triacrylate, the dibutyltin dodecanoate and the p-hydroxyanisole is 1: (18.9-19.0): (0.01-0.03): (0.03-0.05).

6. The anti-fouling release film according to claim 1, characterized in that: The lubricant comprises a mixture of precipitated silica and talc.

7. A method for preparing the anti-fouling release film according to any one of claims 1 to 6, characterized in that: The following steps are involved: Preparation of the base layer: polypropylene, toughening agent, elasticity regulator, release agent, chitosan-modified titanium dioxide, siloxane-modified polyurethane acrylate, and lubricant are stirred and mixed uniformly to obtain a mixture; the mixture is then added to an extruder, melt-extruded, cast, and stretched to obtain a base layer; Surface treatment: add fluorocarbon surfactant to water, stir evenly to obtain a treatment solution; place the base layer in the treatment solution for surface treatment, take it out, wash it, dry it, and obtain an anti-fouling release film.

8. The method for preparing an anti-fouling release film according to claim 7, characterized in that: In the surface treatment step, the weight fraction of the fluorocarbon surfactant in the treatment liquid is 1-3%.

9. The method for preparing an anti-fouling release film according to claim 8, characterized in that: In the surface treatment step, the base layer is placed in a treatment liquid, heated in a water bath at 20-30° C. for 50-70 minutes, taken out, cleaned, and dried to obtain an anti-fouling release film.